A kind of high-efficiency green fluorescent Bi2S3 quantum dot and its preparation method

By using bismuth oxide and hydrobromic acid to react in isopropyl alcohol to generate Bi2S3 quantum dots, and using the morphogens and sulfur sources of thioglycolic acid and thioacetamide, combined with the interfacial reaction of o-phenylenediamine, the Bi2S3 quantum dots were solved Synthesis difficulties have been achieved and efficient green fluorescent Bi2S3 quantum dots have been achieved, which are suitable for biofluorescent probes and imaging.

CN116622373BActive Publication Date: 2024-10-18SHANGHAI UNIV +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310399204.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-18
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

It is difficult to efficiently synthesize Bi2S3 quantum dots with existing technology, resulting in limited applications in biological imaging and molecular fluorescence detection, and low particle size uniformity and low luminescence efficiency.

Method used

The reaction of bismuth oxide and hydrobromic acid is used to generate Bi precursor, combined with thioglycolic acid and thioacetamide as morphogens and sulfur sources, and through the interface reaction between o-phenylenediamine and Bi2S3 particles, a solvothermal method is used in isopropyl alcohol. Synthesize Bi2S3 quantum dots and reduce their surface energy to improve fluorescence efficiency.

Benefits of technology

Green fluorescent Bi2S3 quantum dots with high quantum yield have been achieved. The maximum fluorescence quantum yield reaches 51%. The particle size distribution is uniform and the fluorescence properties are stable. It is suitable for biological fluorescence probes and imaging fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116622373B_ABST
    Figure CN116622373B_ABST
Patent Text Reader

Abstract

The present invention provides a highly efficient green fluorescent Bi2S3 quantum dot and a preparation method thereof. The maximum emission wavelength of the Bi2S3 quantum dot is 502nm, and it can be excited by near-ultraviolet light, purple light or blue light of 360nm to 475nm, and the maximum excitation wavelength band is located at 409nm to 460nm. The emission spectrum of the synthesized Bi2S3 quantum dot has the characteristics of excitation wavelength independence, and the absolute quantum yield of fluorescence reaches 51%. The Bi2S3 quantum dot has good dispersibility in the solution and a narrow particle size distribution of about 4nm. The fluorescence performance of the synthesized Bi2S3 quantum dot has good stability in a dilute solution. The present invention does not use complex equipment, has a short synthesis time and low cost. The Bi2S3 quantum dot has good biocompatibility and can be applied to the fields of biological molecule fluorescence labeling, biological imaging and biological fluorescence probes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a highly efficient green fluorescent Bi 2 S 3 Quantum dots and their preparation method are applied in the field of fluorescent quantum dot nanomaterial technology. Background Art

[0002] Quantum dots generally refer to nanoparticles with a particle size of less than 10nm. They have fluorescent properties related to their particle size. Inorganic fluorescent quantum dots usually have the characteristics of high synthesis efficiency, high fluorescence efficiency and stable fluorescence performance. They are widely used in various aspects such as biological imaging, sensing, lighting, biomedicine, etc.

[0003] Traditional II-VI semiconductor quantum dots have the advantages of narrow half-width, high luminescence efficiency, and adjustable luminescence color, but CdS / CdSe / CdTe quantum dots are biotoxic, which limits the wide application of CdS / CdSe / CdTe quantum dots in bio-imaging and bio-detection. 3+ The compounds can be used as human medicines to treat diseases caused by Helicobacter pylori and other diseases, and have low biological toxicity. Bismuth sulfide is environmentally friendly, chemically stable, and non-toxic to the human body. Due to its good biocompatibility, Bi 2 S 3 Quantum dot fluorescent materials have good application prospects in biological imaging, molecular fluorescence detection, etc. However, the band gap width of bismuth sulfide at room temperature is Eg = 1.3eV, and the synthetic fluorescence is in the visible region of Bi 2 S 3 Quantum dot fluorescent materials are a challenging research task. 2 S 3 There are few reports on fluorescent quantum dots in the literature, because the synthesis of high-efficiency Bi 2 S 3 The research work on quantum dots is difficult. The applicant used 11-mercaptoundecanoic acid as a morphogen and acetylacetone as a ligand to control Bi 2 S 3 The nucleation rate of the particles was regulated by the synthesis of Bi with a maximum emission wavelength of 500 nm in the aqueous phase. 2 S 3 Quantum dots (Journal of Shanghai University, 2019, 25: 227-234.). In the aqueous phase, Bi 2 S 3 The particle size uniformity of the particles is difficult to control. 2 S 3 The particles are not very efficient at emitting light.

