A method of distillative extraction of germanium
By treating coal ash using distillation and alkaline leaching methods, the complex composition and structure issues in germanium extraction were resolved, achieving efficient germanium dissociation and enrichment, and improving germanium recovery rate and economic benefits.
Patent Information
- Application Number
- CN202310763560.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-06-27
AI Technical Summary
Existing technologies struggle to efficiently extract germanium from power plant coal ash, especially due to its complexity involving multiple components, structures, and phases, which leads to low germanium recovery rates.
A method combining distillation with hydrochloric acid and alkali leaching is used to treat coal ash. Through steps such as slurry preparation, distillation, filtration, and hydrolysis, germanium is efficiently dissociated and enriched. The process includes distillation in a distillation kettle, pressurized or atmospheric pressure alkali leaching, filtration, washing, and neutralization.
It achieves efficient extraction and high recovery rate of germanium, with a simple and easy-to-operate process, significantly improving economic benefits.
Smart Images

Figure CN116623019B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of mining engineering technology, and specifically relates to a method for extracting germanium by distillation. Background Technology
[0002] The main methods for germanium extraction, both domestically and internationally, include: classical chlorination, volatilization, zinc powder displacement, distillation (alkaline earth metal chlorination distillation), fumigation, extraction (liquid membrane extraction), and ion exchange. However, classical chlorination, zinc powder displacement, extraction (liquid membrane extraction), and ion exchange all rely on extracting, separating, and enriching germanium from enriched germanium raw materials (dust or germanium-containing aqueous solutions). Germanium oxide in power plant coal ash exists in tetragonal and hexagonal germanium crystal structures, while germanium compounds exist as ferric germanate, calcium germanate, zinc germanate, etc., and some exist in solid solutions, such as SiO2·GeO2 and Al2O3·GeO2. During germanium dust leaching, due to the different crystal structures, complex composition, diverse phases, and intermingling, conventional acid-base leaching and reduction volatilization methods are difficult to achieve efficient germanium enrichment, resulting in low recovery rates. Therefore, developing a method that can solve the above technical problems is essential. Summary of the Invention
[0003] The purpose of this invention is to provide a method for distilling and extracting germanium from coal ash, where the germanium content is low, making it a highly efficient source for dissolving and dissociating multi-component, multi-structure, and multi-phase Ge materials. This method primarily controls the orientation of the metallic element Ge to achieve effective extraction. The process is simple and easy to operate, with a high direct recovery rate of Ge, resulting in significant economic benefits. This invention involves: (1) mixing coal ash, hydrochloric acid, and additives (NaCl, KCl, H3PO4, H2O2, KMnO4, etc.) into a slurry, pumping it into a distillation kettle for distillation to obtain distillate fraction I and residual slurry. The residual slurry is then filtered and washed to obtain washing residue I and washing liquid II; (2) washing residue I is then mixed with alkali (NaOH, KOH, etc.) for pressure leaching; (3) the pressure leached material is filtered and washed to obtain washing residue II and washing liquid III. Washing residue II is stockpiled; (4) distillate fraction I is hydrolyzed and dried to obtain GeO2; (5) washing liquid II and washing liquid III are neutralized and precipitated to obtain neutralized residue III and neutralized liquid IV. Neutralized liquid IV is returned to the water leaching residue washing and residual slurry washing, and neutralized residue III is returned to chlorination distillation. This method has a short and simple process flow, is easy to operate, and can achieve efficient dissociation and enrichment of germanium in coal ash.
[0004] Alternatively, the following steps can be taken: (1) Coal ash, hydrochloric acid, and additives (NaCl, KCl, H3PO4, H2O2, KMnO4, etc.) are mixed into a slurry and pumped into a distillation kettle for distillation to obtain distillate fraction I and residual slurry. The residual slurry is then filtered and washed to obtain washing residue I and washing liquid II; (2) Washing residue I is then mixed with alkali (NaOH, KOH, etc.) for high-temperature and atmospheric-pressure leaching; (3) The atmospheric-pressure leaching material is filtered and washed to obtain washing residue II and washing liquid III. Washing residue II is stockpiled; (4) Distillate fraction I is hydrolyzed and dried to obtain GeO2; (5) Washing liquid II and washing liquid III are neutralized and precipitated to obtain neutralized residue III and neutralized liquid IV. Neutralized liquid IV is returned to the water leaching residue washing and residual slurry residue washing, and neutralized residue III is returned to chlorination distillation. This method has a short and simple process flow, and the procedures are easy to operate. Germanium in coal ash can be efficiently dissociated and enriched.
