Zirconium oxide particles, powder compacts, and methods for producing the same

By oscillating the filling of zirconia particles in the columnar mold and controlling the compression ratio, combined with (meth)acrylic binder and yttrium oxide, the problem of uneven density of zirconia preburned body and sintered body is solved, and high light transmission is achieved Preparation of zirconia sintered bodies with high strength and high strength.

CN116648430BActive Publication Date: 2024-11-26KURARAY NORITAKE DENTAL
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
CN202180086946.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-22
Filing Date
2021-12-22
Publication Date
2024-11-26
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

The prior art is difficult to obtain high-density and uniform density zirconia preburned bodies and sintered bodies, especially at low pressures, density unevenness caused by uniaxial pressurization and difficulty in removing binder. The intensity is difficult to achieve.

Method used

By oscillating the filling of zirconia particles in a columnar mold, and controlling the compression ratio between 0.46 and 0.53 when uniaxially pressurized to 33MPa, using (meth)acrylic binder and yttrium oxide as stabilizers, ensuring that the particles are under low pressure Evenly form to avoid carbonization of the binder.

Benefits of technology

It is achieved to obtain a uniform density pressed powder under low pressure, thereby obtaining a zirconia sintered body with high light transmittance and high intensity, which is suitable for dental materials and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116648430B_ABST
    Figure CN116648430B_ABST
Patent Text Reader

Abstract

The present invention provides particles and powder compacts suitable for obtaining highly translucent and high-strength zirconium oxide sintered bodies and high-density and uniform calcined bodies, and methods for producing the same. The present invention relates to particles containing zirconium oxide, a stabilizer capable of inhibiting the phase transformation of zirconium oxide, and a binder. The particles are filled by oscillation into a columnar mold in accordance with JIS R 1628:1997, and compressed at a rate of 1 mm / sec by uniaxial pressing. When heated to 33 MPa, the compression ratio R calculated by the following formula (1) becomes 0.46 to 0.53. R = (H-D) / H (1). (In the formula, H represents the height of the particles filled by oscillation in the columnar mold before pressurization, and D represents the deformation amount until 33 MPa is reached).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to particles and a powder compact for obtaining a high-density and uniform zirconium oxide (zirconium oxide (IV): ZrO2) calcined body and a highly translucent and high-strength zirconium oxide sintered body, and a method for producing the same. Background Art

[0002] Generally speaking, when ceramic powder or particles are calcined, they shrink depending on the calcination temperature. This shrinkage occurs based on the primary particle density and internal stress inside the ceramic powder. Therefore, for a sintered body obtained by calcining a pressed body of ceramic powder or particles, it is necessary to produce a high-density and uniform pressed body.

[0003] For example, a green compact mainly containing zirconium oxide generally shrinks by about 1% during the manufacture of a calcined body and by about 20% during the manufacture of a sintered body. Therefore, in order to obtain a high-density and high-strength zirconium oxide sintered body, a high-density calcined body and a zirconium oxide green compact with little density variation are sought.

[0004] On the other hand, as a method for manufacturing a powder compact, in the uniaxial pressing method, the powder compact has a non-uniform density distribution, so there is a method to reduce it by CIP (Cold Isostatic Pressing) treatment. However, the non-uniformity inside the powder compact is not completely eliminated, so a method for manufacturing a powder compact with high density and less density non-uniformity is sought.

[0005] In addition, in order to obtain a high-density and low-density compressed powder, on the basis of uniformly filling the dry powder into the mold, it is necessary to rearrange the dry powder according to the pressure during pressurization, and the packing density is uniformly improved to this extent. The fluidity. Therefore, in order to improve the fluidity of the primary particles, there is usually a method of adding a binder as an organic component to obtain a compressed powder. However, until a calcined body or a sintered body is obtained from the compressed powder, the organic component must be removed, but the fluidity and removal are difficult to coexist, and it is difficult to obtain a high-density and low-density compressed powder. Therefore, there is a problem that it is difficult to obtain a sintered body with high light transmittance and high strength.

[0006] For example, polyvinyl alcohol or the like generally used as a binder has a problem in that its fluidity can be easily adjusted due to a large variation in molecular weight, but it cannot be sufficiently removed by calcination and thus is easily carbonized in the process of obtaining a calcined body.

[0007] In addition, regarding the above-mentioned problem, Non-Patent Documents 1 to 3 disclose the compaction and relaxation behaviors of particles used for producing a powder compact.

[0008] In addition, Patent Document 1 discloses a zirconia sintered body having high sintered body density and strength.

[0009] Furthermore, Patent Document 2 discloses ceramic particles used to obtain a large molded body or a molded body of a complicated shape by a press method, and discloses particles for obtaining a high-density sintered body free from breakage and deformation and their compression failure strength.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2015-143178

[0013] Patent Document 2: Japanese Patent Application Publication No. 2006-27914

[0014] Non-patent literature

[0015] Non-patent document 1: Junichiro Tsubaki et al., "Evaluation of mechanical properties of spray-dried granules based on the compaction / relaxation method", Journal of the Ceramic Society of Japan, Vol. 107, 11 (1999) pp. 1093-1098

[0016] Non-patent document 2: Junichiro Tsubaki et al., "Evaluation of mechanical properties of spray-dried granules based on the compaction / relaxation method", Journal of the Ceramic Society of Japan, Vol. 107, 12 (1999) pp. 1183-1187

[0017] Non-patent document 3: Written by Junichiro Tsubaki; "The Role of Chemical Engineering in the Ceramic Industry (セラミックスINDUSTRY におけるCHEMICAL ENGINEERING)", Chemical Engineering Vol. 48, No. 1, pp. 34-38 (2003) Summary of the invention

[0018] Problems to be solved by the invention

[0019] However, in non-patent documents 1 to 3, experiments were conducted using alumina particles, and it cannot be said that they are generally applicable to zirconia. The present inventors have studied the particles obtained using alumina particles, and the results show that: for the particles obtained using the aforementioned alumina particles, if the compression ratio when pressurized to 33MPa by uniaxial pressing is converted, it is 0.54 or more, and the particles are difficult to pack under low pressure, that is, a high-density compressed powder body cannot be obtained. The low pressure mentioned here refers to a pressure of less than 10MPa, which is not preferred because the particles are not fully flattened to form a low-density and highly non-uniformly dense molded body. In addition, non-patent documents 1 to 3 have records that the particles are deformed and destroyed after the inflection point of stress, but the particles obtained using the zirconia particles of the present invention undergo deformation and destruction before the inflection point, and the difference is confirmed.

