Curved ceramic plate and its ceramic hot bending process
By using vegan ceramic tiles for low-temperature hot bending and adjusting the silicon-aluminum content in the glaze formula, the problems of cracking and poor decorative effects of glaze layer in the existing technology are solved, and the problem of poor decorative effects in the existing technology is achieved. The stable production and high-end decorative effect of curved ceramic plates.
Patent Information
- Application Number
- CN202311143948.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-09-05
AI Technical Summary
The existing ceramic thermal bending technology has glaze cracking, matte recrystallization and glaze devitrification, resulting in poor decorative effect of curved ceramic plates and lengthy production process, making it difficult to meet high-end customization needs.
Plain firing porcelain tiles are used for surface decoration and then heat-bending at low temperature. By adjusting the silicon-aluminum content in the glaze formula, an adjustable base glaze and transparent protective glaze formula are designed to achieve crack-free and discolored glaze surface. High definition decorative effect.
The stable and large-scale mass production of curved ceramic plates has been achieved, avoiding the problems of deterioration in the glaze layer texture, gloss deviation and pattern color change, and improving the decorative effect and production control of the product.
Smart Images

Figure CN117185661B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramics, and in particular relates to a curved ceramic plate and a ceramic hot bending process thereof. Background Art
[0002] In order to cater to consumers' aesthetic requirements for buildings, in recent years, various manufacturers have unanimously set their sights on the aesthetic appearance of their products, using various curved materials such as natural stone or artificial stone, acrylic panels, hot-bent glass, etc. for decoration. The number of curved parts of buildings, such as round domes, circular cylinders, curved walls, curved handrails, spiral staircases, etc., is increasing, and the usage is large.
[0003] The curved surface products made of natural stone have a large processing volume and low stone utilization rate, resulting in high production costs of natural stone curved surface products, unstable colors, obvious color differences, relatively simple patterns, and complex construction processes. Even marble with strong processability has disadvantages such as poor physical and chemical properties, low hardness, easy weathering, and poor weather resistance. The polished surface is prone to lose its luster and color change over the years, and the decorative effect is difficult to last. Although organic building materials such as acrylic PMMA, Chevron board, and ABS decorative board can be easily made into curved surface finishing materials, the weather resistance of organic materials is poor. Poor, easy to age, easy to deform, and difficult to meet the use requirements of buildings; hot-bent glass is widely used in construction and civil occasions, such as skylights, sightseeing elevators, arched corridors, glass washbasins, glass counters, glass decorations, etc., but its material characteristics determine that it can only be used in specific designs and special decorative effects. Microcrystalline glass and glass ceramics have good thermal bending properties and can be used to cover round columns. They have a jade-like texture and are of high grade, but the current decorative means and methods of their later processing have a single effect and it is difficult to show the delicate and rich stone texture.
[0004] There are many problems with the above-mentioned curved materials. With the extensive promotion and application of ceramic rock slabs in the field of modern architectural decoration, as the new favorite of the architectural ceramics industry, the demand for processing ceramic rock slabs into various arc curved panels is increasing. At present, the industry basically chooses finished bricks fired once for bending and re-firing. After the finished bricks are hot-bent and calcined, the surface glaze forms tiny gaps due to cracking, which makes the surface stain resistance drop sharply. In addition, the inkjet pattern on the surface of the hot-bent board will cause the pattern texture to become unclear and the color to become dim after the second calcination. Compared with ordinary glazed tiles, its decorative effect is poor. The single texture can be used for complex pattern design, but it cannot present the curved surface decoration effect with more complex texture and darker color. In addition, although the substrate used for the curved rock slab is a finished rock slab with a glossiness of more than 50°, the surface glaze of the surface is hot-bent and calcined, and the surface texture of the glaze layer