A method for preparing a Bi-based high-temperature superconducting block
Through the method of two sintering and intermediate pressing, the superconducting phase and texture of Bi-system high-temperature superconducting blocks are improved, and the problem of difficulty in obtaining high-performance blocks in traditional processes is solved, and high-performance Bi-system high-temperature superconducting blocks are achieved Preparation of conductor blocks, suitable for applications in magnetic levitation and other fields.
Patent Information
- Application Number
- CN202310736014.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-21
AI Technical Summary
It is difficult to obtain that Bi-based high-temperature superconducting blocks have high superconducting phase content and high texture, resulting in lower performance than wire strips and unable to meet practical application requirements.
By controlling the compression and sintering parameters, the close packing of sheet powder and the decoupling of the nucleation growth process is achieved, and the intergranular connectivity is improved, and high-performance Bi-based high-temperature superconducting blocks are prepared. body.
It significantly improves the superconducting phase and texture content of Bi-based high-temperature superconducting blocks, improves its performance, solves the problem that traditional processes are difficult to obtain high-performance blocks, and is suitable for applications in fields such as magnetic levitation.
Smart Images

Figure CN116621576B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-temperature superconducting materials, and in particular relates to a method for preparing a Bi-based high-temperature superconducting block. Background Art
[0002] Bi-based high-temperature superconducting materials that can be used in practice currently include two categories, namely (Bi, Pb)2Sr2Ca2Cu3O x (Bi-2223)-based superconducting materials and (Bi,Pb)2Sr2CaCu2O x (Bi-2212) based superconducting materials, among which Bi-2223 has a T c The T of Bi-2212 is 110K, and it has excellent current carrying performance under 77K self-field conditions. It has been used in many demonstration applications including current leads, superconducting motors, superconducting magnets, and superconducting cables. c The temperature is 85K, and it is mainly used under low temperature and high field conditions of 4.2K to 20K, as an insert coil in a high-field magnet to achieve the preparation of a high-field magnet of more than 25T. With the goal of practical application, Bi-2223 and Bi-2212 need to be prepared into silver alloy-sheathed wire strips, which has a long process flow and many influencing factors. Therefore, in order to conduct basic research on Bi-2223 and Bi-2212-based superconducting materials, to explore the factors affecting the composition and structure of the materials on their superconductivity and intrinsic current-carrying performance, and to carry out research on the application technology of superconducting blocks in fields such as magnetic levitation, the preparation of high-performance Bi-2223 and Bi-2212 blocks is essential.
[0003] However, since the sintering process of Bi-based superconducting materials involves a complex phase evolution process and a slow texture growth process, the blocks obtained by the traditional solid-phase sintering process often have a low superconducting phase content and poor texture, resulting in the block performance being far lower than that of the wire and strip. The related research based on it is not representative and cannot be applied in practice. Therefore, it is extremely important to prepare blocks with high superconducting phase content and high texture for the development of Bi-based superconducting material preparation technology. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a Bi-based high-temperature superconducting block in view of the deficiencies of the above-mentioned prior art. After cold pressing the Bi-based precursor powder, the method adopts a method of two sinterings combined with intermediate pressing, and by controlling the pressing and two sintering parameters, the dense packing of the flaky powder and the decoupling of the nucleation and growth processes are achieved, thereby obtaining a Bi-based high-temperature superconducting block with higher intercrystalline connectivity, improving the superconducting phase and texture content of the Bi-based high-temperature superconducting block, and solving the problem that it is difficult to obtain a high-performance superconducting block with a high superconducting phase content and high texture by the traditional block sintering process.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a Bi-based high-temperature superconducting block, characterized in that the method comprises the following steps:
[0006] Step 1: cold-pressing a Bi-based precursor powder having a specific atomic ratio of Bi, Pb, Sr, Ca, and Cu to obtain a Bi-based cold-pressed block having a diameter of R1;
[0007] Step 2: sintering the Bi-based cold-pressed block obtained in step 1 to obtain a Bi-based sintered block;
[0008] Step 3: intermediate pressing the Bi-based sintered block obtained in step 2 to obtain a Bi-based pressed block with a diameter of R2, wherein R2>R1;
[0009] Step 4: perform secondary sintering on the Bi-based pressed block obtained in step 3 to obtain a Bi-based high-temperature superconducting block.