[0020] In addition, it is known that: Patent Document 1 does not contain any description related to the compaction behavior of particles, and the primary particle size of the powder is small, so the density of the powder compact is low, and further, the density variation is large. Therefore, when the powder particles of Patent Document 1 are used to produce a sintered body, there is a problem that the density variation of the sintered body also becomes large. Furthermore, Patent Document 2 uses a binder that is not easily elongated, such as polyvinyl alcohol and polyethylene glycol, in combination, and has the following problems: high density cannot be obtained unless the molding is performed under high pressure, and the density does not increase under low pressure.

[0021] Therefore, an object of the present invention is to provide particles and a green compact suitable for obtaining a zirconia sintered body having less density unevenness, high light transmittance, and high strength, and a calcined body having less density unevenness, and a method for producing the same.

[0022] Means used to solve problems

[0023] As a result of repeated in-depth research to solve the above-mentioned problems, the inventors of the present invention focused on the compaction and relaxation behavior of particles and found that particles with a specific compression ratio and stress can obtain a compressed powder with uniform density even under low pressure, which can solve the above-mentioned problems. Based on this understanding, further repeated research was carried out to complete the present invention.

[0024] That is, the present invention includes the following inventions.

[0025] [1] A particle containing zirconium oxide, a stabilizer capable of inhibiting phase transformation of zirconium oxide, and a binder,

[0026] According to JIS R 1628:1997, granules are filled into the cylindrical mold by oscillation.

[0027] When the compression is performed at a speed of 1 mm / sec by uniaxial pressing and the pressure is increased to 33 MPa, the compression ratio R calculated by the following formula (1) is 0.46 to 0.53.

[0028] R=(HD) / H(1)

[0029] (wherein H represents the height of the particles filled by oscillation in the columnar mold before pressurization, and D represents the deformation amount until 33 MPa is reached).

[0030] [2] The pellets according to [1], wherein during the pressurization of the pellets in the columnar mold, the stress at a compression ratio R of 0.6 is 7.20 MPa or more.

[0031] [3] The particles according to [1] or [2], wherein the binder is a (meth)acrylic binder.

[0032] [4] The particle according to any one of [1] to [3], wherein the average particle size of primary particles constituting the particle is 45 to 200 nm.

[0033] [5] The particles according to any one of [1] to [4], wherein the stabilizer is yttrium oxide.

[0034] [6] The particles according to [5], wherein the content of the yttrium oxide is 2.5 to 8.5 mol % relative to the total molar amount of zirconium oxide and yttrium oxide.

[0035] [7] A powder compact comprising the particles described in any one of [1] to [6], wherein the bulk density of the powder compact is 2.9 to 3.5 g / cm 3 .

[0036] [8] The powder compact according to [7], wherein the stabilizer contained in the particles is yttrium oxide.

[0037] [9] The powder compact according to [8], wherein the content of the yttrium oxide is 2.5 to 8.5 mol % relative to the total molar amount of zirconium oxide and yttrium oxide.

[0038]

[10] A method for producing particles, comprising:

[0039] A step of mixing zirconium oxide with a stabilizer capable of inhibiting phase change of zirconium oxide to obtain a zirconium oxide raw material composition;

[0040] a pulverizing step of pulverizing the zirconium oxide raw material composition to obtain particles having an average primary particle size of 45 to 200 nm; and

[0041] A step of adding a binder to the above particles and granulating the particles to obtain particles containing zirconium oxide, a stabilizer capable of suppressing phase transformation of zirconium oxide, and the binder.

[0042]

[11] The method for producing pellets according to

[10] , wherein the binder is a (meth)acrylic binder.

[0043]

[12] The method for producing particles according to

[10] or

[11] , wherein the stabilizer is yttrium oxide.

[0044]

[13] A method for producing a powder compact, comprising: filling a columnar mold with the particles described in any one of [1] to [6] by oscillation.

[0045] When the compression is performed at a speed of 1 mm / sec by uniaxial pressing and the pressure is increased to 33 MPa, the compression ratio R calculated by the following formula (1) is 0.46 to 0.53.

[0046] R=(HD) / H(1)

[0047] (wherein H represents the height of the particles filled by oscillation in the columnar mold before pressurization, and D represents the deformation amount until 33 MPa is reached).

[0048]

[14] The method for producing a powder compact according to

[13] , wherein, during the process of pressurizing the particles in the columnar mold, the stress becomes 7.20 MPa or more when the compression ratio R becomes 0.6.

[0049] Effects of the Invention

[0050] According to the present invention, particles, powder compacts and methods for producing the same can be provided, which are suitable for obtaining zirconium oxide sintered bodies with less density variation, high light transmittance and high strength, and calcined bodies with less density variation. In addition, according to the present invention, powder compacts with uniform density even under low pressure can be provided. Furthermore, particles showing the compacting behavior of the present invention can obtain powder compacts with no cracks or defects, high density and less density variation, and can be suitably used in dental materials, etc., which have high light transmittance and high strength after calcination, regardless of which part of the powder compact is used. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a schematic diagram showing the method of measuring the compression ratio R of the present invention. DETAILED DESCRIPTION

[0052] The particles of the present invention are particles containing zirconium oxide, a stabilizer capable of inhibiting the phase transformation of zirconium oxide (hereinafter sometimes referred to as "stabilizer") and a binder. The particles are filled into a columnar mold by oscillation according to JIS R 1628:1997, and compressed at a speed of 1 mm / sec by uniaxial pressing. When the pressure is increased to 33 MPa, the compression ratio R calculated by the following formula (1) becomes 0.46 to 0.53. The uniaxial pressing is preferably performed under atmospheric pressure.

[0053] R=(HD) / H(1)

[0054] (wherein H represents the height of the particles filled by oscillation in the columnar mold before pressurization, and D represents the deformation amount until 33 MPa is reached).

[0055] The compression ratio R of the particles of the present invention is greater than 0.46, preferably greater than 0.47, and more preferably greater than 0.48. When it is less than 0.46, the particles are easily flattened, and when a specified pressure is applied during molding, the particles are locally flattened due to the stress, that is, the density of the compressed powder body is prone to unevenness. In addition, the compression ratio R of the particles of the present invention is less than 0.53, preferably less than 0.52, and more preferably less than 0.51. When it is greater than 0.53, the particles are difficult to flatten, and under a low pressure of less than 10 MPa during molding, a uniform compressed powder body cannot be obtained, and density unevenness is prone to occur. The compressed powder body is formed by applying an external force to the particles of the present invention, and is a material before calcination, which means that it has not undergone necking (fixation). The compression ratio R can be measured using the method described in the embodiments described later.

