A lanthanide element co-doped with Ga and Mo CaBi4Ti4O 15 High temperature piezoelectric ceramic material and preparation method thereof
By doping lanthanides and Ga and Mo ions into CaBi4Ti4O15 ceramic material, the problem of low piezoelectric activity of high-temperature piezoelectric ceramic materials in the prior art is solved, and high-temperature piezoelectric ceramic materials with excellent high-temperature stability and electrical properties are achieved , suitable for high temperature environments.
Patent Information
- Application Number
- CN202311185698.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-09-14
AI Technical Summary
The existing perovskite structure PZT-based piezoelectric ceramic materials cannot work properly above Curie temperature, and the piezoelectric activity of bismuth layered ceramic materials is low, which limits its application in the field of high temperature.
By co-doping with Ga and Mo in CaBi4Ti4O15 ceramic materials, the lanthanide elements (such as La3+, Nd3+, Sm3+) with Ga and Mo, replacing Ca2+ and Ti4+ ions, Ca1-xMxBi4-y[Ga1/3Mo2/3]yO15, improving the material's Piezoelectric properties and high temperature resistivity.
It realizes the improvement of piezoelectric performance and high-temperature resistivity without reducing Curie temperature, and obtains high-temperature piezoelectric ceramic materials with excellent comprehensive electrical performance. They are suitable for high-temperature environments, have good stability and broad application prospects.
Smart Images

Figure CN117263675B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of piezoelectric ceramic materials, and in particular to a bismuth calcium titanate high-temperature piezoelectric ceramic material with a bismuth layered structure and a preparation method thereof. Background Art
[0002] At present, the most widely used piezoelectric ceramic materials are mainly PZT-based piezoelectric ceramics with perovskite structure, but the Curie temperature of this type of piezoelectric ceramics is generally below 400℃. Due to the existence of depolarization phenomenon of piezoelectric materials, piezoelectric materials cannot work normally above the Curie temperature. With the rapid development of aerospace, geological exploration and other work and in line with the needs of sustainable development of human society, it is necessary to seek an environmentally friendly piezoelectric material with high Curie temperature and excellent piezoelectric performance.
[0003] Bismuth layered ceramics have the advantages of high Curie temperature and good fatigue resistance, and are candidate materials for use in high temperature environments. 2 O 2 ) 2+ The layers and perovskite structure lattice layers are alternately stacked, and its chemical formula is (Bi 2 O 2 ) 2+ (A m-1 B m O 3m+1 ) 2- , among which CaBi 4 Ti 4 O 15 (CBT) is a typical bismuth layered ferroelectric material, A is a 12-coordinated Ca 2+ and Bi 3+ , B is 6-coordinated Ti 4+ , m = 4, the material has a high Curie temperature (T C ≈790℃), high voltage coefficient, low conductivity and other advantages, but its piezoelectric activity is low and the temperature coefficient of resonance frequency is large, which restricts its application in high temperature fields. Therefore, how to improve the piezoelectric activity without reducing the Curie temperature and obtain CBT piezoelectric ceramic materials with excellent comprehensive electrical properties has become an important research topic in the field of high temperature piezoelectric ceramic materials. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a lanthanide element and Ga, Mo co-doped CaBi 4 Ti 4 O 15 High temperature piezoelectric ceramic materials, for CaBi 4 Ti 4 O 15Ca in the A position of ceramic materials 2+ Ions are replaced by 12-coordinated +3-valent lanthanide metal ions for doping. 4+ ions, using composite high-valent ions [Ga 1 / 3 Mo 2 / 3 ] 5+ Doping substitution is performed so that through the above-mentioned composite doping modification, the piezoelectric properties and high-temperature resistivity are improved without reducing the Curie temperature, thereby providing a new type of piezoelectric ceramic material with excellent comprehensive electrical properties and environmentally friendly. Another object of the present invention is to provide the above-mentioned lanthanide elements and Ga, Mo co-doped CaBi 4 Ti 4 O 15 Preparation method of high temperature piezoelectric ceramic material.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] The present invention provides a lanthanide element and Ga, Mo co-doped CaBi 4 Ti 4 O 15 High temperature piezoelectric ceramic material, doped with 12-coordinated +3-valent lanthanide metal ion M to replace CaBi 4 Ti 4 O 15 Ca in the A position 2+ ions, with complex high-valent ions [Ga 1 / 3 MO 2 / 3 ] 5+ Doping substitution CaBi 4 Ti 4 O 15 Ti in the middle B position 4+ ions, the chemical formula is Ca 1-x M x Bi 4 Ti 4-y [Ga 1 / 3 MO 2 / 3 ] y O 15 , where 0.03≤x≤0.08, 0.05≤y≤0.075, M is La 3+ 、Nd 3+ , or Sm 3+ ion.
