Cracked frit, ceramic brick and preparation method thereof
By adding B2O3 to the cracked frit and setting a protective glaze layer, the problems of high firing temperature and long firing time of the existing cracked frit are solved, low energy consumption and high efficiency ceramic tile production is achieved, and the artistic crackle effect and Industrial application.
Patent Information
- Application Number
- CN202310795178.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-30
AI Technical Summary
The existing cracked frit is fired at high temperatures and for a long time, resulting in high energy consumption, low efficiency, and high manufacturing costs.
By adding B2O3 as a strong flux in the cracked frit, SiO2 and alkaline oxides are combined to form a glass body at low temperatures, lowering the firing temperature, and setting a protective glaze layer in the ceramic tiles to avoid the pattern decoration layer reacting with the components of the crack layer. , using a secondary firing process to control the firing temperature and time.
It significantly reduces the firing temperature and time of the crack frit, improves production efficiency, reduces energy consumption and manufacturing costs, and avoids the influence of the color development effect of the pattern decorative layer, achieving the control of artistic crack effects and industrialized production.
Smart Images

Figure BDA0004314793080000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramics, and in particular to a cracked frit, a ceramic brick and a preparation method thereof. Background Art
[0002] As a traditional artistic glaze, crackle glaze is cherished by the world for its unique artistic effect. With its unique aesthetic, it adds a poetic and cold beauty to ceramic products. Crackle glaze is perfectly combined with painting art and color glaze, with rich colors, lively stripes, elegant and clean glaze pigments, and a glaze layer as moist as jade. However, the existing crackle glaze or crackle frit needs to be fired in a tunnel kiln or shuttle kiln at a temperature of up to 1230℃, and the firing time is as long as more than 6 hours, and some even as long as more than ten hours, which has the disadvantages of high energy consumption, low efficiency, and high manufacturing cost.
[0003] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0004] Based on the above-mentioned deficiencies of the prior art, the object of the present invention is to provide a crack frit, a ceramic tile and a preparation method thereof, aiming to solve the problem of high sintering temperature of the existing crack frit.
[0005] The technical solution of the present invention is as follows:
[0006] A first aspect of the present invention provides a cracked frit, wherein the chemical composition of the cracked frit comprises, by weight:
[0007] SiO2 50-60 parts, Al2O3 5-13 parts, Fe2O3 0-1 part, CaO 4-7 parts, MgO 0-3 parts, K2O 0-3 parts, Na2O 12-17 parts, BaO 2-6 parts, B2O3 13-17 parts.
[0008] A second aspect of the present invention provides a ceramic tile, which includes a stacked ceramic body and a crack layer, wherein the crack layer is prepared from the crack frit described above in the present invention.
[0009] Optionally, a bottom glaze layer, a pattern decoration layer, and a protective glaze layer are stacked in sequence between the ceramic body and the crack layer, wherein the bottom glaze layer is arranged in contact with the ceramic body, and the protective glaze layer is arranged in contact with the crack layer;
[0010] The protective glaze layer includes the following chemical components:
[0011] SiO2 58-64 parts, Al2O3 10-16 parts, CaO 1-5 parts, MgO 1-5 parts, (K2O+Na2O) 5-12 parts, ZnO 4-8 parts, B2O3 3-7 parts.
[0012] Optionally, the protective glaze layer has a thickness of 0.15 to 0.25 mm by mass.
[0013] Optionally, the pattern decoration layer is prepared from a color glaze, and the color glaze includes a transparent glaze and a colorant. The chemical composition of the transparent glaze includes, by mass:
[0014] SiO2 55-62 parts, Al2O3 6-11 parts, CaO 4-10 parts, MgO 0.5-3 parts, K2O 1-3 parts, Na2O 1-3 parts, ZnO 4-10 parts, BaO 1-5 parts, PbO 6-10 parts, B2O3 5-9 parts, loss on ignition 0-0.6 parts;
[0015] The pigment includes at least one of spinel pigments, tin-based pigments, zirconium-based pigments, and encapsulated pigments.
[0016] The third aspect of the present invention provides a method for preparing a ceramic tile, which comprises the steps of:
[0017] Providing a ceramic green body and then performing a first firing;
[0018] The crack frit of the present invention is applied to the ceramic green body after the first firing, and then fired for the second time to obtain a ceramic tile including a ceramic green body and a crack layer stacked together.