[0056] By setting the compression ratio R of the particles of the present invention within the above range, a green compact with less density variation can be obtained. In addition, the green compact can be used to obtain a calcined body with less density variation, and further, a zirconia sintered body with less density variation, high light transmittance and high strength can be obtained.

[0057] The height of the particles filled by oscillation in the column before pressurization of the aforementioned formula (1) is preferably 8.0 to 13.0 cm, more preferably 8.5 to 12.5 cm, and further preferably 9.0 to 12.0 cm. In addition, the deformation amount until reaching 33 MPa in the aforementioned formula (1) is preferably greater than 4.60 cm and less than 6.00 cm, more preferably greater than 4.65 cm and less than 5.95 cm, and further preferably greater than 4.70 cm and less than 5.95 cm. Within these ranges, by making the compression ratio R of the particles within the aforementioned range, a powder compact with less density unevenness is obtained.

[0058] The particles of the present invention preferably have a stress of 7.20 MPa or more, and more preferably 7.50 MPa or more, when the compression ratio R is 0.6. When the stress is less than 7.20 MPa, the particles may be difficult to collapse when gradually filling the particles, and the density uniformity of the powder compact may decrease, and the density unevenness may increase. The stress when the compression ratio R is 0.6 can be measured by the method of the compression ratio R described in the examples below.

[0059] The tensile elongation of the binder used in the present invention is preferably in the range of 120 to 800%, more preferably in the range of 135 to 720%, and further preferably in the range of 150 to 670%. When it is 120% or more, the compression ratio R becomes 0.53 or less, which is preferred, and when it is 800% or less, the powder compact is not damaged and the shape retention is excellent, which is preferred.

[0060] As the binder of the present invention, there is no particular limitation, and known binders can be used, for example, polymers. As polymers constituting the binder, for example, organic binders can be listed. As organic binders, for example, polymers such as commonly used (meth) acrylic acid binders, (meth) acrylic acid binders, paraffin binders, fatty acid binders, etc. can be listed. Among these organic binders, binders or carboxylic acid derivatives having carboxyl groups in the molecular chain are preferred, (meth) acrylic acid binders are more preferred, and water-soluble poly (meth) acrylates are further preferred. Poly (meth) acrylates can be obtained by copolymerizing acrylic acid or methacrylic acid with maleic acid, and can also contain sulfonic acid, and sodium, ammonium, etc. can be listed as cations of the salt.

[0061] The polymer is preferably a substance that interacts strongly with the surface of zirconium oxide, because this improves the shape retention of the powder compact. For example, the binder is preferably a (meth)acrylic polymer.

[0062] The strength of the interaction between the polymer and the zirconium oxide surface can be estimated based on, for example, the wettability of the polymer with the zirconium oxide and the stabilizer. The wettability can be calculated based on, for example, the Hansen solubility parameter, and its affinity δ can be calculated using the dispersion force term (δd), the dipole force term (δp) and the hydrogen bonding force term (δh) per molar volume as the solubility parameter, and is calculated according to the following formula.

[0063] δ={(δdA-δdB) 2 +(δpA-δpB) 2 +(δhA-δhB) 2} 1 / 2

[0064] The smaller the affinity δ is, the higher the affinity is, and the larger the affinity is, the lower the affinity is.

[0065] The molecular weight of the polymer constituting the binder of the present invention is preferably 10,000 to 1,000,000, more preferably 30,000 to 500,000, further preferably 70,000 to 480,000, further preferably 80,000 to 470,000, and particularly preferably 100,000 to 450,000, from the viewpoint of its mechanical properties, i.e., the formability of the powder compact. In the case of the aforementioned range, when combined with other structures, it is easier to adjust the compression ratio R within the prescribed range, and further, it is also easier to adjust the stress when the compression ratio R is 0.6 within the desired range. The higher the molecular weight, the higher the molecular weight between the entanglement points, the higher the tensile elongation, and the better the formability when formed into a powder compact, so it is preferred. The binder may be a binder containing two or more polymers with different weight average molecular weights, and the weight average molecular weight after mixing is preferably 50,000 to 800,000, and more preferably 100,000 to 500,000.

[0066] The weight average molecular weight refers to a polystyrene-equivalent weight average molecular weight determined by gel permeation chromatography (GPC).

[0067] The polymer constituting the binder of the present invention can use a polymer having a prescribed glass transition temperature (Tg) and a softening point based on the glass transition temperature. If the Tg is low, the tensile strength of the polymer is reduced due to the compression energy during the compacting of the powder body, and the formability is improved, so it is preferred. Tg is preferably below 50°C, more preferably below 30°C, and further preferably below 10°C. The binder can be a binder containing two or more polymers with different Tg. By combining a high Tg polymer and a low Tg polymer, the Tg of the high Tg polymer is preferably reduced. When the Tg or softening point is in the aforementioned range, it is easier to adjust the compression ratio R to within the specified range when combined with other structures. In the determination of Tg or softening point, for example, a DSC (Differential scanning calorimetry) measuring apparatus (DSC822) manufactured by Metler & Toledo Co., Ltd. can be used to perform DSC measurement under the condition of a heating rate of 10°C / min in accordance with ISO 3146:2000, and in the curve obtained thereby, the extrapolation start temperature is set as Tg or softening point. In this specification, Tg is used for crystalline polymers, and softening point is used instead of Tg for substances that are not crystalline polymers (amorphous polymers). The softening point of the polymer constituting the binder is preferably above -40°C, more preferably above -5°C, and further preferably above 0°C. In addition, the softening point is preferably below 50°C, more preferably below 30°C, and further preferably below 10°C.

[0068] The method for producing the polymer constituting the adhesive of the present invention is not particularly limited, and a method based on a known method can be used. For example, as a method for producing the polymer constituting the aforementioned (meth)acrylic adhesive, there can be cited a method of producing by thermally polymerizing a monomer containing a (meth)acryloyl group (a (meth)acryloyloxy group or a (meth)acrylamide group) using a free radical polymerization initiator. The monomer containing a (meth)acryloyl group and the free radical polymerization initiator are not particularly limited as long as they can be set in a manner having the aforementioned specified composition (for example, the tensile elongation of the adhesive, the glass transition temperature (Tg), the softening point, and the weight average molecular weight of the polymer constituting the adhesive), and known substances can be used.

[0069] In the adhesive of the present invention, various additives such as antioxidants, heat stabilizers, lubricants, processing aids, antistatic agents, anti-thermal degradation agents, ultraviolet light absorbers, light stabilizers, polymer processing aids, colorants, impact-resistant aids, etc. can be used in combination. In this case, the manufacturing method of the polymer constituting the adhesive of the present invention is not particularly limited as long as it is a method that can uniformly mix the above-mentioned two or more polymers with the above-mentioned additives. A method based on a known method can be adopted, and it can be dissolved in water or an organic solvent for mixing, or melt kneading can be performed. In addition, the glass transition temperature (Tg) of the polymer constituting the adhesive and the softening point based on this can be adjusted by various additives.