[0007] In the above scheme, the piezoelectric ceramic material of the present invention has a 33 ≥25pC / N, T C ≥760℃; Resistivity (ρ) ≥2.2×10 at 500℃ 7Ω·cm, dielectric loss (tanδ) ≤ 0.48%; d after annealing at 600℃ 33 ≥21pC / N.
[0008] Another object of the present invention is achieved by the following technical solutions:
[0009] The lanthanide elements provided by the present invention are co-doped with Ga and Mo in the form of CaBi 4 Ti 4 O 15 A method for preparing a high temperature piezoelectric ceramic material comprises the following steps:
[0010] (1) Preparation of pre-synthesized precursor powder
[0011] CaCO 3 、Bi 2 O 3 、TiO 2 , Ga 2 O 3 、MoO 3 As the raw materials corresponding to Ca, Bi, Ti, Ga, and Mo in the chemical formula, La 2 O 3 、Nd 2 O 3 , or Sm 2 O 3 as a raw material corresponding to M in the chemical formula; each raw material is prepared according to the chemical amount in the chemical formula, and then a ball milling treatment is performed using anhydrous ethanol as a ball milling medium, and the obtained material is dried, sieved, pressed and formed, and then placed in a sealed crucible for calcination; then the calcined material is ground and sieved, and a secondary ball milling treatment is performed, and the obtained material is dried, ground and sieved to obtain a pre-synthesized precursor powder;
[0012] (2) Preparation of high temperature piezoelectric ceramic materials
[0013] The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a primary calcination treatment to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace for a secondary calcination treatment to decarbonize, to obtain a decarbonized sintered product; finally, the decarbonized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material.
[0014] Furthermore, the purity of each raw material in step (1) of the preparation method of the present invention is not less than 99.9%. The pressure of the pressing molding is 4-6Mpa; and the calcination treatment is to increase the temperature to 800-850°C at 5°C / min.
[0015] Furthermore, in the step (2) of the preparation method of the present invention, the primary calcination treatment is performed by heating the spark plasma sintering furnace at a pressure of 25 to 30 MPa and a DC pulse current of 500 to 550 A to 800 to 850° C. at 100° C. / min, keeping the temperature for 5 to 8 minutes, stopping the DC pulse current, releasing the pressure, and cooling the furnace to room temperature. The secondary calcination treatment is performed by heating the temperature to 600 to 650° C. at 5° C. / min, keeping the temperature for 3 to 4 hours, and cooling the furnace to room temperature.
[0016] Furthermore, the polarization treatment in step (2) of the preparation method of the present invention is to first polish the surface of the decarbonized sintered product; then perform electrode coating treatment, that is, silver electrodes are applied to the upper and lower surfaces of the decarbonized sintered product after polishing; then calcine at 650-680°C at 5°C / min, keep warm for 40-60min, and cool to room temperature with the furnace; finally, polarize in high-temperature silicone oil at 180-200°C with a DC voltage of 5-10kV / mm for 20-30min.
[0017] The above lanthanide elements are co-doped with Ga and Mo to form CaBi 4 Ti 4 O 15 Products obtained by the preparation method of high-temperature piezoelectric ceramic materials.