deteriorates and the glossiness decreases sharply, which cannot really meet the decorative requirements of the curved rock slab. At the same time, after bending, the product glaze cracks more, the production quality rate is low, and the rational use of resources cannot be achieved. To this end, some ceramic companies have solved this problem by adjusting the process. For example, CN113979738A discloses a high-curvature wide-color gamut ceramic curved rock plate and its preparation method and application. The technical solution is that the thickness of the curved rock plate is 3-6 mm, the radius of curvature is ≥100 mm, the center angle of the arc is 0-180°C, the curved rock plate includes a glaze layer, the glaze layer includes a bottom glaze layer and a surface glaze layer arranged on the top of the bottom glaze layer. The raw materials of the bottom glaze layer include: EN-1 frit 81~ 90 parts, kaolin 8-12 parts, quartz 2-7 parts, sodium tripolyphosphate 0.3-0.5 parts, sodium carboxymethyl cellulose 0.15-0.22 parts; the raw materials for the glaze layer include: 7# transparent frit 30-45 parts, kaolin 8 parts, quartz 0-7 parts, albite 0-40 parts, potassium feldspar 0-15 parts, dolomite 0-5 parts, calcite 0-5 parts, barium carbonate 0-6 parts, sodium tripolyphosphate 0.3-0.5 parts, sodium carboxymethyl cellulose 0.15-0.22 parts. This process can prevent the bottom glaze cracks of the curved rock plate after hot bending and re-firing, avoid the occurrence of matte recrystallization and glaze devitrification, and broaden the color gamut. However, its disadvantage is that the finished bricks are bent and re-fired, and the products with different gloss and texture effects need to be prepared on different production process platforms before hot bending and firing. The process is lengthy, and the glaze surface of the finished bricks still has more or less color changes and poor texture after the second calcination, which restricts its promotion and application. Therefore, the existing ceramic hot bending technology needs to be improved and developed. Summary of the invention
[0005] In view of the deficiencies in the above-mentioned prior art, the object of the present invention is to provide a curved ceramic plate and its ceramic hot bending process which are produced by using unglazed ceramic tiles for surface decoration and then hot-bending and firing at low temperature, and can adapt to different product needs by adjusting the silicon and aluminum content of the glaze formula, so as to achieve the curved ceramic plate with no glaze cracks, no discoloration, high-definition decoration and stable production.
[0006] The technical solution of the present invention is the curved ceramic plate, which is special in that the base glaze formula of the curved ceramic plate is composed of the following raw material components by weight: 25-60 parts of frit A, 10-70 parts of frit B, 10-15 parts of zirconium silicate, 5-15 parts of kaolin, 10-20 parts of fixing agent, 0.2-0.4 parts of methyl, and 0.4-0.6 parts of sodium tripolyphosphate;
[0007] The base glaze formula consists of the following chemical components by weight: SiO2 45-54wt%, Al2O3 10.5-13wt%, Fe2O3≤0.20wt%, K2O 3-7wt%, Na2O 1-3wt%, CaO 7-10wt%, MgO 0.1-1wt%, ZnO 7-12wt%, ZrO2 6-10wt%, B2O3 0.5-2wt%, BaO 2.5-6wt%, and ignition loss 0.5-2wt%.
[0008] Preferably, the frit A is composed of the following raw material components by weight: 10-15 parts of zinc oxide, 7-12 parts of barium carbonate, 10-15 parts of aluminum oxide, 30-45 parts of quartz, 15-25 parts of wollastonite, 1-3 parts of magnesium oxide, 1-3 parts of boron oxide, 3-8 parts of sodium carbonate, and 3-8 parts of potassium carbonate;
[0009] The frit A is composed of the following chemical components by weight: SiO2 45-55wt%, Al2O3 10-15wt%, Fe2O3≤0.3wt%, K2O 1-3wt%, Na2O 1-3wt%, CaO 5-10wt%, MgO 1-3wt%, ZnO 10-15wt%, B2O3 1-3wt%, BaO 7-12wt%, and loss on ignition 0.01-0.1wt%.
[0010] Preferably, the frit B is composed of the following raw material components by weight: 10-15 parts of zinc oxide, 0.5-2 parts of barium carbonate, 5-10 parts of aluminum oxide, 30-50 parts of quartz, 25-30 parts of wollastonite, 1-3 parts of boron oxide, 3-8 parts of sodium carbonate, and 8-13 parts of potassium carbonate;
[0011] The frit B is composed of the following chemical components by weight: SiO2 55-65wt%, Al2O3 5-10wt%, Fe2O3≤0.3wt%, K2O 3-8wt%, Na2O 1-3wt%, CaO 8-13wt%, MgO 0.1-0.5wt%, ZnO10-15wt%, B2O3 1-3wt%, BaO 0.5-2wt%, and ignition loss 0.01-0.1wt%.
[0012] Preferably, the frit A and frit B are obtained by uniformly mixing raw materials according to respective formula ratios, calcining and melting them at a temperature of 1400-1600°C to form a melt, and then adding them into water for rapid cooling to obtain a block glass frit. The block glass frit is crushed and sieved for use, and the crushing and sieve mesh size is controlled to be 80-120 mesh.