[0004] Therefore, a high quantum yield green fluorescent Bi 2 S 3Methods for synthesizing quantum dots. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a high-efficiency green fluorescent Bi 2 S 3 Quantum dots and a preparation method thereof, wherein a Bi precursor generated by the reaction of bismuth oxide and hydrobromic acid is dissolved in isopropanol, thioglycolic acid is used as a morphology agent, thioacetamide is used as a sulfur source, and o-phenylenediamine is reacted with Bi to form a quantum dot. 2 S 3 The interface reaction of particles reduces Bi 2 S 3 A green fluorescent Bi with a quantum yield of 51% was synthesized by solvothermal method. 2 S 3 Quantum dots. The particle size ranges from 3 to 6 nm. Under the excitation of light at 360 to 475 nm, they can emit bright green fluorescence, with a maximum excitation wavelength of 460 nm and a maximum emission wavelength of 502 nm. This synthesis method is simple and fast. 2 S 3 Quantum dots are also easily dispersed in solvents such as ethanol, toluene, and tetrahydrofuran. Their fluorescence properties in the solution are stable, and they can maintain bright green fluorescence after being left at room temperature for several months.

[0006] To achieve the above object, the present invention adopts the following technical solution, comprising the following steps:

[0007] a. The reaction was carried out in a molar ratio of bismuth oxide to hydrobromic acid of 1:9, and the reaction was carried out at 100° C. with electromagnetic stirring for 3 to 4 hours. The water was evaporated to obtain a yellow-green viscous oily liquid as a bismuth precursor for the reaction.

[0008] b. Dissolve the bismuth precursor in isopropanol, add thioglycolic acid at a ratio of 1:2 to 1:4 between the amount of bismuth and thioglycolic acid, and react for 30 to 50 minutes under electromagnetic stirring in a nitrogen atmosphere. Add an isopropanol solution of thioacetamide (about half the amount of bismuth), heat to 90°C, and reflux for 1 hour. After cooling, transfer the mixed solution into a polytetrafluoroethylene reactor and react at 130°C for 1 hour.

[0009] c. After cooling to room temperature, add 5-8 mg of o-phenylenediamine to the mixed solution. After stirring and dissolving, continue to react in a polytetrafluoroethylene reactor at 120-150°C for 0.5-2.5 hours, and then cool to room temperature.

[0010] d. Adjust the pH of the mixed solution to 6 with an aqueous solution of NaOH, and then dialyze it with a 3500Da semipermeable membrane for 48 hours to remove small molecules and obtain bright green fluorescent Bi 2 S 3Quantum dots, content 1.5mg / mL.

[0011] The green Bi synthesized by the present invention 2 S 3 The fluorescent quantum dots emit light stably in the solution, and the fluorescence quantum yield reaches 51%.

[0012] In order to improve Bi 2 S 3 Uniformity of particle size distribution of quantum dots, design of Bi synthesis using non-aqueous phase 2 S 3 Quantum dots. 2 O 3 The Bi precursor H was synthesized by reacting with excess HBr to form a yellow-green oil that is easily soluble in isopropanol. 3 Bi 2 Br 9 . 3 Bi 2 Br 9 Dissolved in isopropanol, using thioglycolic acid as a morphogen. 3+ It is easy to form a stable chemical bond with the S atom in the thiol group, and the H 2 S is the sulfur source, synthesizing Bi with high particle size distribution uniformity 2 S 3 For quantum dots, the synthesis route is designed as follows.