[0010] The above-mentioned method for preparing a Bi-based high-temperature superconducting block is characterized in that the specific atomic ratio of Bi, Pb, Sr, Ca, and Cu in the Bi-based precursor powder in step one is 1.65~1.95: 0.30~0.45: 1.85~2.00: 1.80~2.20: 2.80~3.20, and the Bi-based high-temperature superconducting block obtained in step four is a Bi-2223 high-temperature superconducting block; or the specific atomic ratio of Bi, Pb, Sr, Ca, and Cu in the Bi-based precursor powder in step one is 1.65~2.05: 0~0.45: 1.85~2.00: 0.80~1.20: 1.80~2.20, and the Bi-based high-temperature superconducting block obtained in step four is a Bi-2212 high-temperature superconducting block.
[0011] The above-mentioned method for preparing a Bi-based high-temperature superconducting block is characterized in that the diameter R1 of the Bi-based cold-pressed block in step 1 is ≥ 7 mm, the deformation amount of the intermediate pressing in step 3 is not less than 30%, and R2 / R1 ≥ 1.15. The present invention controls the deformation amount of the intermediate pressing, thereby controlling the diameter size of the Bi-based pressed block to promote sufficient deformation and improve the density of the Bi-based high-temperature superconducting block.
[0012] The above-mentioned method for preparing a Bi-based high-temperature superconducting block is characterized in that when the Bi-based high-temperature superconducting block obtained in step four is a Bi-2223 high-temperature superconducting block, the oxygen partial pressure in the sintering atmosphere of the first sintering in step two is 0.1% to 7.5%, and the first sintering time is 15h to 50h, and the oxygen partial pressure in the sintering atmosphere of the second sintering in step four is 7.5% to 25%, and the second sintering time is more than 50h.
[0013] The above-mentioned method for preparing a Bi-based high-temperature superconducting block is characterized in that the oxygen partial pressure in the sintering atmosphere of the first sintering is 0.1% and the temperature is 770°C to 800°C, or the oxygen partial pressure in the sintering atmosphere of the first sintering is 7.5% and the temperature is 810°C to 835°C.
[0014] The above-mentioned method for preparing a Bi-based high-temperature superconducting block is characterized in that the oxygen partial pressure in the sintering atmosphere of the secondary sintering is 7.5% and the temperature is 810°C to 835°C, or the oxygen partial pressure in the sintering atmosphere of the secondary sintering is 25% and the temperature is 840°C to 870°C.
[0015] During the sintering process of the Bi-based high-temperature superconducting block of the present invention, as the oxygen partial pressure in the sintering atmosphere increases, the corresponding sintering temperature also increases to ensure the phase formation rate of the superconducting phase in the target product.
[0016] The above-mentioned method for preparing a Bi-based high-temperature superconducting block is characterized in that, when the Bi-based high-temperature superconducting block obtained in step four is a Bi-2212 high-temperature superconducting block, the primary sintering in step two adopts a pure oxygen atmosphere, the primary sintering temperature is 780°C to 880°C, and the time is 10h to 50h, and the secondary sintering in step four adopts a pure oxygen atmosphere, the secondary sintering temperature is 885°C to 895°C, and the time is 5min to 40min.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] 1. The present invention first cold presses the Bi-based precursor powder, and then continues to perform intermediate pressing and secondary sintering (which can be called a composite pressing texture enhancement method) after the first sintering. By adjusting the pressing parameters twice, the dense packing of the flaky powder is achieved. Combined with adjusting the sintering parameters twice, the decoupling of the nucleation and growth processes is achieved, and a Bi-based high-temperature superconducting block with higher intercrystalline connectivity is obtained, thereby improving the superconducting phase content and texture degree of the Bi-based high-temperature superconducting block.
[0019] 2. The present invention regulates the sintering parameters of the Bi-based high-temperature superconducting block. First, a lower oxygen partial pressure is used in the first sintering, and the sintering temperature is adjusted with the change of oxygen partial pressure to ensure that Bi-2223 or Bi-2212 has a lower nucleation rate and obtains fewer crystal nuclei. Then, the oxygen partial pressure is increased in the second sintering, and the sintering temperature is adjusted with the change of oxygen partial pressure to increase the grain growth rate, achieve sufficient growth of large grains and obtain a high superconducting phase content, thereby obtaining a block with higher intercrystalline connectivity.