[0013] Preferably, the fixing agent is composed of one or a combination of water bubbles, a suspending agent, and super-plastic ball clay, wherein the water bubbles are formed by mixing and grinding sodium carboxymethyl cellulose and water in a ratio of 15:85; the suspending agent is composed of the following raw materials in parts by weight: 20 parts of methyl glycol, 20 parts of sodium carboxymethyl cellulose, 20 parts of polymethylsiloxane, 1 part of sodium metaphosphate, 0.4 parts of sodium dodecylbenzene sulfonate, and 0.6 parts of dodecyltrimethylammonium bromide; and 38 parts of deionized water.
[0014] Another technical solution of the present invention is the curved ceramic plate, which is special in that the transparent glaze protective glaze formula of the curved ceramic plate is composed of the following raw material components by weight: 10 to 90 parts of bright transparent frit, 5 to 80 parts of matte transparent frit, 4 to 10 parts of kaolin, 0.2 to 0.4 parts of methyl, and 0.3 to 0.5 parts of sodium tripolyphosphate;
[0015] The transparent protective glaze formula consists of the following chemical components by weight: SiO2 42-50wt%, Al2O3 3-16wt%, Fe2O3 0.1-0.5wt%, K2O 0.1-1.0wt%, Na2O 0-10wt%, CaO 0.8-5wt%, MgO0.1-2wt%, ZnO 0.5-6wt%, B2O3 12-25wt%, BaO 1-10wt%, SrO 0-2wt%, and ignition loss 0.5-1.0wt%.
[0016] Preferably, the bright transparent frit is composed of the following raw material components by weight: 3-8 parts of zinc oxide, 8-13 parts of barium carbonate, 2-5 parts of aluminum oxide, 30-50 parts of quartz, 2-5 parts of wollastonite, 20-25 parts of boron oxide, 20-30 parts of sodium carbonate, and 1-3 parts of potassium carbonate;
[0017] The bright transparent frit is composed of the following chemical components by weight: SiO2 40-50wt%, Al2O3 2-5wt%, Fe2O3≤0.3wt%, K2O 0.5-2wt%, Na2O 7-12wt%, CaO1-3wt%, ZnO 3-6wt%, B2O3 20-25wt%, BaO 8-13wt%, and ignition loss 0.01-0.1wt%.
[0018] Preferably, the matte transparent frit is composed of the following raw material components by weight: 13-18 parts of aluminum oxide, 25-45 parts of quartz, 5-10 parts of wollastonite, 20-25 parts of boron oxide, 1-3 parts of magnesium oxide, 8-13 parts of sodium carbonate, 0.5-1 part of potassium carbonate, and 3-8 parts of strontium carbonate;
[0019] The matte transparent frit consists of the following chemical components by weight: SiO2 45-55wt%, Al2O3 13-18wt%, Fe2O3≤0.3wt%, K2O 0.1-0.5wt%, Na2O 3-6wt%, CaO 2-5wt%, MgO 1-3wt%, B2O3 20-25wt%, SrO 2-5wt%, and ignition loss 0.01-0.1wt%.
[0020] Preferably, the bright transparent frit and the matte transparent frit are obtained by uniformly mixing raw materials according to respective formula ratios, calcining and melting at a temperature of 1300-1500°C to form a melt, and then adding the melt into water for rapid cooling to obtain a block glass frit. The block glass frit is crushed and sieved for use, and the crushing and sieving mesh size is controlled to be 80-120 meshes.
[0021] Another technical solution of the present invention is the ceramic hot bending process of the curved ceramic plate, which is special in that it includes the following steps:
[0022] ⑴ Preparation of powder: ball milling according to the proportion of raw materials in the formula, and spray powdering to obtain green body powder and store it for aging;
[0023] (2) Pressing and forming, feeding the obtained powder into a press for pressing to obtain a ceramic green body, the green body thickness is controlled to be 6-10 mm, the width is controlled to be 600-1750 mm, and the length is controlled to be 1200-3500 mm;
[0024] ⑶ Drying of green body: sending the formed ceramic green body into roller kiln for drying;
[0025] (4) Primary bisque firing: the dried body is sent to a roller kiln for firing at a temperature of 1100-1200°C. The strength of the bisque-fired porcelain body is controlled to be 45-55 MPa.
