A method for manufacturing a semiconductor array substrate that can increase pixel capacitance
By depositing a SiOx buffer layer on a glass substrate and adjusting the film deposition sequence, the problem of IGZO etching damaging the pixel electrodes in the 6 Mask process of IGZO array boards was solved, ensuring electrical stability and pixel capacitance area, and enabling normal display of IGZO array boards.
Patent Information
- Application Number
- CN202310348233.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-04-04
AI Technical Summary
When existing 6-mask Top-com add-on models directly apply the a-Si array board manufacturing process to the IGZO array board, the IGZO etching method will damage the pattern of another film layer, causing the pixels to fail to display properly.
A SiOx buffer layer is deposited on a glass substrate. The deposition sequence of the pixel electrode and the active layer is adjusted. Dry etching and low-temperature annealing processes are used to increase the SiOx buffer layer to protect the pixel electrode. Electrical stability and pixel capacitance area are ensured by adjusting the film thickness and material selection without increasing the number of photomasks.
This effectively avoids the mutual etching problem between IGZO and pixel electrodes, ensuring electrical stability and pixel capacitance area, and preventing capacitance reduction due to increased film thickness, thus enabling normal display of the IGZO array board.
Smart Images

Figure CN116613168B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of display device manufacturing technology, specifically referring to a method for manufacturing a semiconductor array substrate that can increase pixel capacitance. Background Technology
[0002] The working principle of a liquid crystal display (LCD) panel involves placing liquid crystal molecules between two parallel glass substrates. Numerous fine vertical and horizontal wires are located between the two substrates. The direction of the liquid crystal molecules is controlled by whether or not electricity is applied, thus refracting light from the backlight module to produce an image. Typically, an LCD panel consists of a color filter (CF) substrate, a thin-film transistor (TFT) substrate, liquid crystal (LC) sandwiched between the CF and TFT substrates, and a sealant.
[0003] a-Si (amorphous silicon), LTPS (low-temperature polycrystalline silicon), and IGZO (indium gallium zinc oxide) are types of thin-film transistor (TFT) materials. In recent years, with the development of small- and medium-sized display technologies, the market has seen the coexistence of multiple technologies such as a-Si and LTPS. Comparatively, a-Si technology has the longest development history and is relatively simple, dominating the market due to its good cost-performance ratio; LTPS technology, with its mature supply chain and higher performance, also holds a certain market share.
[0004] IGZO is an amorphous oxide containing indium, gallium, and zinc. Its carrier mobility is 20 to 30 times that of amorphous silicon, which can greatly improve the charging and discharging rate of the pixel electrode in TFT, improve the response speed of the pixel, and enable a faster panel refresh rate, thus achieving ultra-high resolution TFT-LCD.
[0005] Currently, the array manufacturing processes applied to TFT substrates are mainly concentrated in 8-mask off-line machines, 9-mask Top-com TIC machines, and 10-mask Mid-com TIC machines. To save costs, existing a-Si machines have also been developed into 6-mask Top-com off-line machines, which not only shortens cycle time but also simplifies the process flow and effectively improves efficiency.
[0006] If the Top-com a-Si array board manufacturing process based on 6 Mask is directly used to produce IGZO array boards, it is found, combined with the substrate design and process technology, that due to the design of the 6 Mask a-Si array board manufacturing process (such as... Figure 1As shown, the PV insulating film layer and organic planarization layer (OC) of traditional TFT devices are omitted. The pixel electrode PE-ITO is designed to be coplanar with a-Si. The traditional a-Si patterning process uses dry etching, while the pixel electrode PE-ITO uses oxalic acid wet etching. If this process is used to directly produce IGZO array boards, the IGZO etching method is also oxalic acid wet etching. This will inevitably cause damage to the pattern of the other film layer, regardless of whether IGZO or ITO is patterned sequentially, thus affecting the normal display of pixels. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to provide a method for manufacturing a semiconductor array substrate that can increase pixel capacitance, applicable to Top-com add-on models with 6 masks.