[0019] Optionally, the method for preparing the ceramic tile specifically comprises the steps of:
[0020] Providing a ceramic green body;
[0021] Applying a base glaze on the ceramic green body and performing a first firing;
[0022] Then, after applying color ink, protective glaze and crack frit in sequence, a second firing is carried out to obtain a ceramic tile including a ceramic body, a base glaze layer, a pattern decoration layer, a protective glaze layer and a crack layer stacked together.
[0023] Optionally, the temperature of the first sintering is 1200-1250° C., and the time of the first sintering is 38-42 minutes.
[0024] Optionally, the temperature of the second sintering is 1100-1130° C., and the time of the second sintering is 60-70 minutes.
[0025] Optionally, the method for preparing the color ink comprises the steps of:
[0026] Mixing transparent glaze and colorant to obtain color glaze;
[0027] Adding a solvent and a diluent to the color glaze to obtain a color ink;
[0028] Wherein, the chemical composition of the transparent glaze includes, by weight:
[0029] SiO2 55-62 parts, Al2O3 6-11 parts, CaO 4-10 parts, MgO 0.5-3 parts, K2O 1-3 parts, Na2O 1-3 parts, ZnO 4-10 parts, BaO 1-5 parts, PbO 6-10 parts, B2O3 5-9 parts, loss on ignition 0-0.6 parts;
[0030] The pigment includes at least one of spinel pigment, tin-based pigment, zirconium-based pigment and encapsulated pigment;
[0031] And / or, the color ink is applied by splashing ink, painting or pen painting.
[0032] Beneficial effects: The present invention adds a relatively large amount of B2O3 to the crack frit. B2O3, as a strong flux and network former, can be co-melted with SiO2 and alkaline oxides to form a glass body at low temperature, which can significantly reduce the sintering temperature of the crack frit. DETAILED DESCRIPTION
[0033] The present invention provides a cracked frit, a ceramic tile and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0034] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0035] The existing crack frits require a firing temperature of up to 1230°C when fired in a tunnel kiln or shuttle kiln, and the required firing time is as long as more than 6 hours, and some even as long as more than ten hours. Based on this, an embodiment of the present invention provides a crack frit, whose firing temperature is 1100-1130°C and the firing time is 60-70 minutes. Specifically, the chemical composition of the crack frit includes, by mass:
[0036] SiO2 50-60 parts, Al2O3 5-13 parts, Fe2O3 0-1 part, CaO 4-7 parts, MgO 0-3 parts, K2O 0-3 parts, Na2O 12-17 parts, BaO 2-6 parts, B2O3 13-17 parts.
[0037] The crack frit in the embodiment of the present invention has significantly higher contents of B2O3 and Na2O than ordinary frit. B2O3, as a strong flux and network former, can be eutectic with SiO2 and alkaline oxides to form a glass body at low temperature, which can significantly reduce the firing temperature of the crack frit. Specifically, the addition of B2O3 can reduce the initial melting temperature and firing temperature of the crack frit, greatly shortening the firing cycle. At the same time, the high content of Na2O further reduces the melting temperature of the crack frit, greatly reduces the melt viscosity, reduces the generation of crack layer (crack layer formed after the crack frit is fired) defects, and shortens the firing time.
[0038] In addition, when a large amount of B2O3 is added to the crack frit, boron anomaly will occur, which will not only fail to reduce the expansion coefficient of the crack frit, but will increase the expansion coefficient of the crack frit, making it greater than the expansion coefficient of the ceramic body and the bottom glaze layer, and then generate a large tensile stress during the cooling process, resulting in cracks. The B2O3 ratio described in this embodiment can make the crack frit have a suitable expansion coefficient, and realize the preparation of the crack layer.
[0039] An embodiment of the present invention further provides a ceramic tile, which includes a stacked ceramic body and a crack layer, wherein the crack layer is prepared from the crack frit described above in the embodiment of the present invention.