[0018] The present invention has the following beneficial effects:
[0019] (1) In the preparation of CaBi 4 Ti 4 O 15 In the process of preparing piezoelectric ceramic materials, due to the volatilization of bismuth at high temperature, bismuth vacancies will inevitably be formed, thereby generating vacancy defects. In view of this phenomenon, the present invention adopts a valence ratio of A-site Ca 2+ Ion high La 3+ 、Nd 3+ , or Sm 3+ Ions are doped and replaced, and the valence ratio of B-site Ti is also used. 4+ Ion high composite ion [Ga 1 / 3 Mo 2 / 3 ] 5+ Doping and substitution are performed to make the A and B positions both defective, making the perovskite layer (A m-1 B m O 3m+1 ) 2- Producing electrons, thereby enhancing the bismuth oxide layer (Bi 2 O 2 ) 2+ and perovskite-like layers (A m-1 B m O 3m+1 ) 2-The interaction between them changes the growth behavior of the grains, and finally the CaBi with excellent performance is obtained. 4 Ti 4 O 15 High temperature piezoelectric ceramic materials.
[0020] (2) The present invention adopts advanced spark plasma sintering technology, which requires low sintering temperature and short sintering time, thus low energy consumption, and high density of the sintered material, which can obtain CaBi with excellent performance. 4 Ti 4 O 15 High temperature piezoelectric ceramic materials.
[0021] (3) The lanthanide elements and Ga, Mo co-doped CaBi 4 Ti 4 O 15 Piezoelectric ceramic material, Curie temperature ≥ 760℃, piezoelectric constant d 33 ≥25pC / N, d after annealing at 600℃ 33 ≥21pC / N; resistivity ≥2.2×10 at 500℃ 7 Ω·cm, dielectric loss ≤0.48%. This material has good high temperature stability and has broad application prospects in high temperature fields.
[0022] (4) The preparation method of the present invention adopts advanced ceramic preparation technology, has low firing temperature, low preparation cost, simple and easy process operation, and easy control of influencing factors. It is suitable for large-scale industrial production and is conducive to promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described in detail below in conjunction with the embodiments and drawings:
[0024] Figure 1 The lanthanide element and Ga, Mo co-doped CaBi prepared in the embodiment of the present invention 4 Ti 4 O 15 XRD patterns of high temperature piezoelectric ceramics and comparative piezoelectric ceramic materials;
[0025] Figure 2 The lanthanide element and Ga, Mo co-doped CaBi prepared in the embodiment of the present invention 4 Ti 4 O 15 The curve of dielectric constant variation with temperature of high temperature piezoelectric ceramics. DETAILED DESCRIPTION
[0026] Embodiment 1:
[0027] This embodiment is a lanthanide element and Ga, Mo co-doped CaBi4 Ti 4 O 15 The preparation method of high temperature piezoelectric ceramic material comprises the following steps:
[0028] (1) Preparation of pre-synthesized precursor powder
[0029] With 99.9% pure CaCO 3 ,La 2 O 3 、Bi 2 O 3 、TiO 2 , Ga 2 O 3 、MoO 3 As with the chemical formula Ca 0.95 La 0.05 Bi 4 Ti 3.935 [Ga 1 / 3 Mo 2 / 3 ] 0.065 O 15 The raw materials corresponding to Ca, La, Bi, Ti, Ga and Mo are prepared according to the chemical quantities in the general chemical formula, and then anhydrous ethanol is used as the ball milling medium, and the ball: material: anhydrous ethanol = 4: 1: 3 is used, and the ball milling treatment is performed once on a planetary ball mill at a speed of 400 r / min for 24 hours. The obtained material is dried, passed through an 80-mesh sieve, pressed and formed at 4 MPa, and then placed in a sealed crucible, and the temperature is increased to 800° C. at 5° C. / min and calcined in an oxidizing atmosphere for 2 hours; the calcined material is ground and passed through an 80-mesh sieve, and a secondary ball milling treatment is performed using the same process as the primary ball milling treatment, and the obtained material is dried, ground and passed through an 80-mesh sieve to obtain a pre-synthesized precursor powder;
[0030] (2) Preparation of high temperature piezoelectric ceramic materials
[0031] (2-1) 0.8 g of the above-mentioned pre-synthesized precursor powder was loaded into a cylindrical graphite mold with a diameter of 20 mm, placed in a spark plasma sintering furnace, set the pressure to 25 MPa, and the DC pulse current to 500 A, and heated to 800 ° C at 100 ° C / min for a calcination treatment. After keeping the temperature for 5 min, the DC pulse current was stopped, and then the pressure was released, and the furnace was cooled to room temperature to obtain a carbon-containing sintered product;
[0032] (2-2) placing the carbon-containing sintered product in a common high-temperature furnace, heating the temperature to 600° C. at 5° C. / min for secondary calcination to decarbonize the product, keeping the temperature for 3 hours, and cooling the product to room temperature to obtain a decarbonized sintered product;
[0033] (2-3) The decarburized sintered product is subjected to the following polarization treatment: first, the surface of the decarburized sintered product is polished; then, electrode coating is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 650°C at 5°C / min, the temperature is kept for 40 minutes, and the product is cooled to room temperature with the furnace; finally, the product is polarized in high-temperature silicone oil at 180°C with a DC voltage of 5 to 10 kV / mm for 20 minutes, thereby obtaining a high-temperature piezoelectric ceramic material.