[0008] This invention is implemented as follows: A method for manufacturing a semiconductor array substrate that can increase pixel capacitance includes the following steps: Step 1: Sequentially deposit a SiOx buffer layer on the glass substrate using CVD; Step 2: Use a common electrode layer photomask, paired with negative photoresist, to perform the exposure and development process; Step 3: Dry etching is performed on the developed area to etch away the SiOx in the area not covered by the photoresist; Step 4: The negative photoresist is stripped off. Step 5: Sequentially pattern the first metal layer, i.e., the gate metal layer, on the SiOx buffer layer; Step 6: Deposit a first insulating layer using CVD; Step 7: Deposit a pixel electrode layer on the first insulating layer and pattern it, then perform low-temperature annealing at 220°C and crystallize the process. Step 8: Deposit an IGZO active layer on the first insulating layer using PVD and pattern it; Step 9: Deposit a second metal layer, namely the source and drain metal layer, on the patterned IGZO active layer and the pixel electrode layer using PVD. Step 10: A second insulating layer is deposited on the second metal layer using CVD as a passivation insulating layer to protect the TFT device and simultaneously serve as the dielectric layer for the pixel capacitor; Step 11: Deposit a common electrode layer on the second insulating layer.
[0009] Furthermore, in the fifth step, the first metal layer is selected as Mo / Al / Mo or Ti / Al / Ti.
[0010] Furthermore, the first insulating layer in the sixth step is selected from SiOx.
[0011] Furthermore, the pixel electrode layer in the seventh step is made of ITO.
[0012] Furthermore, in the ninth step, the second metal layer is selected as Mo / Al / Mo or Ti / Al / Ti.
[0013] Furthermore, the second insulating layer in the tenth step is selected from SiOx.
[0014] Furthermore, the common electrode layer in the eleventh step is made of ITO.
[0015] The advantages of this invention are as follows: After the first insulating layer is formed, the pixel electrode layer is preferentially deposited and patterned, and then annealed at 220°C. The crystallized pixel electrode is resistant to oxalic acid etching, and the pixel electrode will not be over-etched by oxalic acid when the IGZO active layer is patterned. This invention, without changing the number of 6 masks in the original a-Si process, modifies the deposition order of the pixel electrode and active layer, adjusts and optimizes the array process, and effectively avoids the mutual etching problem between IGZO and the pixel electrode. While changing the film deposition sequence effectively avoids the coexistence problem of the pixel electrode ITO and the active layer IGZO, directly converting the active layer of the TFT device from a-Si to IGZO requires simultaneous changes to the film composition of the original TFT device to ensure electrical stability. For example, the second insulating layer is changed from SiNx (active layer is a-Si) to SiOx (active layer is IGZO). This is because SiNx contains a large number of H ions, which can have an irreversible effect on the back channel of the BCE structure IGZO, resulting in poor device stability and Vth offset. Furthermore, based on past debugging experience, the thickness of the second insulating layer is increased after conversion to SiOx to ensure electrical stability. However, under the existing 6-mask process design, the increase in film thickness will simultaneously reduce the capacitance between the pixel electrode ITO and the common electrode ITO. Insufficient capacitance will directly affect the normal display of the original design. Therefore, this invention adds a layer of SiOx between the glass substrate and the first metal layer without adding a photomask. The buffer layer utilizes the existing common electrode layer photomask paired with negative photoresist for patterning. Without affecting transmittance or increasing photomask cost, it can effectively increase the pixel capacitance area, offsetting the reduction in pixel capacitance caused by the increase in the thickness of the second insulating layer. Therefore, it solves the problem of effective conversion from a-Si semiconductor layer to IGZO semiconductor layer in existing products. Attached Figure Description
[0016] The present invention will now be further described with reference to the accompanying drawings and embodiments.
[0017] Figure 1This is a schematic diagram of the structure of an existing a-Si array substrate.