[0005] The objective of this invention is achieved by including distillation and post-treatment steps, specifically including: A. Distillation: 1) Add hydrochloric acid and additives to coal ash to make a slurry to obtain material a; 2) Material a is distilled to obtain slurry b and distillate c; 3) Hydrolyze the distillate c in dilute hydrochloric acid solution, and then dry it to obtain GeO2; B. Post-processing: 1) The residual slurry b is filtered and washed to obtain washing residue e and residual slurry mixture f; the residual slurry mixture f consists of distillation residue and residual washing liquid; 2) After adding alkali to the washing residue e, perform alkaline leaching under normal or pressure, then filter and wash to obtain washing residue g and alkaline leaching mixture h. The alkaline leaching mixture h and residual slurry mixture f are neutralized to obtain neutralized residue and neutralized liquid; the neutralized liquid is returned to the filtration and washing step.
[0006] The specific steps are as follows: (1) After preparing the slurry with coal ash, hydrochloric acid, and additives (NaCl, KCl, H3PO4, H2O2, KMnO4, etc.), the mixture is pumped into a distillation kettle for distillation. Distillation conditions: distillation temperature 80℃~200℃, distillation l:s ratio 1:1~5:1, HCl concentration 6 mol / L~12 mol / L, and pH value at the distillation endpoint <0.5. The distillate can be prepared with 0.1%~20% NaCl / KCl (based on coal ash mass) and 0.1%~20% H3PO4 / HF / HNO3 / H2O2 / KMnO4 (based on coal ash mass).
[0007] (2) The distillation residue is filtered and washed, and the distillation residue and the residue washing liquid are mixed to obtain a residue mixture. The pH value of the washing liquid is less than 0.5, and the washing liquid is adjusted with HCl.
[0008] (3) After distillation and washing, the residue is mixed with alkali (NaOH, KOH, LiOH, choline (HOCH2CH2N(CH3)3(OH)), quaternary ammonium alkali (NR4OH), sodium alkoxide, etc.) and then subjected to pressure alkali leaching. Alkali leaching conditions: alkali leaching temperature 100℃~200℃, time 0.1h~10h, l:s=1:1~20:1, alkali concentration 10g / L~400g / L, mechanical stirring speed 20r / min~1000r / min, pH value at the end of alkali leaching >13.5.
[0009] (4) After alkali soaking, filter and wash, and mix the filtrate and washing solution to obtain a water soaking mixture; the pH value of the alkali soaking washing solution is greater than 13.5, and the washing solution is prepared with an alkali with the same cation as the alkali used in alkali dissolution.
[0010] (5) Neutralize the alkaline leaching mixture and the residual slurry mixture to a pH of 1-4.1.
[0011] (6) Hydrolyze the distillate fraction. Hydrolyze with 2 mol / L dilute hydrochloric acid solution. After hydrolysis, filter, wash and dry to obtain germanium oxide.
[0012] Alternatively, you can do the following: (1) After preparing the slurry with coal ash, hydrochloric acid, and additives (NaCl, KCl, H3PO4, H2O2, KMnO4, etc.), the mixture is pumped into a distillation kettle for distillation. Distillation conditions: distillation temperature 80℃~200℃, distillation l:s ratio 1:1~5:1, HCl concentration 6 mol / L~12 mol / L, and pH value at the distillation endpoint <0.5. The distillate can be prepared with 0.1%~20% NaCl / KCl (based on coal ash mass) and 0.1%~20% H3PO4 / HF / HNO3 / H2O2 / KMnO4 (based on coal ash mass).
[0013] (2) The distillation residue is filtered and washed, and the distillation residue and the residue washing liquid are mixed to obtain a residue mixture. The pH value of the washing liquid is less than 0.5, and the washing liquid is adjusted with HCl.
[0014] (3) The distillation residue is leached under normal pressure with alkali (NaOH, KOH, LiOH, choline (HOCH2CH2N(CH3)3(OH)), quaternary ammonium alkali (NR4OH), sodium alkoxide, etc.). Alkali leaching conditions: leaching temperature room temperature ~ 100℃, leaching time 0.1h ~ 10h, l:s = 1:1 ~ 20:1, alkali concentration 10g / L ~ 400g / L, mechanical stirring speed 20r / min ~ 1000r / min, pH value at the end of leaching > 13.5.
[0015] (4) After alkali soaking, filter and wash, and mix the filtrate and washing solution to obtain a water soaking mixture; the pH value of the alkali soaking washing solution is greater than 13.5, and the washing solution is prepared with an alkali with the same cation as the alkali used in alkali dissolution.