[0020] 3. For Bi-based high-temperature superconducting blocks with different compositions, the present invention adopts a slightly lower sintering temperature in the primary sintering process of Bi-2212 to promote the full sintering of Bi-2212, and adopts a slightly higher sintering temperature in the secondary sintering process of Bi-2212 to perform partial melting heat treatment to promote the formation of textured Bi-2212 high-temperature superconducting blocks.
[0021] 4. The present invention introduces a certain amount of deformation in the intermediate pressing after the primary sintering to achieve close packing of Bi-based superconducting lamellar grains with a simple process, thereby increasing the block density and ensuring the acquisition of a higher texture degree.
[0022] 5. The preparation method of the present invention is simple, does not require any modification to existing equipment, and is easy to implement.
[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a comparison chart of the preparation process flow of the Bi-based high-temperature superconducting block between the conventional one-step sintering method and the present invention.
[0025] Figure 2a This is the XRD diffraction pattern of Bi-2223 high-temperature superconducting bulk prepared by the traditional one-step sintering method.
[0026] Figure 2b This is the XRD diffraction pattern of the Bi-2223 high temperature superconducting block prepared in Example 1 of the present invention.
[0027] Figure 3 This is a diagram showing changes in block density and porosity during the preparation of a Bi-2223 high-temperature superconducting block in Example 1 of the present invention.
[0028] Figure 4a This is a micrograph of the surface morphology of a Bi-2223 high-temperature superconducting block prepared by the traditional one-step sintering method.
[0029] Figure 4b This is a micrograph of the surface morphology of the Bi-2223 high temperature superconducting block prepared in Example 1 of the present invention.
[0030] Figure 5a This is a micrograph of the cross-sectional morphology of a Bi-2223 high-temperature superconducting block prepared by the traditional one-step sintering method.
[0031] Figure 5b This is a micrograph of the cross-sectional morphology of the Bi-2223 high-temperature superconducting block prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The conventional one-step sintering method for preparing Bi-2223 high temperature superconducting bulk includes the following steps:
[0033] Step 1: cold-pressing Bi-2223 precursor powder with an atomic ratio of Bi, Pb, Sr, Ca, and Cu of 1.95:0.30:1.85:2.20:3.20 to obtain a Bi-2223 cold-pressed block with a diameter of 10 mm;
[0034] Step 2: sinter the Bi-2223 cold pressed block obtained in step 1 once, with the oxygen partial pressure in the sintering atmosphere being 7.5%, the sintering temperature being 826° C., and the primary sintering time being 93 h, to obtain a Bi-2223 sintered block having a Bi-2223 mass content of 78%;
[0035] According to the test, the superconducting phase content of the Bi-2223 high-temperature superconducting block prepared by the existing traditional one-step sintering method is 78%, the texture degree in the (00l) direction is 59%, and the critical current is 45A under 77K self-field conditions.
[0036] Example 1
[0037] like Figure 1 As shown, this embodiment includes the following steps:
[0038] Step 1: cold-pressing Bi-2223 precursor powder with an atomic ratio of Bi, Pb, Sr, Ca, and Cu of 1.95:0.30:1.85:2.20:3.20 to obtain a Bi-2223 cold-pressed block with a diameter of 10 mm;
[0039] Step 2: sinter the Bi-2223 cold pressed block obtained in step 1 once, wherein the oxygen partial pressure in the sintering atmosphere is 0.1%, the sintering temperature is 770° C., and the primary sintering time is 15 h, to obtain a Bi-2223 sintered block having a Bi-2223 mass content of 65%;
[0040] Step 3: Place the Bi-2223 sintered block obtained in step 2 in a mold with a diameter of 12 mm for intermediate pressing to obtain a Bi-2223 pressed block with a diameter of 12 mm;
[0041] Step 4: perform secondary sintering on the Bi-2223 pressed block obtained in step 3, with the oxygen partial pressure in the sintering atmosphere being 7.5%, the sintering temperature being 810° C., and the secondary sintering time being 80 h, to obtain a Bi-2223 high temperature superconducting block.
[0042] According to the test, the superconducting phase content of the Bi-2223 high-temperature superconducting bulk prepared in this embodiment is 96%, the texture degree in the (001) direction is 87%, and the critical current is 82A under the self-field condition of 77K.