[0018] Figure 2 This is a schematic diagram of the first step of the present invention.
[0019] Figure 3 This is a schematic diagram of the second step of the present invention.
[0020] Figure 4 This is a schematic diagram of the third step of the present invention.
[0021] Figure 5 This is a schematic diagram of the fourth step of the present invention.
[0022] Figure 6 This is a schematic diagram of the fifth step of the present invention.
[0023] Figure 7 This is a schematic diagram of the sixth step of the present invention.
[0024] Figure 8 This is a schematic diagram of the seventh step of the present invention.
[0025] Figure 9 This is a schematic diagram of the eighth step of the present invention.
[0026] Figure 10 This is a schematic diagram of the ninth step of the present invention.
[0027] Figure 11 This is a schematic diagram of the tenth step of the present invention.
[0028] Figure 12 This is a schematic diagram of the eleventh step of the present invention.
[0029] Figure label: 1-Glass substrate, 2-First metal layer, 3-First insulating layer, 4-Pixel electrode layer, 5'-a-Si active layer, 5-IGZO active layer; 6-Second metal layer; 7-Second insulating layer, 8-Common electrode layer, 9-SiOx buffer layer, A-Common electrode photomask, A1-Transparent area of common electrode photomask, A2-Non-transparent area of common electrode photomask, B-Negative photoresist. Detailed Implementation
[0030] like Figures 2 to 12 As shown, a method for manufacturing a semiconductor array substrate that can increase pixel capacitance includes the following steps: Step 1: Sequentially deposit a SiOx buffer layer-9 on glass substrate-1 using CVD; Step 2: Use a common electrode layer photomask A, paired with a negative photoresist B, to perform the exposure and development process; Step 3: Dry etching is performed on the developed area to etch away the SiOx in the area not covered by photoresist. Step 4: Peel off the negative photoresist B; Step 5: Sequentially pattern the first metal layer-2, i.e. the gate metal layer, on the SiOx buffer layer-9. The first metal layer-2 can be Mo / Al / Mo or Ti / Al / Ti. Step 6: Deposit a first insulating layer -3 using CVD. This first insulating layer -3 can be made of SiOx. Step 7: Deposit pixel electrode layer 4 (optional ITO) on the first insulating layer-3 and pattern it, then perform low-temperature annealing at 220°C to crystallize the process, improve the conductivity and transparency of the pixel electrode, and make the crystallized pixel electrode resistant to oxalic acid etching. Step 8: Deposit an IGZO active layer-5 on the first insulating layer-3 using PVD and pattern it. At this time, the oxalic acid etching during the patterning process will not cause over-etching risk to the pixel electrode layer-4. Step 9: Deposit a second metal layer -6, i.e., a source / drain metal layer, on the patterned IGZO active layer-5 and pixel electrode layer-4 using PVD. The second metal layer-6 can be Mo / Al / Mo or Ti / Al / Ti. Step 10: Deposit a second insulating layer -7 on the source and drain metal layers (second metal layer -6) using CVD. This layer serves as a passivation insulating layer to protect the TFT device and simultaneously acts as the dielectric layer for the pixel capacitor. SiOx can be selected. Step 11: Deposit a common electrode layer -8 on the second insulating layer -7, ITO is optional.
[0031] The method of the present invention, after the first insulating layer 3 is formed, preferentially deposits and patterns the pixel electrode layer 4, and performs a 220° process annealing on the pixel electrode layer 4. The crystallized pixel electrode can resist oxalic acid etching, and the pixel electrode will not be over-etched by oxalic acid when the IGZO active layer 5 is patterned.