[0040] The embodiments of the present invention do not limit the specific composition of the ceramic body, and any ceramic body that can form a crack layer on the surface of the cracked frit is within the protection scope of the present invention. As an example, the raw materials of the ceramic body include, by weight:
[0041] 15-23 parts of kaolin, 9-17 parts of ball clay, 48-58 parts of feldspar, 1-5 parts of black talc, 1-5 parts of diopside;
[0042] Wherein, the feldspar includes at least one of albite and potassium feldspar.
[0043] Existing artistic ceramics usually use crackle glaze (or crackle frit) and color glaze for glaze decoration. When color glaze is used as in-glaze color or under-glaze color, some coloring oxides will react with crackle glaze components (or crackle frit components) to affect the coloring effect. Based on this, the present invention sets a protective glaze layer between the crack layer and the pattern decoration layer to prevent the crack layer from reacting with the components of the pattern decoration layer and affecting the coloring effect. Specifically, in some embodiments, the ceramic body and the crack layer also include a bottom glaze layer, a pattern decoration layer, and a protective glaze layer stacked in sequence, wherein the bottom glaze layer is arranged in contact with the ceramic body, and the protective glaze layer is arranged in contact with the crack layer; the protective glaze layer includes the following chemical components:
[0044] SiO2 58-64 parts, Al2O3 10-16 parts, CaO 1-5 parts, MgO 1-5 parts, (K2O+Na2O) 5-12 parts, ZnO 4-8 parts, B2O3 3-7 parts.
[0045] In the present embodiment, the provision of the protective glaze layer can not only prevent the crack layer from reacting with the components of the pattern decoration layer to affect the coloring effect, but its most important function is to adjust the coloring of the pattern decoration layer and increase the sense of transparency. ZnO contributes to the coloring of colors such as bright red and orange, while B2O3 contributes to the coloring of colors such as yellow and black, thereby minimizing the covering of the crack melt on the pattern decoration layer.
[0046] In some embodiments, the protective glaze layer may further include 0.05 to 0.1 parts by weight of an ink-repellent agent. The addition of the ink-repellent agent provides a better protective effect and is more conducive to preventing the crack layer from reacting with the components of the pattern decoration layer.
[0047] In some embodiments, the protective glaze layer has a thickness of 0.15 to 0.25 mm by mass, for example, 0.15 mm, 0.18 mm, 0.20 mm, 0.22 mm, 0.24 mm or 0.25 mm, etc. This thickness can effectively prevent the crack layer from reacting with the components of the pattern decoration layer.
[0048] In some embodiments, the pattern decoration layer is prepared from a color glaze, and the color glaze includes a transparent glaze and a colorant. The chemical composition of the transparent glaze includes, by mass:
[0049] SiO2 55-62 parts, Al2O3 6-11 parts, CaO 4-10 parts, MgO 0.5-3 parts, K2O 1-3 parts, Na2O 1-3 parts, ZnO 4-10 parts, BaO 1-5 parts, PbO 6-10 parts, B2O3 5-9 parts, loss on ignition 0-0.6 parts;
[0050] The pigment includes at least one of spinel pigments, tin-based pigments, zirconium-based pigments, and encapsulated pigments.
[0051] In this embodiment, the transparent glaze is a lead-boron transparent glaze, which can reduce the firing temperature of the colorant while ensuring the coloring effect of the colorant. Compared with glass white (mainly made of arsenic, lead, and saltpeter, which is only good for the coloring of some colorants, such as brown), the transparent glaze in this embodiment contains a larger amount of CaO, ZnO, PbO, BaO, etc., and comprehensively considers the coloring effects of different types and colors of colorants.
[0052] In some embodiments, the spinel pigment includes but is not limited to 0.2CoO·0.8ZnO·Al2O3 spinel cobalt blue pigment. The encapsulated pigment includes but is not limited to ZrSiO4 / Cd(S x Se 1-x ) encapsulates the pigment, which can present all transitional colors from bright red to orange and yellow, where 0≤x≤1, ZrSiO4 / Cd(S x Se 1-x ) indicates that ZrSiO4 is used as an inclusion to encapsulate Cd(S x Se 1-x ).
[0053] In some embodiments, the transparent glaze and the colorant have finenesses that can pass through a 350-mesh sieve.