[0043] Figure 2aThis is the XRD diffraction pattern of Bi-2223 high temperature superconductor block prepared by the traditional one-step sintering method. Figure 2a It can be seen that the main phase of the Bi-2223 high-temperature superconducting block is the Bi-2223 phase, and there is also a small amount of lead-rich phase Pb-3321 phase; however, the texture degree of the Bi-2223 phase is relatively low, with more obvious non-(00l) texture peaks such as (115) and (200). By calculation, it can be obtained that the (00l) texture degree is 59%.
[0044] Figure 2b is the XRD diffraction pattern of the Bi-2223 high temperature superconducting bulk prepared in Example 1 of the present invention. Figure 2b It can be seen that the main phase of the Bi-2223 high temperature superconducting bulk is the Bi-2223 phase, and the diffraction peak of the lead-rich phase Pb-3321 disappears.
[0045] Will Figure 2a and Figure 2b By comparison, it can be seen that the texture degree of the Bi-2223 phase in the Bi-2223 high-temperature superconducting block prepared by the method of the present invention is significantly improved, and the intensity of non-(00l) texture peaks such as (115) and (200) is significantly reduced, indicating that the preparation method of the present invention improves the superconducting phase content and texture degree of the Bi-based high-temperature superconducting block.
[0046] Figure 3 is a graph showing the change in block density and porosity during the preparation of Bi-2223 high temperature superconducting block in Example 1 of the present invention. Figure 3 It can be seen that in the preparation process of the present invention, the Bi-2223 cold-pressed block density obtained by cold-pressing the Bi-2223 precursor powder is 4.6 g / cm 3 After one sintering, the powder melted and the liquid phase appeared, and the block volume expanded, so the density of the Bi-2223 sintered block decreased to 3.4g / cm 3 After the intermediate pressing process, the density of the block is significantly increased to 5.8g / cm 3 In the subsequent secondary sintering process, due to the lack of excessive liquid phase, the block density did not further decrease, and due to the further formation of the sintered Bi-2223 phase, the block density increased slightly to 5.9 g / cm 3 At this time, the porosity of the Bi-2223 high-temperature superconducting block reaches about 6%, and its density reaches 94% of the theoretical density, ensuring the transport of superconducting current in the Bi-2223 high-temperature superconducting block.
[0047] Figure 4a This is a micrograph of the surface morphology of Bi-2223 high-temperature superconducting block prepared by the conventional one-step sintering method. Figure 4aIt can be seen that the surface of the Bi-2223 high-temperature superconducting block can obtain a certain (00l) direction texture, that is, the surface is composed of Bi-2223 grains grown in lamellar stacking, but there are a large number of holes in the Bi-2223 high-temperature superconducting block, and there are a certain amount of non-textured grains around the holes, resulting in a decrease in the system density and texture degree.
[0048] Figure 4b is a micrograph of the surface morphology of the Bi-2223 high temperature superconducting block prepared in Example 1 of the present invention. Figure 4b and Figure 4a By comparison, it can be seen that the density of the Bi-2223 high-temperature superconducting block is significantly improved by introducing intermediate pressing and two sinterings, and there are no obvious holes. At the same time, the grain arrangement is relatively flat, so it has a higher density; the microstructure of the Bi-2223 high-temperature superconducting block is conducive to obtaining high current-carrying performance.
[0049] Figure 5a This is a micrograph of the cross-sectional morphology of a Bi-2223 high-temperature superconducting block prepared by the conventional one-step sintering method. Figure 5a It can be seen that the arrangement of Bi-2223 grains in the fracture direction of the Bi-2223 high-temperature superconductor block is more disordered, there are a large number of non-textured grains, and there are a large number of holes on the fracture.
[0050] Figure 5b is a micrograph of the cross-sectional morphology of the Bi-2223 high temperature superconducting block prepared in Example 1 of the present invention. Figure 5b and Figure 5a Comparison shows that the present invention significantly improves the texture of the Bi-2223 high-temperature superconducting block by introducing intermediate pressing and two sinterings, a large number of grains can grow with the ab plane perpendicular to the pressing direction, and the grain growth is denser.