[0034] Embodiment 2:
[0035] This embodiment is a lanthanide element and Ga, Mo co-doped CaBi 4 Ti 4 O 15 The method for preparing high temperature piezoelectric ceramic material is different from that of the first embodiment in that:
[0036] 1. The general chemical formula of this embodiment is Ca 0.94 Nd 0.06 Bi 4 Ti 3.935 [Ga 1 / 3 Mo 2 / 3 ] 0.065 O 15 , the raw material corresponding to Nd is Nd 2 O 3 .
[0037] 2. The calcination temperature in step (1) is 830°C; the calcination temperature in step (2-1) is 830°C.
[0038] Embodiment three:
[0039] This embodiment is a lanthanide element and Ga, Mo co-doped CaBi 4 Ti 4 O 15 The method for preparing high temperature piezoelectric ceramic material is different from that of the first embodiment in that:
[0040] 1. The general chemical formula of this embodiment is Ca 0.93 Sm 0.07 Bi 4 Ti 3.935 [Ga 1 / 3 Mo 2 / 3 ] 0.065 O 15 , the raw material corresponding to Sm is Sm 2 O 3 .
[0041] 2. The calcination temperature in step (1) is 820°C; the calcination temperature in step (2-1) is 820°C.
[0042] Comparative Example:
[0043] Undoped, chemically CaBi 4 Ti 4 O 15 A high temperature piezoelectric ceramic material is used as a comparative example, and its preparation steps are the same as those in Example 1.
[0044] The XRD crystal phase spectra of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are as follows: Figure 1 As shown, from Figure 1 It can be seen that the diffraction peaks of the piezoelectric ceramic materials obtained in the embodiments and comparative examples are completely consistent with the standard spectrum PDF 00-052-1640, indicating that the obtained materials are CaBi with a single crystal phase. 4 Ti 4 O 15 Material.
[0045] Lanthanide elements and Ga, Mo co-doped CaBi prepared in the embodiment of the present invention 4 Ti 4 O 15 The dielectric constant of high temperature piezoelectric ceramics varies with temperature. Figure 2 The performance test results of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are shown in Table 1.