[0070] The binder content of the present invention is preferably 1.1 parts by mass or more relative to 100 parts by mass of the zirconium oxide raw material composition, more preferably 1.3 parts by mass or more, and further preferably 1.5 parts by mass or more. In this specification, a composition containing zirconium oxide and a stabilizer but not containing a binder is referred to as a "zirconium oxide raw material composition". In addition, a composition containing zirconium oxide, a stabilizer and a binder is referred to as a "zirconium oxide composition". Zirconium oxide may contain hafnium oxide that is difficult to separate from zirconium oxide. If the binder content is 1.1 parts by mass or more relative to 100 parts by mass of the zirconium oxide raw material composition, the compact can maintain its shape, the end will not be damaged, and there is no need to worry about its fragmentation. On the other hand, if the binder content is too much, the density of the compact will be increased, and the density of the calcined body or sintered body will be easily increased. From this point of view, the binder content is preferably 5.0 parts by mass or less relative to 100 parts by mass of the zirconium oxide raw material composition, more preferably 4.5 parts by mass or less, and further preferably 4.0 parts by mass or less. In addition, when the binder content is in the above range, it is easier to adjust the compression ratio R to the specified range when combined with other structures. In addition, for example, in one embodiment, it is preferred to use a binder whose glass transition temperature (Tg) or softening point of a polymer constituting the binder is within the above range (e.g., -10°C to 50°C, or more than 0°C to 30°C). In another embodiment, it is preferred to use a binder whose weight average molecular weight of a polymer constituting the binder is within the above range (e.g., 70,000 to 480,000) at a content within the above range.

[0071] Furthermore, in another embodiment, by using (adjusting the blending ratio (mass ratio) of the zirconium oxide raw material composition and the binder) in the above-mentioned range of contents (i) a binder having a tensile elongation within the above-mentioned range (e.g., 120 to 800%), (ii) a binder having a weight average molecular weight of a polymer constituting the binder within the above-mentioned range (e.g., 70,000 to 480,000), (iii) a binder having a glass transition temperature (Tg) or a softening point of a polymer constituting the binder within the above-mentioned range (e.g., above -10°C and below 50°C, above 0°C and below 30°C), and a binder obtained by combining them, it is easier to adjust the compression ratio R within the specified range, and further, it is easier to adjust the stress when the compression ratio R is 0.6 within the desired range.

[0072] The average particle size of the primary particles constituting the particles of the present invention (hereinafter also referred to as "average primary particle size") is preferably 45 to 200 nm, more preferably 50 to 180 nm, and further preferably 60 to 160 nm. When it is less than 45 nm, the compression ratio is less than 0.46, which is not preferred. When it is greater than 200 nm, the sintering ability becomes low, the density increase after calcination is not likely to occur, and the light transmittance is difficult to improve, which is not preferred. The BET specific surface area of ​​the particles constituting the particles is preferably 7.0 m when measured in accordance with JIS Z8830:2013. 2 / g or more, more preferably 7.5m 2 / g or more, more preferably 8m 2 / g or more. 2 / g, it is difficult to sinter, or even if it can be sintered, the sintered body will be turbid. In addition, the BET specific surface area is preferably 30m 2 / g or less, more preferably 25m 2 / g or less, more preferably 20m 2 / g or less. If it exceeds 30m 2 / g, the heating rate described later becomes high and is easily affected by the temperature unevenness in the calcining furnace. In addition, if the calcining time for sintering is shortened, the light transmittance of the sintered body decreases. In the present invention, the BET specific surface area refers to the specific surface area measured without distinguishing between primary particles and secondary particles.

[0073] The compact produced from the granules of the present invention preferably has a bulk density of 2.9 to 3.5 g / cm 3 , more preferably 3.0 to 3.45 g / cm 3 , more preferably 3.1 to 3.4 g / cm 3 . Less than 2.9g / cm 3 When the density of the calcined or sintered body is greater than 3.5 g / cm 3 In the case of , the gas generated by thermal decomposition of the binder will expand the powder compact, reduce the density of the calcined body, or cause damage or cracking, which is not preferred.

[0074] The granules or powder compact of the present invention contain a stabilizer capable of inhibiting the phase transformation of zirconium oxide. The stabilizer is preferably capable of forming partially stabilized zirconium oxide. Examples of the stabilizer include calcium oxide (CaO), magnesium oxide (MgO), yttrium oxide (Y2O3) (hereinafter referred to as "yttrium oxide"), cerium oxide (CeO2), scandium oxide (Sc2O3), niobium oxide (Nb2O5), lanthanum oxide (La2O3), erbium oxide (Er2O3), praseodymium oxide (Pr6O3), and tantalum oxide (T). 11), samarium oxide (Sm2O3), europium oxide (Eu2O3) and thulium oxide (Tm2O3), preferably yttrium oxide. The stabilizer can be used alone or in combination of two or more. The content of the stabilizer in the zirconium oxide powder compact of the present invention can be determined by, for example, inductively coupled plasma (ICP; Inductively Coupled Plasma) emission spectrometry, fluorescent X-ray analysis, etc. In the zirconium oxide powder compact of the present invention, the content of the stabilizer is preferably 0.1 to 18 mol%, more preferably 1 to 15 mol%, and further preferably 3 to 8 mol% relative to the total molar amount of zirconium oxide and the stabilizer.

[0075] From the viewpoint of the strength and light transmittance of the obtained zirconium oxide sintered body, the zirconium oxide powder compact preferably contains yttrium oxide as a stabilizer. The content of yttrium oxide is preferably 2.5 mol% or more, more preferably 3 mol% or more, and further preferably 3.5 mol% or more relative to the total molar amount of zirconium oxide and yttrium oxide. When the content of yttrium oxide is 3 mol% or more, the light transmittance of the zirconium oxide sintered body can be further improved. In addition, the content of yttrium oxide is preferably 8.5 mol% or less, more preferably 7.5 mol% or less, and further preferably 7.0 mol% or less relative to the total molar amount of zirconium oxide and yttrium oxide. When the content of yttrium oxide is 7.5 mol% or less, the reduction in the strength of the obtained zirconium oxide sintered body can be further suppressed.

[0076] Hereinafter, a method for producing the particles will be described. In addition, in this specification, particles containing zirconium oxide, a stabilizer, and a binder may be referred to as "zirconium oxide particles".