[0054] The present invention does not limit the specific chemical composition of the bottom glaze layer, and any bottom glaze layer that can form a crack layer on the surface of the cracked frit is within the protection scope of the present invention. As an example, the chemical composition of the bottom glaze layer includes, by weight:
[0055] SiO2 48-56 parts, Al2O3 14-22 parts, CaO 3-9 parts, MgO 2-8 parts,
[0056] (K2O+Na2O) 2-6 parts, ZnO 2-4 parts, BaCO3 1-5 parts, ZrO2 8-18 parts, TiO2 0-1 parts, Fe2O3 0-0.5 parts, loss on ignition (IL) 0.4-0.8 parts;
[0057] Among them, K2O and Na2O are 2 to 6 parts in total, and the ratio between the two can be any value, such as 1:1, 1:2, 2:1, etc.
[0058] The embodiment of the present invention also provides a method for preparing a ceramic tile, which comprises the steps of:
[0059] S11, providing a ceramic green body, and then performing a first firing;
[0060] S12, applying the crack frit described in the embodiment of the present invention to the ceramic green body after the first firing, and then firing for a second time to obtain a ceramic tile including a ceramic green body and a crack layer stacked together.
[0061] In this embodiment, the ceramic green body is formed after two firings, and the crack frit applied to the ceramic green body is formed after two firings to form a crack layer. In the ceramic tile of this embodiment, the crack frit as described above in the embodiment of the present invention is used, and the crack frit is fired at a low temperature.
[0062] In some embodiments, the temperature of the first sintering is 1200-1250° C., and the time of the first sintering is 38-42 minutes.
[0063] In some embodiments, the second firing temperature is 1100-1130°C, and the second firing time is 60-70 minutes. That is, the firing temperature of the cracked frit is 1100-1130°C, and the firing time is 60-70 minutes, which is significantly lower than the firing temperature of the existing cracked frit and shorter than the firing time of the existing cracked frit.
[0064] In some embodiments, the method for preparing the ceramic tile specifically comprises the steps of:
[0065] S21, providing a ceramic green body;
[0066] S22, applying a base glaze on the ceramic green body and performing a first firing;
[0067] S23, then apply color ink, protective glaze, and crack frit in sequence, and then perform a second firing to obtain a ceramic tile including a ceramic body, a base glaze layer, a pattern decoration layer, a protective glaze layer, and a crack layer stacked together.
[0068] In this embodiment, the ceramic green body is formed after two firings, and the base glaze, color ink, protective glaze and crack frit applied on the ceramic green body in sequence are respectively formed after two firings to form a base glaze layer, a pattern decoration layer, a protective glaze layer and a crack layer. For the convenience of description, the ceramic green body and the base glaze are fired for the first time to obtain a ceramic green body fired once and a base glaze layer fired once.
[0069] In this embodiment, the ceramic tile is prepared by a double firing process, and the color effect of the ceramic body and the bottom glaze layer fired once is not limited; artistic painting can be applied on the surface of the bottom glaze layer fired once, and different types of paintings can be outlined and altered at will to form a pattern decoration layer. In this embodiment, "using pottery as paper" facilitates creation, adds verve to architectural ceramic products, and enhances product value.
[0070] In step S21, in some embodiments, the method for preparing the ceramic green body comprises the steps of:
[0071] S211, by weight, 15-23 parts of kaolin, 9-17 parts of ball clay, 48-58 parts of feldspar, 1-5 parts of black talc, 1-5 parts of diopside, 0.1-0.2 parts of water glass, and 0.2-0.3 parts of sodium tripolyphosphate are mixed, and then wet-milled to obtain a green body slurry, wherein the fineness of the green body slurry is 0.6-1.5% of the mass of the residual mud after passing through a 325-mesh sieve;
[0072] S212, spray drying the green body slurry to obtain a green body powder, wherein the green body powder has a moisture content of 6.5-7.5% by weight;
[0073] S213, after aging for 48 hours to balance the moisture, the green body powder is pressed into shape, and after drying, the ceramic green body is obtained.