[0016] (5) Neutralize the alkaline leaching mixture and the residual slurry mixture to a pH of 1-4.1.
[0017] (6) Hydrolyze the distillate fraction. Hydrolyze with 2 mol / L dilute hydrochloric acid solution. After hydrolysis, filter, wash and dry to obtain germanium oxide. Attached Figure Description
[0018] Figure 1 This is a schematic diagram of the process flow of the present invention; Figure 2 This is a schematic diagram of another process flow of the present invention. Detailed Implementation
[0019] The present invention will be further described below with reference to embodiments, but this is not intended to limit the present invention in any way. Any modifications or substitutions made based on the teachings of the present invention shall fall within the protection scope of the present invention.
[0020] The method for extracting germanium by distillation according to the present invention includes distillation and post-processing steps, specifically including: A. Distillation: 1) Add hydrochloric acid and additives to coal ash to make a slurry to obtain material a; 2) Material a is distilled to obtain slurry b and distillate c; 3) Hydrolyze the distillate c in dilute hydrochloric acid solution, and then dry it to obtain GeO2; B. Post-processing: 1) The residual slurry b is filtered and washed to obtain washing residue e and residual slurry mixture f; the residual slurry mixture f consists of distillation residue and residual washing liquid; 2) After adding alkali to the washing residue e, perform alkaline leaching under normal or pressure, then filter and wash to obtain washing residue g and alkaline leaching mixture h. The alkaline leaching mixture h and residual slurry mixture f are neutralized to obtain neutralized residue and neutralized liquid; the neutralized liquid is returned to the filtration and washing step.
[0021] The additive mentioned in step 1) is one or more of NaCl, KCl, H3PO4, H2O2 and KMnO4.
[0022] The amount of additives mentioned in step 1) is 0.1% to 20% of the mass of coal ash.
[0023] The distillation conditions in step 2) are: distillation temperature 80℃~200℃, distillation l:s ratio 1:1~5:1 (the volume ratio of liquid to solid during distillation is 1:1~5:1), HCl concentration 6 mol / L~12 mol / L, and pH value at the distillation endpoint <0.5.
[0024] The concentration of the dilute hydrochloric acid solution mentioned in step 3) is 1 mol / L to 3 mol / L.
[0025] The base mentioned in step 2) is one or more of NaOH, KOH, LiOH, choline (HOCH2CH2N(CH3)3(OH)), quaternary ammonium base (NR4OH) and sodium alkoxide.
[0026] The atmospheric pressure alkaline leaching conditions described in step 2) are as follows: alkaline leaching temperature: room temperature to 100℃; time: 0.1h to 10h; l:s = 1:1 to 20:1 (the volume ratio of liquid to solid during alkaline leaching is 1:1 to 20:1); alkaline concentration: 10g / L to 400g / L; mechanical stirring speed: 20r / min to 1000r / min; and pH value at the end of alkaline leaching: >13.5.
[0027] The pressurized alkali leaching conditions described in step 2) are as follows: alkali leaching temperature 100℃~200℃, time 0.1h~10h, l:s=1:1~20:1 (the volume ratio of liquid to solid during alkali leaching is 1:1~20:1), alkali concentration 10g / L~400g / L, mechanical stirring speed 20r / min~1000r / min, and pH value at the end of alkali leaching >13.5.
[0028] The invention will be further illustrated below with specific implementation examples: Example 1 (1) 100g of coal ash is mixed with 500ml of 35%~37% hydrochloric acid, and additives NaCl 10g, 17g of 85% H3PO4, and 10ml of 27% H2O2. After mixing, the mixture is pumped into a distillation kettle for distillation. Distillation conditions: distillation temperature 140℃, distillation l:s ratio 5:1, HCl concentration 7mol / L, and pH value at the distillation endpoint <0.5.
[0029] (2) The distillation residue is filtered and washed, and the distillation residue and the residue washing liquid (HCl concentration 20g / L) are mixed to obtain the residue mixture.
[0030] (3) 50g of distilled residue (dry weight) was mixed with 160g of NaOH. The mixture was leached for 1h under the conditions of liquid-solid ratio of 16:1, pressure leaching temperature of 150℃, and stirring speed of 500r / min.
[0031] (4) After pressurized alkaline leaching, filter and wash. Mix the filtrate and washing solution to obtain a water leaching mixture. The washing solution is a 15 g / L NaOH solution.
[0032] (5) Neutralize the alkaline leaching mixture and the residual slurry mixture to a pH of 1-3.
[0033] (6) Hydrolyze the distillate fraction. Hydrolyze with 2 mol / L dilute hydrochloric acid solution. After hydrolysis, filter, wash and dry to obtain germanium oxide.