[0077] Examples of a method for producing zirconium oxide particles include a method for producing zirconium oxide particles comprising the following steps: for example, a step of mixing zirconium oxide (suitably zirconium oxide powder) with the aforementioned stabilizer to obtain a zirconium oxide raw material composition (mixture) (mixing step); a step of pulverizing the aforementioned zirconium oxide raw material composition to obtain particles (pulverized material) having an average particle size of primary particles within a specified range (pulverized material) (pulverizing step); and a step of adding a binder to the aforementioned pulverized particles (pulverized material) and granulating the particles to obtain zirconium oxide particles (granulation step).

[0078] First, zirconium oxide (suitably zirconium oxide powder) and a stabilizer are mixed in a prescribed ratio to prepare a mixture (mixing step). For example, when the stabilizer is yttrium oxide, the mixing ratio of zirconium oxide and yttrium oxide can be mixed in a manner that yttrium oxide becomes the aforementioned content. There is no particular limitation on the mixing, and a known mixing device can be used. When a solvent is used in the mixing, the resulting mixture can be in the form of a slurry or the like. The solvent is not particularly limited, and water or an organic solvent can be used. The mixing can be dry mixing or wet mixing. The mixture can be crushed in a manner that the particles constituting the zirconium oxide particles become the aforementioned average primary particle size (suitably 45 to 200 nm), and further, as required, in a manner that the particles constituting the zirconium oxide particles become the aforementioned BET specific surface area (crushing step). The crushing method is not particularly limited, and a known crushing device (such as a ball mill, a bead mill, etc.) can be used. The mixing step and the crushing step can be performed in the same step.

[0079] The binder is added to the pulverized material of the zirconium oxide raw material composition (the aforementioned mixture) in the aforementioned specified content. In addition, as another embodiment, the binder can be added in the mixing process or in the pulverizing process. In the case where the binder is added in the mixing process, the zirconium oxide composition obtained by the mixing process is pulverized in the pulverizing process. The types of binders are as described above. It can be added to the mixture in a manner such that the content of the binder becomes the aforementioned content. For example, in the case where the binder is added in the pulverizing process, the pulverization can be carried out, for example, after the mixture and the binder are dispersed in a solvent such as water (dispersion process), using a pulverizing device such as a ball mill or a bead mill until the powder constituting the mixture becomes the desired average primary particle size. The average primary particle size can be measured, for example, by a laser diffraction / scattering particle size distribution measurement method. For example, a laser diffraction / scattering particle size distribution measurement device (trade name "Partica LA-950") manufactured by Horiba, Ltd. can be used to irradiate the slurry diluted with water with ultrasonic waves for 30 minutes, and then the slurry is measured on a volume basis while in contact with ultrasonic waves. After the mixing step and / or the pulverizing step, the obtained mixture is dried by spray drying to obtain zirconium oxide particles (granulation step). The spray drying is not particularly limited, and a known spray drying device (spray dryer, etc.) can be used.

[0080] Zirconia and a stabilizer (preferably yttrium oxide) are preferably prepared separately. For example, zirconium oxide and a stabilizer are not precipitated at the same time (in the same process), but the preparation process (for example, the manufacturing process) of zirconium oxide and the preparation process (for example, the manufacturing process) of the stabilizer are preferably independent processes. In this way, it is possible to suppress the stabilizer (preferably yttrium oxide) from being dissolved in zirconium oxide in the manufacturing process of the zirconium oxide calcined body described later.

[0081] The following is an explanation of the case where the stabilizer is yttrium oxide. Zirconium oxide powder with yttrium oxide solid solution is usually produced according to a coprecipitation method and a hydrolysis method. In the coprecipitation method and the hydrolysis method, a mixture of water, zirconium oxide and yttrium oxide is produced from zirconium oxychloride and yttrium chloride by the same process, and the mixture is calcined at 800°C to 900°C to produce a stable zirconium oxide powder with yttrium oxide (yttrium) solid solution. The yttrium oxide solid solution zirconium oxide is mainly tetragonal and / or cubic. The particle size of the zirconium oxide powder thus obtained is at the level of tens of nm. In order to make the zirconium oxide powder into a raw material for a zirconium oxide sintered body, after the calcined product is crushed into a specified particle size, granulation is performed to produce zirconium oxide particles.

[0082] Regarding the zirconium oxide particles produced by such a coprecipitation method or hydrolysis method, the fixing temperature in the temperature range for producing the zirconium oxide calcined body is close to the temperature for removing the organic binder, and / or the temperature dependence becomes high. When the existence state of the organic binder is uneven, the primary particles constituting the zirconium oxide particles produced by the coprecipitation method or hydrolysis method form a strong neck locally according to their particle size. Therefore, when the zirconium oxide calcined body is cut to produce a cut body, the chipping rate of the cut body increases, which is not preferred.

[0083] The zirconium oxide particles are formed by applying external force to form a powder compact. The forming method is not limited to a specific method, and a suitable method can be appropriately selected according to the purpose. As the forming method, for example, press forming, injection molding, etc. can be listed. In addition, multi-stage forming can be performed. For example, after the zirconium oxide particles are press-formed, CIP treatment can be further performed. As a method for manufacturing a powder compact, for example, the following method can be listed: oscillating and filling zirconium oxide particles in a columnar mold, compressing at a speed of 1 mm / second by uniaxial pressing, and when the pressure is pressed to a stress of 33 MPa, the compression ratio R becomes 0.46 to 0.53. The uniaxial pressing is preferably performed under atmospheric pressure. In order to further reduce the density unevenness, the formed body obtained by uniaxial pressing can be subjected to CIP treatment thereafter. As the CIP pressure, it is preferably higher than the stress of uniaxial pressing. As the CIP pressure, it is preferably more than 33 MPa, more preferably more than 50 MPa, further preferably more than 100 MPa, and particularly preferably more than 150 MPa. By using the zirconium oxide particles of the present invention, a green compact having excellent shape retention and little density variation can be obtained, and a calcined body having little density variation can be obtained using the green compact. Figure 1 A schematic diagram is shown in FIG.

[0084] exist Figure 1In the process, a testing machine having a head, a mold 2 and a base 3 is used, zirconium oxide particles as dry powder are filled into the mold 2, and the mold 2 is pressed at a speed of 1 mm / sec toward the axial direction 1 of the head by uniaxial pressing, and when the generated stress reaches 33 MPa, the position of the head is fixed to obtain a powder compact. As the testing machine, for example, a precision universal testing machine (trade name: AG-I 100 kN, manufactured by Shimadzu Corporation) can be used.