[0074] In step S22, in some embodiments, the step of applying a base glaze on the ceramic green body and performing a first firing specifically includes:
[0075] S221. According to parts by mass, 48-56 parts of SiO2, 14-22 parts of Al2O3, 3-9 parts of CaO, 2-8 parts of MgO, 2-6 parts of (K2O+Na2O), 2-4 parts of ZnO, 1-5 parts of BaCO3, 8-18 parts of ZrO2, 0-1 parts of TiO2, 0-0.5 parts of Fe2O3, 0.4-0.8 parts of loss on ignition, and 0.3-0.5 parts of sodium carboxymethyl cellulose and sodium tripolyphosphate in total are subjected to wet ball milling and then aged to obtain a base glaze slurry, wherein the base glaze slurry has a fineness of 0.2-0.5% of the mass of the base glaze slurry remaining after passing through a 325-mesh sieve, a specific gravity of 1.7-1.8, and a flow rate of 26-35s;
[0076] S222, according to 500 ~ 600g / m 2 The base glaze slurry is applied to the ceramic body in a pouring manner with a glazing amount, and after drying, the first firing is performed (temperature is 1200-1250° C., time is 38-42 minutes).
[0077] In step S23, in some embodiments, the method for preparing the color ink comprises the steps of:
[0078] S231, mixing the transparent glaze and the colorant to obtain a colored glaze;
[0079] Wherein, the chemical composition of the transparent glaze includes, by weight:
[0080] SiO2 55-62 parts, Al2O3 6-11 parts, CaO 4-10 parts, MgO 0.5-3 parts, K2O 1-3 parts, Na2O 1-3 parts, ZnO 4-10 parts, BaO 1-5 parts, PbO 6-10 parts, B2O3 5-9 parts, loss on ignition 0-0.6 parts;
[0081] The pigment includes at least one of spinel pigments, tin-based pigments, zirconium-based pigments, and encapsulated pigments.
[0082] S232, adding a solvent and a diluent to the color glaze to obtain a color ink.
[0083] In this embodiment, the color ink has a wide range of applications and can be used for both light-colored and dark-colored products; some defective products can also be artistically processed by applying color ink, greatly reducing the waste of ceramic products.
[0084] In steps S231-S232, the transparent glaze and the pigments of different components may be mixed to obtain the colored glaze, and then a certain solvent may be added thereto for grinding to obtain a paste pigment, and then a diluent may be added to the paste pigment according to actual needs to obtain a colored ink. The fineness of the transparent glaze and the pigment is such that they can pass through a 350-mesh screen.
[0085] In the present invention, a variety of single-color inks can be obtained by combining different colorants with transparent glazes. When preparing a pattern decoration layer for painting, different color inks can be matched to obtain the desired color. Different color inks can also be mixed by adopting different processes according to the picture effect.
[0086] In some embodiments, the solvent includes but is not limited to at least one of glycerin, rosin resin, and castor oil. In some specific embodiments, the solvent includes 1.5 to 2.5 parts of glycerin, 0.4 to 0.5 parts of rosin resin, and 0.8 to 2 parts of castor oil by weight. The color ink uses glycerin, rosin resin, and castor oil as solvents to paint on the surface of ceramic tiles, and the drying degree is fast and the adhesion performance is good.
[0087] In some embodiments, the diluent includes but is not limited to camphor oil.
[0088] In some embodiments, the color ink is applied by splashing, painting or brushing, and then dried at a temperature of 170 to 200° C. for 10 to 20 minutes.
[0089] In some embodiments, the chemical composition of the protective glaze includes:
[0090] SiO2 58-64 parts, Al2O3 10-16 parts, CaO 1-5 parts, MgO 1-5 parts, (K2O+Na2O) 5-12 parts, ZnO 4-8 parts, B2O3 3-7 parts;
[0091] Among them, K2O and Na2O are 5 to 12 parts in total, and the ratio between K2O and Na2O can be any ratio, such as 1:1, 1:2, etc.
[0092] In some embodiments, the second firing temperature is 1100°C to 1130°C, for example, 1100, 1110, 1120 or 1130°C; the second firing time is 60 to 70 min, for example, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69 or 70 min.
[0093] Example 1
[0094] This embodiment provides a cracked frit, the cracked frit has a fineness of being able to pass through a 40-mesh sieve, and includes the following chemical components by weight:
[0095] SiO2 50.3 parts, Al2O3 6.93 parts, Fe2O3 0.14 parts, CaO 6.29 parts, MgO 0.63 parts, K2O 1.52 parts, Na2O 15.73 parts, BaO 3.68 parts, B2O3 14.78 parts.