[0034] (7) After extraction, separation and enrichment, the germanium content in the coal ash decreased from 3657 g / t in the coal ash to 240 g / t in the water-leached residue, and the germanium recovery rate reached 98.33%.
[0035] Example 2 (1) 400g of coal ash was mixed with 1600ml of 35%~37% hydrochloric acid, 40g of NaCl, 68g of 85% H3PO4, and 10ml of analytical grade HF. After mixing, the mixture was pumped into a distillation kettle for distillation. Distillation conditions: distillation temperature 140℃, distillation l:s ratio 4:1, HCl concentration 6.5mol / L, and pH value at the distillation endpoint <0.5.
[0036] (2) The distillation residue is filtered and washed, and the distillation residue and the residue washing liquid (HCl concentration 20g / L) are mixed to obtain the residue mixture.
[0037] (3) 160g of distilled residue (dry residue) was mixed with 192g of NaOH. The residue was leached for 2 hours at a liquid-to-solid ratio of 8:1, a normal pressure leaching temperature of 85℃~90℃, and a stirring speed of 600r / min.
[0038] (4) After leaching with alkaline solution under normal pressure, filter and wash. Mix the filtrate and washing solution to obtain a water leaching mixture. The washing solution is a 15 g / L NaOH solution.
[0039] (5) Neutralize the alkaline leaching mixture and the residual slurry mixture to a pH of 1-3.
[0040] (6) Hydrolyze the distillate fraction. Hydrolyze with 2 mol / L dilute hydrochloric acid solution. After hydrolysis, filter, wash and dry to obtain germanium oxide.
[0041] (7) After extraction, separation and enrichment, the germanium content in the coal ash decreased from 3657 g / t in the coal ash to 335 g / t in the water-leached residue, and the germanium recovery rate reached 97.17%.
Claims
1. A method for extracting germanium by distillation, characterized in that, It includes distillation and post-processing steps, specifically including: A. Distillation: 1) Add hydrochloric acid, one or more of NaCl, KCl, H3PO4, H2O2 and KMnO4 as additives to coal ash, and adjust the slurry to obtain material a; 2) Material a is distilled to obtain slurry b and distillate c; 3) Hydrolyze the distillate c in dilute hydrochloric acid solution, and then dry it to obtain GeO2; B. Post-processing: 1) The residual slurry b is filtered and washed to obtain washing residue e and residual slurry mixture f; the residual slurry mixture f consists of distillation residue and residual washing liquid; 2) Add one or more of the following alkalis to the washing residue e: NaOH, KOH, LiOH, quaternary ammonium alkali, and sodium alkoxide, and then perform alkaline leaching under normal or pressure. After filtration and washing, wash residue g and alkaline leaching mixture h are obtained. Alkaline leaching mixture h and residual slurry mixture f are neutralized to obtain neutralized residue and neutralized liquid. Neutralized residue is returned to chlorination distillation, and neutralized liquid is returned to the filtration and washing step.
2. The method for distilling and extracting germanium according to claim 1, characterized in that, The amount of additives mentioned in step 1) is 0.1-20% of the mass of coal ash.
3. The method for distilling and extracting germanium according to claim 1, characterized in that, The distillation conditions in step 2) are: distillation temperature 80℃~200℃, distillation l:s ratio 1:1~5:1, HCl concentration 6mol / L~12mol / L, and final pH value <0.
5.
4. The method for distilling and extracting germanium according to claim 1, characterized in that, The concentration of the dilute hydrochloric acid solution mentioned in step 3) is 1 mol / L to 3 mol / L.
5. The method for distilling and extracting germanium according to claim 1, characterized in that, The atmospheric pressure alkaline leaching conditions described in step 2) are as follows: alkaline leaching temperature: room temperature to 100℃; time: 0.1h to 10h; l:s = 1:1 to 20:1; alkaline concentration: 10g / L to 400g / L; mechanical stirring speed: 20r / min to 1000r / min; and pH value at the end of alkaline leaching: >13.
5.
6. The method for distilling and extracting germanium according to claim 1, characterized in that, The pressurized alkali leaching conditions described in step 2) are as follows: alkali leaching temperature 100℃~200℃, time 0.1h~10h, l:s=1:1~20:1, alkali concentration 10g / L~400g / L, mechanical stirring speed 20r / min~1000r / min, and pH value at the end of alkali leaching >13.5.
Citation Information
Patent Citations
Method for recovery germanium from germanium-containing flue dust
CN103173624A
Method for recycling germanium from distillation reacted acid
CN106498163A