[0051] Example 2
[0052] like Figure 1 As shown, this embodiment includes the following steps:
[0053] Step 1: cold-pressing Bi-2223 precursor powder with an atomic ratio of Bi, Pb, Sr, Ca, and Cu of 1.65:0.45:2.00:1.80:2.80 to obtain a Bi-2223 cold-pressed block with a diameter of 9 mm;
[0054] Step 2: sinter the Bi-2223 cold pressed block obtained in step 1 once, wherein the oxygen partial pressure in the sintering atmosphere is 0.1%, the sintering temperature is 800° C., and the primary sintering time is 50 h, to obtain a Bi-2223 sintered block having a Bi-2223 mass content of 78%;
[0055] Step 3: Place the Bi-2223 sintered block obtained in step 2 in a mold with a diameter of 12 mm for intermediate pressing to obtain a Bi-2223 pressed block with a diameter of 12 mm;
[0056] Step 4: perform secondary sintering on the Bi-2223 pressed block obtained in step 3, with the oxygen partial pressure in the sintering atmosphere being 7.5%, the sintering temperature being 835° C., and the secondary sintering time being 78 h, to obtain a Bi-2223 high temperature superconducting block.
[0057] According to the test, the superconducting phase content of the Bi-2223 high-temperature superconducting bulk prepared in this embodiment is 98%, the texture degree in the (001) direction is 86%, and the critical current is 76A under the self-field condition of 77K.
[0058] Example 3
[0059] like Figure 1 As shown, this embodiment includes the following steps:
[0060] Step 1: cold-pressing Bi-2223 precursor powder with an atomic ratio of Bi, Pb, Sr, Ca, and Cu of 1.76:0.34:1.91:2.02:3.10 to obtain a Bi-2223 cold-pressed block with a diameter of 7 mm;
[0061] Step 2: sinter the Bi-2223 cold pressed block obtained in step 1 once, with the oxygen partial pressure in the sintering atmosphere being 7.5%, the sintering temperature being 810° C., and the primary sintering time being 15 h, to obtain a Bi-2223 sintered block having a Bi-2223 mass content of 79%;
[0062] Step 3: Place the Bi-2223 sintered block obtained in step 2 in a mold with a diameter of 13 mm for intermediate pressing to obtain a Bi-2223 pressed block with a diameter of 13 mm;
[0063] Step 4: perform secondary sintering on the Bi-2223 pressed block obtained in step 3, with the oxygen partial pressure in the sintering atmosphere being 25%, the sintering temperature being 840° C., and the secondary sintering time being 80 h, to obtain a Bi-2223 high temperature superconducting block.
[0064] According to the test, the superconducting phase content of the Bi-2223 high-temperature superconducting block prepared in this embodiment is 98%, the texture degree in the (001) direction is greater than 80%, and the critical current is 72A under the self-field condition of 77K.
[0065] Example 4
[0066] like Figure 1 As shown, this embodiment includes the following steps:
[0067] Step 1: cold-pressing Bi-2223 precursor powder with an atomic ratio of Bi, Pb, Sr, Ca, and Cu of 1.80:0.34:1.95:2.12:3.13 to obtain a Bi-2223 cold-pressed block with a diameter of 10 mm;
[0068] Step 2: sinter the Bi-2223 cold pressed block obtained in step 1 once, wherein the oxygen partial pressure in the sintering atmosphere is 7.5%, the sintering temperature is 835° C., and the primary sintering time is 15 h, to obtain a Bi-2223 sintered block having a Bi-2223 mass content of 81%;
[0069] Step 3: Place the Bi-2223 sintered block obtained in step 2 in a mold with a diameter of 13 mm for intermediate pressing to obtain a Bi-2223 pressed block with a diameter of 13 mm;
[0070] Step 4: perform secondary sintering on the Bi-2223 pressed block obtained in step 3, with the oxygen partial pressure in the sintering atmosphere being 25%, the sintering temperature being 870° C., and the secondary sintering time being 80 h, to obtain a Bi-2223 high temperature superconducting block.
[0071] According to tests, the superconducting phase content of the Bi-2223 high-temperature superconducting bulk prepared in this embodiment is greater than 95%, the texture degree in the (001) direction is greater than 80%, and the critical current is 98A under 77K self-field conditions.