[0096] Comparative Example 1
[0097] This comparative example provides a cracked frit, which is different from Example 1 only in that the chemical composition of the cracked frit in Comparative Example 1 is 0 parts of B2O3, and the remaining chemical components and parts are the same as those in Example 1.
[0098] Comparative Example 2
[0099] This comparative example provides a cracked frit, which is different from Example 1 only in that the chemical composition of the cracked frit in Comparative Example 2 is 7 parts of B2O3, and the remaining chemical components and the proportions are the same as those in Example 1.
[0100] The initial melting temperature, firing temperature and glaze gloss of the cracked frits in Example 1 and Comparative Example 1 were tested, and the results are shown in Table 1 below; the expansion coefficient of the cracked frits in Example 1 and Comparative Examples 1-2 was tested, and the results are shown in Table 2 below.
[0101] Table 1 Test results of the initial melting temperature, firing temperature and glaze gloss of the crack frit in Example 1 and Comparative Example 1
[0102]
[0103]
[0104] It can be seen that the introduction of B2O3 into the cracked frit can significantly reduce the initial melting temperature and sintering temperature of the cracked frit. At the same time, when a large amount of B2O3 is added to the formula, it will cause boron anomaly, which will not only fail to reduce the expansion coefficient of the cracked frit, but will increase the expansion coefficient of the cracked frit, as shown in Table 2 below.
[0105] Table 2 Expansion coefficient results
[0106] Example Expansion coefficient Comparative Example 1 230 Comparative Example 2 210 Example 1 305
[0107] It can be seen from Comparative Examples 1 and 2 that adding a certain amount of B2O3 to the cracked frit will reduce the expansion coefficient of the cracked frit. It can be seen from Comparative Examples 1-2 and Example 1 that when more B2O3 is added to the cracked frit, boron anomaly will occur, which will not only fail to reduce the expansion coefficient of the cracked frit, but will increase the expansion coefficient of the cracked frit.
[0108] Example 2
[0109] This embodiment provides a protective glaze, the fineness of the protective glaze is that a 40-mesh screen can pass through it, and the chemical composition of the protective glaze includes, by weight:
[0110] SiO2 60.85 parts, Al2O3 14.91 parts, CaO 3.97 parts, MgO 2.58 parts, K2O 4 parts, Na2O 4.42 parts, ZnO 6.01 parts, B2O3 3.26 parts.
[0111] Example 3
[0112] This embodiment provides a color glaze, which includes 70 parts of a uniformly mixed transparent glaze and 30 parts of a 0.2CoO·0.8ZnO·Al2O3 spinel cobalt blue colorant, by weight. The chemical composition of the transparent glaze includes:
[0113] SiO2 55.32 parts, Al2O3 6.71 parts, CaO 6.01 parts, MgO 0.84 parts, K2O 2.31 parts, Na2O 2.34 parts, ZnO 8.65 parts, BaO 1.96 parts, PbO 8.75 parts, B2O3 6.43 parts, loss on ignition 0.55 parts.
[0114] This embodiment also provides a color ink, which includes, by weight, 70 parts of a transparent glaze, 30 parts of a 0.2CoO·0.8ZnO·Al2O3 spinel type cobalt blue colorant, 40 parts of a solvent, and 30 parts of camphor oil. The preparation method thereof includes the following steps:
[0115] Mix 70 parts of a transparent glaze and 30 parts of a 0.2CoO·0.8ZnO·Al2O3 spinel type cobalt blue colorant by weight to obtain a colored glaze;
[0116] Add 40 parts of solvent to the above color glaze, and mix to obtain a paste pigment;
[0117] The paste pigment is mixed with 30 parts of camphor oil to obtain color ink.
[0118] The solvent includes glycerin, rosin resin and castor oil mixed in a mass ratio of 2:0.4:1.
[0119] Example 4
[0120] This embodiment provides a method for preparing an artistic crack ceramic tile, comprising the steps of:
[0121] (1) Preparation of ceramic greenware
[0122] Each raw material is aged, homogenized, and crushed (to improve the efficiency and accuracy of wet ball milling) so that the fineness of each raw material D50 is <3mm.