[0046] Table 1 Performance of ceramic materials of the embodiments of the present invention and comparative examples
[0047]
Claims
1. A lanthanide element co-doped with Ga and Mo CaBi4Ti4O 15 A method for preparing a high temperature piezoelectric ceramic material, characterized in that: The chemical formula of the piezoelectric ceramic material is Ca 1-x M x Bi4Ti 4-y [Ga 1 / 3 Mo 2 / 3 ] y O 15 , where 0.03≤x≤0.08, 0.05≤y≤0.075, M is La 3+ 、Nd 3+ , or Sm 3+ ions, doped with +3-valent lanthanide metal ions M with 12 coordination to replace CaBi4Ti4O 15 Ca in the A position 2+ ions, with complex high-valent ions [Ga 1 / 3 Mo 2 / 3 ] 5+ Doped substituted CaBi4Ti4O 15 Ti in the middle B position 4+ ions are formed; The preparation method comprises the following steps: (1) Preparation of pre-synthesized precursor powder CaCO3, Bi2O3, TiO2, Ga2O3, and MoO3 are used as raw materials corresponding to Ca, Bi, Ti, Ga, and Mo in the chemical formula, and La2O3, Nd2O3, or Sm2O3 is used as the raw material corresponding to M in the chemical formula; each raw material is prepared according to the stoichiometric amount in the chemical formula, and then a ball milling treatment is performed using anhydrous ethanol as a ball milling medium, and the obtained material is dried, sieved, pressed and formed at a pressure of 4 to 6 MPa, and then placed in a sealed crucible, and the temperature is increased to 800 to 850° C. at a rate of 5° C. / min for calcination; the calcined material is then ground and sieved, and a second ball milling treatment is performed, and the obtained material is dried, ground, and sieved to obtain a pre-synthesized precursor powder; (2) Preparation of high temperature piezoelectric ceramic materials The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a calcination treatment, that is, the spark plasma sintering furnace pressure is 25-30 MPa, the DC pulse current is 500-550 A, the temperature is raised to 800-850°C at 100°C / min, and after keeping warm for 5-8 min, the DC pulse current is stopped, and then the pressure is released, and the furnace is cooled to room temperature to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace for a secondary calcination treatment for decarburization, that is, the temperature is raised to 600-650°C at 5°C / min, and the temperature is kept for 3-4 h, and the furnace is cooled to room temperature to obtain a decarburized sintered product; finally, the decarburized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material; the piezoelectric ceramic material corresponds to the A and B positions are replaced by high-priced doping to form A and B position defects, so that the perovskite layer (A m-1 B m O 3m+1 ) 2- Generate electrons to enhance the bismuth oxide layer (Bi2O2) 2+ and perovskite-like layers (A m-1 B m O 3m+1 ) 2- The interaction between them changes the growth behavior of the grains.
2. The lanthanide element co-doped with Ga and Mo according to claim 1 CaBi4Ti4O 15 A method for preparing a high temperature piezoelectric ceramic material, characterized in that: The purity of each raw material in step (1) is not less than 99.9%.
3. The lanthanide element co-doped with Ga and Mo according to claim 1 CaBi4Ti4O 15 A method for preparing a high temperature piezoelectric ceramic material, characterized in that: The polarization treatment in step (2) is as follows: first, the surface of the decarburized sintered product is polished; then, an electrode coating treatment is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 650-680°C at 5°C / min for calcination, the temperature is kept at that temperature for 40-60 min, and the product is cooled to room temperature with the furnace; finally, the product is polarized in high-temperature silicone oil at 180-200°C with a DC voltage of 5-10 kV / mm for a polarization time of 20-30 min.
4. A lanthanide element co-doped with Ga and Mo as described in any one of claims 1 to 3 in the form of CaBi4Ti4O 15 The product obtained by the method for preparing high temperature piezoelectric ceramic material is characterized by: The piezoelectric ceramic material d 33 ≥25 pC / N, T C ≥760℃; Resistivity at 500℃( ρ )≥2.2×10 7 Ω·cm, dielectric loss (tan δ )≤0.48%; after annealing at 600℃ d 33 ≥21 pC / N.
Citation Information
Patent Citations
DEVELOPMENT OF A FERROELECTRIC CERAMICS DIELECTRIC RESONATOR BY THE CERAMIC PROCESS BASED ON CABI4TI4O15 WITH ADDITION OF V2O5 (VANADIUM PENTOXIDE) FOR USE IN MICROWAVES AND RESULTING PRODUCT
BR102017003436A2
Nb-position Cr / Mo codoped bismuth-calcium niobate high-temperature piezoelectric ceramic material and preparation method therefor
CN109704761A
Bismuth layered structure calcium bismuth titanate high-temperature piezoelectric ceramic material and preparation method thereof
CN111362691A
Piezoelectric material with high piezoelectricity and good high-temperature insulativity and preparation method thereof
CN113896526A
Preparation method of CaBi4Ti4O15 ceramic with high piezoelectric property
CN113929450A