[0085] In the method for producing a powder compact, during the process of pressurizing the particles in the columnar mold, the stress when the compression ratio R becomes 0.6 is preferably 7.20 MPa to 16 MPa, more preferably 7.50 MPa to 14 MPa, and further preferably 8.50 MPa to 12 MPa.

[0086] The aforementioned powder compact may have a disc shape, a rectangular parallelepiped shape, or a dental product shape (eg, a crown shape).

[0087] A zirconia calcined body is obtained by calcining (i.e., pre-calcining) the aforementioned powder compact at a temperature that does not result in sintering. The zirconia calcined body of the present invention becomes a precursor (intermediate product) of the zirconia sintered body of the present invention described later. A zirconia calcined body refers to a substance in which the zirconia particles (powder) are necked (fixed) but not completely sintered. In addition, the zirconia calcined body also includes a formed substance. The zirconia calcined body described in the present invention also includes a dental product (e.g., a crown-shaped prosthesis) obtained by processing a pre-calcined zirconia disk using a CAD / CAM (Computer-Aided Design / Computer-Aided Manufacturing) system.

[0088] The content of zirconium oxide and the stabilizer in the calcined zirconium oxide of the present invention is the same as the content in the zirconium oxide particles and the green compact before the calcined zirconium oxide is prepared. From the viewpoint of the strength and light transmittance of the sintered body prepared from the calcined zirconium oxide of the present invention, the stabilizer contained in the calcined zirconium oxide is preferably yttrium oxide.

[0089] The calcining temperature in the method for producing a calcined zirconium oxide body of the present invention is preferably 830 to 1080°C, more preferably 850 to 1050°C, and even more preferably 895 to 1000°C from the viewpoint of the strength of the obtained calcined zirconium oxide body.

[0090] If the above-mentioned calcination temperature is set to the maximum calcination temperature and maintained at the maximum calcination temperature for a predetermined time, the hardness of the calcined zirconia body sometimes becomes a preferred range and the chipping rate is reduced, which is preferred. The calcination conditions can be changed according to the density of the target calcined zirconia body, the average particle size of the primary particles constituting the calcined zirconia body, and the content of the binder. It is preferred to maintain the calcination temperature at the maximum for 30 minutes to 6 hours. In addition, the heating rate to the maximum calcination temperature and the cooling rate from the maximum calcination temperature are preferably 300°C / min or less.

[0091] According to the zirconium oxide particles and green compact of the present invention, a zirconium oxide calcined body with less density variation can be produced.

[0092] The calcined zirconium oxide of the present invention can be subjected to cutting to produce a cut-processed body. The cutting method is not limited to a specific method, and a suitable method can be appropriately selected according to the purpose. For example, a calcined zirconium oxide disk can be cut into the shape of a dental product (e.g., a crown-shaped prosthesis) using a CAD / CAM system to produce a cut-processed body.

[0093] The surface smoothness of the cut body can be improved by using a tool such as an abrasive (for example, trade name "Parsal Fines (registered trademark)", manufactured by Claretta Chemical Co., Ltd.).

[0094] By subjecting the zirconia calcined body of the present invention or its cut body to a sintering step of calcining at a temperature at which zirconia particles sinter (sinterable temperature), a zirconia sintered body (hereinafter sometimes referred to as "zirconia sintered body" or "sintered body") can be produced. The calcining temperature is, for example, preferably 1400°C or higher, and more preferably 1450°C or higher. In addition, the calcining temperature is, for example, preferably 1650°C or lower, and more preferably 1600°C or lower. The heating rate and the cooling rate are preferably 300°C / min or lower. The zirconia sintered body refers to a substance in a completely sintered state.

[0095] In the above-mentioned sintering step, the holding time at the sinterable temperature (e.g., the maximum calcining temperature) is preferably less than 120 minutes, more preferably less than 90 minutes, further preferably less than 75 minutes, further preferably less than 60 minutes, particularly preferably less than 45 minutes, and most preferably less than 30 minutes. The holding time is preferably more than 1 minute, more preferably more than 5 minutes, and further preferably more than 10 minutes.

[0096] In the sintering step, the holding time at the sinterable temperature (eg, the maximum calcination temperature) may be, for example, 25 minutes or less, 20 minutes or less, or 15 minutes or less.

[0097] The heating rate and cooling rate in the sintering process are preferably set in a manner that the time required for the sintering process is shortened. For example, the heating rate can be set in a manner that reaches the maximum calcining temperature in the shortest time according to the performance of the calcining furnace. The heating rate to the maximum calcining temperature can be set, for example, to be 10°C / minute or more, 50°C / minute or more, 100°C / minute or more, 120°C / minute or more, 150°C / minute or more, or 200°C / minute or more. The speed of cooling from the maximum calcining temperature is preferably set to a speed that does not produce defects such as cracks in the sintered body. For example, after the heating is completed, the sintered body can be naturally cooled at room temperature.

[0098] According to the zirconium oxide particles and the green compact of the present invention, a zirconium oxide sintered body having less density unevenness, high light transmittance and high strength can be produced.

[0099] The particles of the present invention can be suitably used in ceramics for pressure molding.

[0100] Example

[0101] Next, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples at all.

[0102] <Method for measuring compression ratio R>

[0103] The universal testing machine used was AGS-X manufactured by Shimadzu Corporation, the control software used was TRAPEZIUM LITE X manufactured by Shimadzu Corporation, and the load cell used was a load cell 5000N manufactured by Shimadzu Corporation.

[0104] According to JIS R 1628:1997, the particles obtained in the following examples and comparative examples are filled into a columnar mold by oscillation, clamped from top to bottom with a universal testing machine fixed with a punch, and compression is started just before the top surface filled with particles contacts the upper punch of the mold. Just before the compression starts, the distance between the punches is adjusted to be the height H of the particles filled by oscillation before pressurization in the columnar mold. The control software is set to stop the punch compression when 33MPa is reached, and the measurement is performed using the low-speed mode. The compression speed of the punch is set to 1mm / second, and the test force is measured every 0.1 seconds. The value obtained by dividing the measured test force by the cross-sectional area of ​​the columnar mold is taken as stress. At the stage where the stress of the particles filled by oscillation reaches the specified pressure, the movement of the punch is stopped, and the deformation at this time is set to D, and the compression ratio R (average value of n=3) is calculated. In addition, the stress (average value of n=3) when the compression ratio R is 0.6 is also calculated according to the above method.

[0105] <Measurement of Elongation of Adhesive>

[0106] By film casting, samples of various adhesives with a length of 5 mm × a width of 30 mm × a thickness of 1 mm were obtained. The samples were suspended along the length direction, and a weight of 200 g was installed at the lower end. The length before the change was set as 100%, and the elongation was calculated using the following formula (average value of n=3) based on the length after 180 seconds.