[0123] By weight, 20 parts of kaolin, 13 parts of ball clay, 20 parts of albite, 28 parts of potassium feldspar, 5 parts of black talc, 2 parts of diopside, 0.1 parts of water glass, and 0.3 parts of sodium tripolyphosphate are mixed, and then wet-milled to obtain a green body slurry, wherein the fineness of the green body slurry is 0.8% of the mass of the green body slurry remaining after passing through a 325-mesh sieve;
[0124] The green body slurry is spray-dried to obtain a green body powder (with a water content of 6.5%);
[0125] After aging for 48 hours, the green body powder was hydraulically formed by an automatic hydraulic press with a pressure of 50 MPa, and after drying, a ceramic green body with a specification of 670 mm×670 mm (with a water content of less than 0.5% by mass) was obtained.
[0126] (2) Applying base glaze on the surface of ceramic green body
[0127] By mass, according to 50 parts of SiO2, 18 parts of Al2O3, 5 parts of CaO, 6 parts of MgO, 2 parts of K2O, 3 parts of Na2O, 3 parts of ZnO, 2 parts of BaCO3, 15 parts of ZrO2, 1 part of TiO2, 0.2 parts of Fe2O3, 0.4 parts of loss on ignition, 0.2 parts of sodium carboxymethyl cellulose, and 0.2 parts of sodium tripolyphosphate, the raw materials for the base glaze are wet-ball milled, and then aged for 24 hours to obtain a base glaze slurry, the fineness of the base glaze slurry is 0.3% of the mass of the base glaze slurry remaining after passing through a 325-mesh sieve, the specific gravity is 1.7, and the flow rate is 34s;
[0128] According to 550g / m 2 The base glaze slurry is applied to the ceramic green body in a pouring manner with a glazing amount, and after drying, it is fired in an oxidizing atmosphere of a roller kiln at 1200° C. for 40 minutes to form a once-fired base glaze layer.
[0129] (3) Apply color ink, protective glaze, and crack frit
[0130] The color ink in Example 3 is applied on the primary fired base glaze layer in a splashing manner and dried at 180° C. for 10 min;
[0131] Then, the protective glaze in Example 2 and the crack frit in Example 1 are applied in sequence, and fired in an oxidizing atmosphere of a roller kiln at 1100°C for 65 minutes to form the artistic crack ceramic tile, which includes a ceramic body, a base glaze layer, a pattern decoration layer, a protective glaze layer, and a crack layer stacked in sequence, wherein the thickness of the protective glaze layer is 0.2 mm.
[0132] In this embodiment, the artistic crack ceramic tiles pass through the roller kiln, and the temperature difference in the kiln is small, which can achieve stable temperature control and precise firing time control; the surface flatness of the ceramic body is high, and the weight of the crack frit applied can be accurate to grams, ensuring the uniform thickness of the artistic crack layer; ensuring that the crack effect is controllable, while greatly compressing the firing time, and achieving the industrialization of artistic ceramic products. In this embodiment, low-temperature color ink is used, and the protective glaze is combined with the crack frit to achieve the preparation of repeatable and controllable artistic architectural ceramics with a certain crack effect.
[0133] In summary, the present invention adds a relatively large amount of B2O3 to the crack frit. B2O3, as a strong flux and network former, can be eutectic with SiO2 and alkaline oxides to form a glass body at low temperature, which can significantly reduce the firing temperature of the crack frit. The color glaze (including transparent glaze and colorant) provided by the present invention has a low firing temperature, bright color, and controllable effect; compared with the existing high-temperature color glaze, the firing temperature is high, the heat preservation time is long, and the effect difference is large, which has obvious advantages, can greatly reduce production costs, improve production efficiency, and can also be used for the industrialized production of artworks. The ceramic tile provided by the present invention adopts a secondary firing process, and is not limited to the color effect of the ceramic body and the bottom glaze layer fired once; through the combination of different colorants and transparent glazes, a variety of single-color color inks can be obtained, and different color inks can be proportioned to obtain the required color. The color ink is used to perform artistic painting on the surface of the bottom glaze layer after the primary firing, and different types of paintings can be outlined, and can be altered at will to form a pattern decoration layer. The present invention "uses pottery as paper" to facilitate creation, add verve to architectural ceramic products, and enhance product value. The pattern decoration layer is protected by the protective glaze layer to prevent the chemical components of the pattern decoration layer and the crack layer from directly reacting, which fundamentally solves the problem of poor color development of the pattern decoration layer after the composite crack layer; At the same time, crack frits are used to obtain better artistic cracks, thereby achieving the special-shaped crack art effect. In addition, the present invention adopts roller kiln firing for both the primary and secondary firing, and the firing temperature and time are controllable. The artistic crack effect after firing is controllable and repeatable, and the color development of the pattern decoration layer is adjustable, controllable, and repeatable.