[0013] Synthetic route 1:

[0014]

[0015] In order to improve Bi 2 S 3 The fluorescence quantum luminescence efficiency of quantum dots is improved by using a small amount of o-phenylenediamine and Bi 2 S 3 Quantum dot-1 particle surface reacts to stabilize Bi 2 S 3 The surface energy of quantum dots can reduce the probability of non-radiative transitions, greatly improving the Bi 2 S 3 The fluorescence quantum luminescence efficiency of quantum dots. The designed synthesis route is as follows.

[0016] Synthesis route 2:

[0017]

[0018] Synthetic Bi 2 S 3 The quantum dot morphogen is not limited to thioglycolic acid, but can also be sodium thioglycolate, L-cysteine, or other carboxylic acid ligands containing thiol groups. 2S 3 The stabilizing agent for the surface energy of quantum dots is not limited to o-phenylenediamine, and other aromatic compounds containing two amino groups at the ortho position may also be selected, such as 1,2-diaminonaphthalene, 2,3-diaminonaphthalene, 1,8-diaminonaphthalene, etc.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] In the present invention, the applicant synthesizes a Bi precursor by reacting bismuth oxide with hydrobromic acid, and the Bi precursor is easily soluble in isopropanol. Then, thioacetamide is used as a sulfur source, thioglycolic acid is used as a morphology agent, and o-phenylenediamine is reacted with Bi to form a Bi precursor. 2 S 3 The interfacial reaction of the particles stabilizes Bi 2 S 3 The surface energy of the particles increases 2 S 3 The fluorescence efficiency of quantum dots is very high, and bright green fluorescent Bi 2 S 3 Quantum dots, the maximum fluorescence quantum yield reached 51%, the prepared Bi 2 S 3 Quantum dots have good fluorescence stability in solution and can be used in the fields of bioluminescent probes, bioluminescent imaging, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The green fluorescent Bi obtained in Example 1 of the present invention 2 S 3 Fluorescence emission spectrum of a 64-fold diluted isopropanol solution of quantum dots under 460nm light excitation. The inset is a photograph of its green fluorescence under 365nm light irradiation.

[0022] Figure 2 The green fluorescent Bi obtained in Example 1 of the present invention 2 S 3 The excitation spectrum of the isopropanol solution of quantum dots diluted 64 times at a detection wavelength of 502nm.

[0023] Figure 3 The green fluorescent Bi obtained in Example 1 of the present invention 2 S 3 Emission spectra of isopropanol solutions of quantum dots diluted 64 times at different excitation wavelengths.

[0024] Figure 4 The green fluorescent Bi prepared by the present invention 2 S 3 High-resolution transmission electron microscopy (HRTEM) of quantum dots, with the inset showing green fluorescent Bi 2 S 3Characteristic lattice diffraction fringes of quantum dots.

[0025] Figure 5 The green fluorescent Bi obtained in Example 1 of the present invention 2 S 3 Particle size distribution of quantum dots.

[0026] Figure 6 The green fluorescent Bi obtained in Example 1 of the present invention 2 S 3 Infrared absorption spectrum of quantum dots.

[0027] Figure 7 The green fluorescent Bi obtained in Example 1 of the present invention 2 S 3 The fluorescence intensity of quantum dots at an emission wavelength of 502 nm changes with time. DETAILED DESCRIPTION

[0028] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0029] Any features such as preparation methods, materials, structures or composition ratios that are not clearly described in this technical solution shall be deemed as common technical features disclosed in the prior art.

[0030] In the following examples, the raw materials used are all commercially available.

[0031] Embodiment 1:

[0032] See Synthesis Route 1, Bi 2 S 3 The synthesis of quantum dot-1 includes the following steps:

[0033] a.Bi Precursor H 3 Bi 2 Br 9 Synthesis. 2.33g bismuth oxide (5mmol), add 6.0mL 48% hydrobromic acid to react, stir with electromagnetic, react at 100℃ for 4-6h, evaporate water and excess HBr to obtain oily viscous yellow-green liquid, slowly crystallize at below 10℃ to obtain 5.7g yellow-green crystals, the composition of which is H 3 Bi 2 Br 9 , the yield is close to 100%.