[0032] This invention, without changing the number of photomasks in the original a-Si process (6 Masks), changes the deposition order of pixel electrodes and active layers, adjusts and optimizes the array process, and effectively avoids the mutual etching problem between IGZO and pixel electrodes. While changing the film deposition sequence effectively avoids the coexistence problem of the pixel electrode ITO and the active layer IGZO, directly converting the active layer of the TFT device from a-Si to IGZO requires simultaneous changes to the film composition of the original TFT device to ensure electrical stability. For example, the second insulating layer is changed from SiNx (active layer is a-Si) to SiOx (active layer is IGZO). This is because SiNx contains a large number of H ions, which can have an irreversible effect on the back channel of the BCE structure IGZO, resulting in poor device stability and Vth offset. Furthermore, based on past debugging experience, the thickness of the second insulating layer is increased after conversion to SiOx to ensure electrical stability. However, under the existing 6-mask process design, the increase in film thickness will simultaneously reduce the capacitance between the pixel electrode ITO and the common electrode ITO. Insufficient capacitance will directly affect the normal display of the original design. Therefore, this invention adds a layer of SiOx between the glass substrate-1 and the first metal layer-2 without adding a photomask. The buffer layer-9 utilizes the existing common electrode layer photomask with negative photoresist for patterning. Without affecting transmittance or increasing photomask cost, it can effectively increase the pixel capacitance area, offsetting the reduction in pixel capacitance caused by the increase in the thickness of the second insulating layer. Therefore, it solves the problem of effective conversion from a-Si semiconductor layer to IGZO semiconductor layer in existing products.
[0033] The above embodiments and figures are not intended to limit the form and style of the present invention. Any appropriate changes or modifications made by those skilled in the art should be considered as not departing from the patent scope of the present invention.
Claims
1. A method of manufacturing a semiconductor array substrate capable of increasing pixel capacitance, characterized by: Includes the following steps: Step 1: Sequentially deposit a SiOx buffer layer on the glass substrate using CVD; Step 2: Use a common electrode layer photomask, paired with negative photoresist, to perform the exposure and development process; Step 3: Dry etching is performed on the developed area to etch away the SiOx in the area not covered by photoresist. Step 4: Peel off the negative photoresist; Step 5: Sequentially pattern the first metal layer, i.e., the gate metal layer, on the SiOx buffer layer; Step 6: Deposit a first insulating layer using CVD; Step 7: Deposit a pixel electrode layer on the first insulating layer and pattern it, then perform low-temperature annealing at 220°C and crystallize the process. Step 8: Deposit an IGZO active layer on the first insulating layer using PVD and pattern it; Step 9: Deposit a second metal layer, namely the source and drain metal layer, on the patterned IGZO active layer and the pixel electrode layer using PVD. Step 10: A second insulating layer is deposited on the second metal layer using CVD as a passivation insulating layer to protect the TFT device and simultaneously serve as the dielectric layer for the pixel capacitor; Step 11: Deposit a common electrode layer on the second insulating layer.
2. The method of manufacturing a semiconductor array substrate capable of increasing pixel capacitance according to claim 1, wherein: The first metal layer in the fifth step is selected from Mo / Al / Mo or Ti / Al / Ti.
3. The method of manufacturing a semiconductor array substrate capable of increasing pixel capacitance according to claim 1, wherein: The first insulating layer in the sixth step is selected from SiOx.
4. The method of manufacturing a semiconductor array substrate capable of increasing pixel capacitance according to claim 1, wherein: The pixel electrode layer in the seventh step is made of ITO.
5. A method for manufacturing a semiconductor array substrate capable of increasing pixel capacitance as described in claim 1, characterized in that: The second metal layer in the ninth step is selected from Mo / Al / Mo or Ti / Al / Ti.
6. A method for manufacturing a semiconductor array substrate capable of increasing pixel capacitance as described in claim 1, characterized in that: The second insulating layer in the tenth step is selected from SiOx.
7. A method for manufacturing a semiconductor array substrate capable of increasing pixel capacitance as described in claim 1, characterized in that: The common electrode layer in step eleven is made of ITO.
Citation Information
Patent Citations
Manufacturing method of a-Si model-to-IGZO (Indium Gallium Zinc Oxide) array substrate
CN115472562A