[0134] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A ceramic tile, It is characterized in that The invention comprises a ceramic body and a crack layer which are stacked, wherein the crack layer is prepared from a crack frit, and the chemical composition of the crack frit comprises, by weight: SiO 2 50-60 parts, Al 2 O 3 5-13 parts, Fe 2 O 3 0~1 parts, CaO 4~7 parts, MgO 0~3 parts, K 2 O 0 to 3 parts, Na 2 O 12-17 parts, BaO 2-6 parts, B 2 O 3 13-17 servings; The ceramic body and the crack layer further include a bottom glaze layer, a pattern decoration layer, and a protective glaze layer stacked in sequence, wherein the bottom glaze layer is arranged in contact with the ceramic body, and the protective glaze layer is arranged in contact with the crack layer; by weight, The protective glaze layer includes the following chemical components: SiO 2 58~64 parts, Al 2 O 3 10-16 parts, CaO 1-5 parts, MgO 1-5 parts, (K 2 O+Na 2 O) 5-12 parts, ZnO 4-8 parts, B 2 O 3 3 to 7 servings.
2. The ceramic tile according to claim 1, It is characterized in that The thickness of the protective glaze layer is 0.15-0.25 mm.
3. The ceramic tile according to claim 1, It is characterized in that The pattern decoration layer is prepared from color glaze, and the color glaze includes transparent glaze and colorant. The chemical composition of the transparent glaze includes: SiO 2 55~62 parts, Al 2 O 3 6-11 parts, CaO 4-10 parts, MgO 0.5-3 parts, K 2 O 1 to 3 parts, Na 2 O 1-3 parts, ZnO 4-10 parts, BaO 1-5 parts, PbO 6-10 parts, B 2 O 3 5-9 parts, loss on ignition 0-0.6 parts; The pigment includes at least one of spinel pigments, tin-based pigments, zirconium-based pigments, and encapsulated pigments.
4. A method for preparing the ceramic tile according to claim 1, It is characterized in that Includes steps: Providing a ceramic green body; Applying a base glaze on the ceramic green body and performing a first firing; Then, after applying color ink, protective glaze and crack frit in sequence, a second firing is carried out to obtain a ceramic tile including a ceramic body, a base glaze layer, a pattern decoration layer, a protective glaze layer and a crack layer stacked together.
5. The preparation method according to claim 4, It is characterized in that The temperature of the first sintering is 1200-1250° C., and the time of the first sintering is 38-42 minutes.
6. The preparation method according to claim 4, It is characterized in that The temperature of the second firing is 1100-1130° C., and the time of the second firing is 60-70 minutes.
7. The preparation method according to claim 4, It is characterized in that The method for preparing the color ink comprises the steps of: Mixing transparent glaze and colorant to obtain color glaze; Adding a solvent and a diluent to the color glaze to obtain a color ink; Wherein, by weight, the chemical composition of the transparent glaze includes: SiO 2 55~62 parts, Al 2 O 3 6-11 parts, CaO 4-10 parts, MgO 0.5-3 parts, K 2 O 1 to 3 parts, Na 2 O 1-3 parts, ZnO 4-10 parts, BaO 1-5 parts, PbO 6-10 parts, B 2 O 3 5-9 parts, loss on ignition 0-0.6 parts; The pigment includes at least one of spinel pigments, tin-based pigments, zirconium-based pigments, and encapsulated pigments.
8. The preparation method according to claim 7, It is characterized in that The color ink is applied by splashing ink, painting or pen painting.
Citation Information
Patent Citations
Light-transmitting ceramic tile with ice crack effect and preparation process of light-transmitting ceramic tile
CN115433022A