[0034] b.Bi 2 S3 Synthesis of quantum dots-1. 0.116 g H 3 Bi 2 Br 9 (0.10mmol) was dissolved in 20mL isopropanol, 30μL thioglycolic acid was added, nitrogen was protected, and the reaction was carried out at 30-40℃ for 30-60min. Then the temperature was raised to 90℃, and an isopropanol solution containing 11.3mg thioacetamide was added, and the reaction was refluxed for 1-1.5h. Naturally cooled to room temperature, the mixed solution was transferred to a polytetrafluoroethylene reactor, and the reaction was carried out at 130℃ for 1h. The pH of the solution was adjusted to 4-5 with NaOH solution to obtain green fluorescent Bi 2 S 3 Quantum dot-1.

[0035] c.Bi 2 S 3 For the synthesis of quantum dot-2, see Synthesis Route 2. 2 S 3 Add 5-8 mg of o-phenylenediamine to the quantum dot-1 solution (only for surface modification reaction, the excess o-phenylenediamine is removed during purification), and continue to react at 130°C for 1-1.5 hours in a polytetrafluoroethylene reactor. Cool naturally to room temperature, adjust the pH of the solution to 5-6 with NaOH solution, and the fluorescence brightness of the solution is similar to that of Bi 2 S 3 Compared with the solution of quantum dots-1, the fluorescence intensity is significantly enhanced.

[0036] d.Bi 2 S 3 Purification of quantum dots-2. Dialyze with a semipermeable membrane with a molecular weight of 3500Da for 48 hours to remove small molecules and obtain bright green fluorescent Bi 2 S 3 Quantum dots, content 1.5mg / mL.

[0037] Figure 1 is the Bi prepared in Example 1 2 S 3 Fluorescence emission spectrum of isopropanol solution of quantum dots, the maximum emission wavelength is 502nm, the inset is the fluorescence photograph under 365nm ultraviolet light, the absolute fluorescence quantum yield reaches 51%.

[0038] Figure 2 is the Bi prepared in Example 1 2 S 3The fluorescence excitation spectrum of the isopropanol solution of quantum dots is a wide excitation absorption band from 360nm to 475nm. A 365nm ultraviolet lamp can be used as the excitation light source, or a 400-450nm purple light or a 450-475nm blue light can be used as the excitation light source. The maximum excitation wavelength is located in a wide and strong excitation absorption band of 409-460nm.

[0039] Figure 3 It shows that under the excitation of 370-470nm light, the Bi prepared in Example 1 2 S 3 The shape of the fluorescence emission spectrum of quantum dots remains unchanged, and their fluorescence color is independent of the excitation wavelength.

[0040] Figure 4 is the Bi prepared in Example 1 2 S 3 High-resolution transmission electron microscopy image of quantum dots. The particles are spherical and evenly dispersed. The illustration is Bi 2 S 3 The lattice fringes of quantum dots, their interplanar spacing Corresponding to Bi 2 S 3 The

[520] interplanar spacing (PDF#17-0320) proves that Bi 2 S 3 Successful synthesis of quantum dots.

[0041] Figure 5 is the Bi prepared in Example 1 2 S 3 The particle size distribution of quantum dots shows that Bi 2 S 3 The particles are evenly distributed and the particle size is about 4nm.

[0042] Figure 6 is the Bi prepared in Example 1 2 S 3 Infrared absorption spectrum of quantum dots. As shown in the figure, 3400cm -1 The broad absorption peak is the stretching vibration absorption peak of -COO-H of thioglycolic acid, 1631 cm -1 and 1383cm -1 Thioglycolic acid-COO - The asymmetric and symmetric stretching vibration absorption peaks are located at 3448cm -1 The weak and narrow single peak is the -NH- characteristic absorption peak of o-phenylenediamine. 2 There are two weak and narrow absorption peaks, while -NH- has one weak absorption peak, indicating that o-phenylenediamine reacts with Bi 2 S 3 Bi on the particle surface 3+During the reaction, -NH 2 The group removes one hydrogen atom and forms -NH- with Bi 2 S 3 Bi on the particle surface 3+ Combined. Located at 1590cm -1 The stronger absorption peak is the vibration absorption peak of the benzene ring skeleton of o-phenylenediamine, located at 1350cm -1 The absorption peak is the stretching vibration absorption peak of -NC- of o-phenylenediamine. - The asymmetric and symmetric stretching vibration absorption peaks are very strong, and the vibration absorption peak of the benzene ring skeleton is of medium intensity. 2 -2850~2980cm -1 The region has a strong double-peak characteristic stretching vibration absorption peak. Figure 6 It shows that in Bi 2 S 3 Most of the thioglycolic acid molecules on the particle surface were replaced by o-phenylenediamine molecules.