[0107] (Elongation) = (length after 180 seconds) ÷ (initial length) × 100

[0108] <Method for measuring the average particle size of primary particles constituting particles>

[0109] Using the particles obtained in the following embodiments or comparative examples, scanning electron microscope (trade name " VE-9800 ", Keyence company system) is utilized to obtain the imaging of surface. For the obtained image, average grain size is calculated by image analysis. Image analysis software (trade name " Image-Pro Plus ", Bodong company system) is used in the measurement of particle diameter, the SEM image read is binarized, the brightness range is adjusted so that the crystal boundary is clear, and particles are identified from the visual field (region). About the unclear part of crystal boundary, degenerate filter is applied in the region, each region is degenerated to 1 or more points, and the mode that this point becomes the mother point of Thiessen polygon is mapped out Thiessen polygon, and the line segment connecting the midpoint of 2 mother points of adjacency is drawn, and this line segment is overlapped with the original particle image, thus separating between the adjacent particles. For example, in image processing, sometimes a particle looks like a gourd shape. In this case, it is assumed that two round particles are in contact and are seen as one, and then separated into two (two separated). Using the processing file that recognizes the primary particle size, select "Diameter" in "Count / Size Dialog" and calculate the distribution (n = 4). Specifically, for the four fields of view of a sample, calculate the average value of the particle size (primary particle size) measured in each field of view using image analysis software (trade name "Image-Pro Plus").

[0110] <Shape Retention of Powder Compressed Body>

[0111] In the powder compact obtained when the compression ratio R is obtained, visually check whether the corners of the rectangle are damaged (n=5). The absence of damage is considered to have high shape retention and is evaluated as "○", and even if there is only one sub-millimeter damage, it is considered to have no shape retention and is evaluated as "×". The results are shown in Table 2.

[0112] <Method for measuring bulk density of powder compact>

[0113] The columnar powder compacts obtained by the methods of the following examples or comparative examples were accurately measured for size using a micrometer, and their mass was measured using a precision balance. The density (average value for n=3) was calculated by (mass of the powder compact) / (volume of the powder compact). The results are shown in Table 2. For the calculated bulk density, the bulk density of less than 2.9 g / cm 3 or greater than 3.5g / cm 3 The case of 2.9 g / cm 3 The above situation was evaluated as "△", and 3.1 g / cm 3 The above cases were evaluated as "○".

[0114] <Evaluation method of density uniformity of calcined body>

[0115] The powder compact obtained by the following examples or comparative examples is put into an electric furnace set at a temperature of 1,000°C for pre-sintering to obtain a calcined body. From the obtained calcined body, a plurality of 10 mm square test bodies are cut out at arbitrary locations while changing the cutting position, and the respective bulk densities (average value of n=3) are calculated based on the mass and volume. The results are shown in Table 2. If the error of the calculated multiple bulk density values ​​is within 3.5%, the density uniformity is regarded as high and is evaluated as "○". If it is greater than 3.5%, the density uniformity is regarded as low and is evaluated as "×". The error of the bulk density value is preferably within 3.5%, more preferably within 3.4%, and further preferably within 3.3%. If it is greater than 3.5%, the shrinkage rate of the sintered body may increase due to the uneven bulk density of the calcined body, and a sintered body of the target shape cannot be obtained.

[0116] <Evaluation Method of Density Uniformity of Sintered Body>

[0117] From the calcined body obtained by the same operation as above, a plurality of 10 mm square test bodies are cut out at arbitrary positions while changing the cutting position. In Examples 1 to 10 and Comparative Examples 1 to 7, 1,500°C is set as the maximum calcination temperature, and in Comparative Examples 8 to 10, 1,450°C is set as the maximum calcination temperature. The sintered body is retained at this temperature for 2 hours for calcination to obtain a sintered body. The density of each (average value of n=3) is calculated based on the mass and volume of the obtained sintered body. The results are shown in Table 2. If the error of the calculated bulk density values ​​of the plurality of calcined bodies is within 3.1%, the density uniformity is regarded as high and is evaluated as "○". If it is greater than 3.1%, the density uniformity is regarded as low and is evaluated as "×". The error of the bulk density value is preferably within 3.1%, and more preferably within 3.0%.

[0118] <Method for measuring light transmittance of sintered body>

[0119] A sample was cut out from the calcined body obtained by the same method as above so that the thickness became 1.2 mm after calcination. In Examples 1 to 10 and Comparative Examples 1 to 7, the maximum calcination temperature was 1,500°C, and in Comparative Examples 8 to 10, the maximum calcination temperature was 1,450°C. The sample was retained at this temperature for 2 hours to obtain a sintered body with a thickness of 1.2 mm. The lightness (L) of the obtained sintered body was measured using a spectrophotometer (trade name "Crystalline", manufactured by Orinpass Corporation) under the condition of a seven-band measurement mode and a LED light source against a white background. W *) and the brightness (L) when the chromaticity is measured on a black background using the same test piece, the same measuring device, the same measuring mode, and the same light source. B *), the difference between the two (ΔL* (W-B) =(L W *)-(L B *)) as light transmittance (ΔL* (W-B) ) (average value of n=3).

[0120] In addition, the judgment criteria are as follows.

[0121] When the yttrium oxide content is 4 mol% or less, the light transmittance is considered to be 0 if it is 12.0 or more.

[0122] When the yttrium oxide content exceeds 4 mol% and is 5.5 mol% or less, the light transmittance is regarded as 0 if it is 15.0 or more.

[0123] When the yttrium oxide content exceeds 5.5 mol%, the light transmittance is regarded as 0 if it is 16.0 or more.

[0124] The results are shown in Table 2.

[0125] <Method for measuring biaxial bending strength of sintered body>

[0126] A sample was cut out from the calcined body obtained by the same method as above so that the sample had a diameter of 15 mm and a thickness of 1.2 mm after calcination, and was calcined at 1,500°C for 2 hours in Examples 1 to 10 and Comparative Examples 1 to 7, and was calcined at 1,450°C for 2 hours in Comparative Examples 8 to 10, to obtain a sintered body having a diameter of 15 mm and a thickness of 1.2 mm. The biaxial bending strength (average value of n=3) of the obtained sintered body was measured at a crosshead speed of 0.5 mm / min using a universal precision testing machine Autograph (trade name "AG-I 100 kN") manufactured by Shimadzu Corporation in accordance with JIS T 6526:2012. The results are shown in Table 2.