[0072] Example 5
[0073] like Figure 1 As shown, this embodiment includes the following steps:
[0074] Step 1: cold-pressing Bi-2212 precursor powder with an atomic ratio of Bi, Sr, Ca, and Cu of 2.05:1.85:1.20:1.80 to obtain a Bi-2212 cold-pressed block with a diameter of 7 mm;
[0075] Step 2: sinter the Bi-2212 cold pressed block obtained in step 1 once, the sintering atmosphere is a pure oxygen atmosphere, the sintering temperature is 780° C., and the sintering time is 50 h, to obtain a Bi-2212 sintered block with a texture degree of 43%;
[0076] Step 3: Place the Bi-2212 sintered block obtained in step 2 in a mold with a diameter of 10 mm for intermediate pressing to obtain a Bi-2212 pressed block with a diameter of 10 mm;
[0077] Step 4: perform secondary sintering on the Bi-2212 pressed block obtained in step 3, the sintering atmosphere is pure oxygen atmosphere, the sintering temperature is 885° C., and the secondary sintering time is 40 min to obtain a Bi-2212 high temperature superconducting block.
[0078] According to the test, the superconducting phase content of the Bi-2212 high-temperature superconducting bulk prepared in this embodiment is 98%, the texture degree in the (001) direction is 81%, and the critical current is 45A under the self-field condition of 65K.
[0079] Example 6
[0080] like Figure 1 As shown, this embodiment includes the following steps:
[0081] Step 1: cold-pressing Bi-2212 precursor powder with an atomic ratio of Bi, Pb, Sr, Ca, and Cu of 1.65:0.45:2.00:0.80:2.20 to obtain a Bi-2212 cold-pressed block with a diameter of 10 mm;
[0082] Step 2: sinter the Bi-2212 cold pressed block obtained in step 1 once, the sintering atmosphere is pure oxygen atmosphere, the sintering temperature is 880° C., the sintering time is 15 h, and a Bi-2212 sintered block with a texture degree of 56% is obtained;
[0083] Step 3: Place the Bi-2212 sintered block obtained in step 2 in a mold with a diameter of 13 mm for intermediate pressing to obtain a Bi-2212 pressed block with a diameter of 13 mm;
[0084] Step 4: perform secondary sintering on the Bi-2212 pressed block obtained in step 3, the sintering atmosphere is pure oxygen atmosphere, the sintering temperature is 895° C., and the secondary sintering time is 5 min to obtain a Bi-2212 high temperature superconducting block.
[0085] According to the test, the superconducting phase content of the Bi-2212 high-temperature superconducting bulk prepared in this embodiment is 98.5%, the texture degree in the (001) direction is 85%, and the critical current is 43A under the self-field condition of 65K.
[0086] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a Bi-based high-temperature superconducting block, characterized in that: The method comprises the following steps: Step 1, cold pressing a Bi-based precursor powder having a specific atomic ratio of Bi, Pb, Sr, Ca, and Cu to obtain a Bi-based cold-pressed block with a diameter of R1; the specific atomic ratio of Bi, Pb, Sr, Ca, and Cu in the Bi-based precursor powder is 1.65-1.95: 0.30-0.45: 1.85-2.00: 1.80-2.20: 2.80-3.20; Step 2: sintering the Bi-based cold-pressed block obtained in step 1 to obtain a Bi-based sintered block; Step 3: intermediate pressing the Bi-based sintered block obtained in step 2 to obtain a Bi-based pressed block with a diameter of R2, wherein R2>R1; Step 4: performing secondary sintering on the Bi-based pressed block obtained in step 3 to obtain a Bi-based high temperature superconducting block; The Bi-based high-temperature superconducting block is a Bi-2223 high-temperature superconducting block, the oxygen partial pressure in the sintering atmosphere of the first sintering in step 2 is 0.1%, and the temperature is 770°C~800°C, and the oxygen partial pressure in the sintering atmosphere of the second sintering in step 4 is 7.5%, and the temperature is 810°C~835°C; or the oxygen partial pressure in the sintering atmosphere of the first sintering in step 2 is 7.5%, and the temperature is 810°C~835°C, and the oxygen partial pressure in the sintering atmosphere of the second sintering in step 4 is 25%, and the temperature is 840°C~870°C.
2. The method for preparing a Bi-based high temperature superconducting block according to claim 1, characterized in that: The diameter R1 of the Bi-based cold-pressed block in step 1 is ≥7 mm, the deformation of the intermediate pressing in step 3 is not less than 30%, and R2 / R1 is ≥1.15.
Citation Information
Patent Citations
Method for producing Bi-series high-temperature superconductive wire
CN101075486A
Bismuth series high-temperature superconducting strip and preparation method thereof
CN101465177A
Preparation method for Bi-2212-based high-temperature superconducting block material
CN102807362A
Method for optimizing oxygen content in Bi-2223 phase of superconductive tape and superconductive lead produced by same