[0043] Figure 7 Indicate Bi 2 S 3 The fluorescence performance of quantum dots in isopropanol solution is relatively stable. After being placed naturally for 7 days, the fluorescence performance maintains more than 90% of its intensity, and after being placed naturally for 60 days, the fluorescence performance maintains more than 80%. After being placed in natural conditions for several months, it can emit strong green fluorescence under ultraviolet light.

[0044] From the above, it can be seen that the Bi prepared by the present invention 2 S 3 The characteristics of quantum dots are:

[0045] 1. Bi synthesized by the present invention 2 S 3 Quantum dots, with an absolute quantum efficiency of 51%.

[0046] 2.Bi 3+ The compound can be used for human medicine and has good compatibility with biological molecules. 2 S 3 Quantum dots can be used in the fields of luminescent labeling of biomolecules, fluorescence imaging analysis of biomolecules, and fluorescent probes of biomolecules.

[0047] 3. Bi synthesized by the present invention 2 S 3 The fluorescence properties of quantum dots in dilute solutions are relatively stable and they can be left under natural conditions for more than half a year and still emit bright green fluorescence.

[0048] 4. Bi synthesized by the present invention 2 S 3The emission spectrum of quantum dots is independent of the excitation wavelength.

[0049] 5. Bi synthesized by the present invention 2 S 3 The excitation wavelength range of quantum dots is wide, 360nm to 475nm, and near-ultraviolet light, purple light, and blue light can be used as excitation light sources.

[0050] 6. The present invention does not use complicated equipment, has a short reaction time and a low synthesis cost.

[0051] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing highly efficient green fluorescent Bi2S3 quantum dots, characterized by: The reaction is carried out with a molar ratio of bismuth oxide and hydrobromic acid of 2:9, and the reaction is carried out at 100°C with electromagnetic stirring for 3 to 4 hours, and the water is evaporated to obtain a yellow-green viscous oily liquid as a bismuth precursor for the reaction; the bismuth precursor is dissolved in isopropanol, and the morphology agent is added at a molar ratio of bismuth element to morphology agent of 1:2 to 1:4, and the reaction is carried out with electromagnetic stirring for 30 to 50 minutes in a nitrogen atmosphere; an isopropanol solution of thioacetamide is added, the temperature is raised to 90°C, and the reaction is refluxed for 1 hour; after cooling, the mixed solution is transferred to a polytetrafluoroethylene reactor and reacted at 130°C for 1 to 1.5 hours; after cooling to room temperature, 5 to 8 mg of a surface energy stabilizing agent is added to the mixed solution; after stirring and dissolving, the reaction is continued at 120 to 150°C in the polytetrafluoroethylene reactor for 0.5 to 2.5 hours, and then cooled to room temperature; the pH of the mixed solution is adjusted to 6 with an aqueous solution of NaOH, and then 3500 Da was dialyzed through a semipermeable membrane for 48 h to remove small molecules and obtain Bi2S3 quantum dots with bright green fluorescence; The morphology agent is thioglycolic acid; The surface energy stabilizing agent used is o-phenylenediamine.

2. The highly efficient green fluorescent Bi2S3 quantum dots prepared by the preparation method according to claim 1 are characterized in that: The particle size ranges from 3 to 6 nm. Under light excitation from 360 nm to 475 nm, it emits bright green fluorescence, and the absolute quantum yield of fluorescence reaches 51%.

Citation Information

Cited By

  • Preparation method of PMMA (Polymethyl Methacrylate) composite fluorescent film for converting electroluminescence of LED (Light Emitting Diode) chip into white light

    CN117106274A

  • Method for preparing pmma composite fluorescent film for converting electroluminescence of led chip into white light

    CN117106274B