[0127] <Examples 1 to 10, Comparative Examples 1 to 7>

[0128] Zirconium oxide raw materials (zirconium dioxide, ZrO2) and yttrium oxide raw materials (yttrium oxide, Y2O3) are measured in a manner that the yttrium oxide content is the amount recorded in Table 1 relative to the total molar amount of zirconium oxide and yttrium oxide, and are put into water. It is put into a rotary container with zirconium oxide beads, crushed by a ball mill, and the raw materials are mixed and crushed until the desired primary particle size is reached. The primary particle size is measured as follows: a laser diffraction / scattering particle size distribution measuring device (trade name "Partica LA-950") manufactured by Horiba, Ltd. is used to irradiate the slurry diluted with water with ultrasound for 30 minutes, and then, it is measured on a volume basis while in contact with ultrasound. Next, a binder measured in a manner that becomes the content recorded in Table 1 is added to the slurry, and it is stirred using a rotating blade. The stirred slurry is dried and granulated using a spray dryer to obtain particles. The pellets were filled in a columnar mold, shaken thoroughly to apply vibration, compressed at a speed of 1 mm / sec, uniaxially pressed at a pressure of 33 MPa, and then CIP treated at a water pressure of 170 MPa to obtain a powder compact.

[0129] <Comparative Examples 8 to 10>

[0130] As the pellets, Zpex (registered trademark), Zpex (registered trademark) 4, and Zpex Smile (registered trademark) manufactured by Tosoh Corporation were used, and a powder compact was prepared by the same method as in Example 1.

[0131] [Table 1]

[0132]

[0133] [Table 2]

[0134]

[0135] As a result, it can be seen that in Comparative Examples 1 to 4 where the compression ratio R is less than 0.45, the shape retention of the powder compact is deteriorated and damage is observed, and in Comparative Examples 5 to 7 where the compression ratio R is more than 0.54, the light transmittance of the sintered body is deteriorated. In addition, it can be seen that in Comparative Examples 8 to 10 where the stress is small when the compression ratio R is less than 0.45 and the compression ratio is 0.6, the bulk density of the powder compact is low, and only calcined bodies and sintered bodies with low uniformity can be obtained. In contrast, it can be seen that in the examples where the compression ratio R is within the range of 0.46 to 0.53, the shape retention of the powder compact is also good, uniform calcined bodies and sintered bodies can be obtained, and zirconia sintered bodies with high light transmittance and high strength can be obtained. It can be confirmed that in the examples, even when the content of yttrium oxide is increased, high light transmittance and high strength can be achieved, and the balance is excellent.

[0136] Description of Reference Numerals

[0137] 1 Uniaxial pressure direction of the head

[0138] 2 Mould

[0139] 3 abutments

Claims

1. A particle containing zirconium oxide, a stabilizer capable of inhibiting phase transformation of zirconium oxide, and a binder, According to JIS R 1628:1997, granules are filled into the cylindrical mold by oscillation. When the compression is performed at a speed of 1 mm / sec by uniaxial pressing and the pressure is increased to 33 MPa, the compression ratio R calculated by the following formula (1) is 0.46 to 0.

53. R=(HD) / H (1) Where H represents the height of the particles filled by oscillation in the columnar mold before pressurization, and D represents the deformation amount until reaching 33 MPa. The weight average molecular weight of the polymer constituting the binder is 70,000 to 480,000. The glass transition temperature of the polymer is 50° C. or lower, or the softening point of the polymer is -40° C. or higher and 50° C. or lower, The tensile elongation of the adhesive is in the range of 120 to 800%. The average particle size of primary particles constituting the particles is 45 to 200 nm.

2. The particle according to claim 1, in, In the process of pressurizing the pellets in the columnar die, the stress when the compression ratio R reached 0.6 became 7.20 MPa or more.

3. The particle according to claim 1 or 2, in, The adhesive is a (meth)acrylic adhesive.

4. The particle according to claim 1 or 2, in, The stabilizer is yttrium oxide.

5. The particle according to claim 4, in, The content of the yttrium oxide is 2.5 to 8.5 mol % based on the total mole of zirconium oxide and yttrium oxide.

6. A powder compact comprising the granules according to any one of claims 1 to 5, wherein the bulk density of the powder compact is 3.1 to 3.5 g / cm 3 .

7. The powder compact according to claim 6, in, The stabilizer contained in the particles is yttrium oxide.

8. The powder compact according to claim 7, in, The content of the yttrium oxide is 2.5 to 8.5 mol % based on the total mole of zirconium oxide and yttrium oxide.

9. The method for producing particles according to any one of claims 1 to 5, wherein include: A step of mixing zirconium oxide with a stabilizer capable of inhibiting phase change of zirconium oxide to obtain a zirconium oxide raw material composition; a pulverizing step of pulverizing the zirconium oxide raw material composition to obtain particles having an average primary particle size of 45 to 200 nm; and a step of adding a binder to the particles and granulating the particles to obtain particles containing zirconium oxide, a stabilizer capable of inhibiting phase transformation of zirconium oxide, and the binder; The weight average molecular weight of the polymer constituting the binder is 70,000 to 480,000. The glass transition temperature of the polymer is 50° C. or lower, or the softening point of the polymer is -40° C. or higher and 50° C. or lower, The tensile elongation of the adhesive is in the range of 120 to 800%. The average particle size of primary particles constituting the particles is 45 to 200 nm.

10. The method for producing particles according to claim 9, in, The adhesive is a (meth)acrylic adhesive.

11. The method for producing particles according to claim 9 or 10, in, The stabilizer is yttrium oxide.

12. Method for manufacturing a powder compact, in, The particles according to any one of claims 1 to 5 are filled into a cylindrical mold by oscillation, When the compression is performed at a speed of 1 mm / sec by uniaxial pressing and the pressure is increased to 33 MPa, the compression ratio R calculated by the following formula (1) is 0.46 to 0.

53. R=(HD) / H (1) In the formula, H represents the height of the particles filled by oscillation in the columnar mold before pressurization, and D represents the deformation amount until 33 MPa is reached.

13. The method for producing a powder compact according to claim 12, in, In the process of pressurizing the pellets in the columnar die, the stress when the compression ratio R reached 0.6 became 7.20 MPa or more.

Citation Information

Patent Citations

  • Ceramic granule for press molding

    JP2006027914A

  • Light-transmitting zirconia sintered compact, zirconia powder and application thereof

    JP2015143178A

  • Translucent zirconia sintered body and zirconia powder, and use therefor

    CN105829264A

  • Light transmittance zirconium oxide sintered body, preparation method and application thereof

    CN106396676A

  • Zirconia fine powder and production method therefor

    CN108137342A