[0026] ⑸ Dust removal and heating: the surface of the unglazed porcelain tile blank is dusted and sent to the infrared drying kiln for heating to obtain an unglazed porcelain blank with a certain temperature. After heating, the temperature of the unglazed porcelain blank is controlled to be 65-150°C, and the heating time is 6-9 minutes;
[0027] ⑹ Base glaze spraying: the heated unglazed porcelain body is decorated with base glaze under high pressure spraying. The base glaze spraying pressure is 6-15 bar, the base glaze specific gravity is 1.50±0.02, and the glaze application amount is 300-400g / m2 , the average particle size D50 of the base glaze slurry is controlled to be 6-8μm, and the glossiness of the base glaze is controlled to be 6-10°;
[0028] ⑺ Glaze drying: the bricks after base glaze application are dried by infrared rays at a temperature of 120-240°C and a drying time of 3-5 minutes;
[0029] ⑻ Pattern decoration: pattern decoration according to product effect requirements;
[0030] ⑼ Heating the bricks: heating the bricks decorated with patterns, using electric infrared heating or flame burning heating, with a heating temperature of 150-300°C and a heating time of 8-15 minutes. The temperature of the bricks after heating is controlled at 70-120°C to ensure that the decorative patterns are completely dry;
[0031] ⑽ Apply protective glaze: spray the heated bricks with transparent protective glaze at high pressure. The spraying pressure of the transparent protective glaze is 8-15 bar, the specific gravity of the transparent protective glaze is 1.30-1.60, and the glaze amount is 120-400g / m 2 , the average particle size D50 of the transparent protective glaze is controlled to be 6-8 μm, and the glossiness of the transparent protective glaze is controlled to be 10-95°;
[0032] ⑾ Hot bending and firing: the ceramic tile blanks with transparent protective glaze are sent into a shuttle kiln for firing. The hot bending temperature is controlled at 900-950°C and the firing time is 350-500 minutes to obtain a semi-finished curved ceramic plate. The semi-finished curved ceramic plate is polished or not polished and edged to finally obtain a finished curved ceramic plate.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] ⑴ The present invention proposes a curved ceramic plate and a ceramic hot bending process thereof, in which the surface of the ceramic blank after primary bisque firing is decorated and then hot bent and fired at low temperature. At the same time, by designing a base glaze and a transparent protective glaze formula with an adjustable SiO2 / Al2O3 molar ratio, the ratio of the base glaze and the transparent protective glaze can be adjusted according to the situation to meet the needs of products with different glaze textures and gloss. Compared with the industry's use of finished bricks for hot processing and bending forming, the process operation is highly controllable, and the risks of texture deterioration, gloss deviation and pattern color shift caused by devitrification of the glaze layer during secondary firing of the finished bricks are effectively avoided, thereby realizing stable large-scale mass production of curved ceramic plates.
[0035] (2) The present invention solves the problem that the glaze is difficult to adhere to and easy to fall off due to the poor adsorption of the once-fired porcelain brick blank by introducing a fixing agent into the glaze formula, effectively enhances the adhesion of the glaze, improves the smoothness of the glaze spraying, and thus improves the glaze decoration quality of the product.
[0036] ⑶ The present invention adjusts the glaze structure, calcines the ceramic raw material at high temperature into a molten block and then applies it to the glaze, so that the viscosity and surface tension of the glaze are reduced during hot bending and re-firing, thereby improving the exhaust capacity of the glaze layer, thereby effectively avoiding the occurrence of defects such as pinholes and bubbles on the glaze of curved ceramic tiles during the hot bending and firing process. While reducing the firing temperature of the product, it broadens the firing range and color gamut, enriches the product decorative effect, and makes personalized high-end customized paving of curved ceramic panels possible in terminal design. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic diagram of the process of preparing the curved ceramic plate of the present invention;
[0038] Figure 2A , Figure 2B This is a rendering of the curved ceramic plate of the present invention. DETAILED DESCRIPTION
[0039] The present invention will be further described in detail below in conjunction with embodiments:
[0040] Example 1
[0041] See also Figure 1 As shown, the curved ceramic plate is composed of a base glaze and a transparent glaze protective glaze constituting a composite layer. The ceramic hot bending process of the curved ceramic plate includes the following steps:
[0042] ⑴ Preparation of powder: ball milling according to the proportion of raw materials in the formula, and spray powdering to obtain green body powder and store it for aging;
[0043] (2) Pressing and forming, feeding the obtained powder into a press for pressing to obtain a ceramic green body with a green body thickness of 6.5 mm, a width of 1271 mm, and a length of 2754 mm;
[0044] ⑶ Drying of green body: sending the formed ceramic green body into roller kiln for drying;
[0045] (4) Primary bisque firing: the dried body is sent to a roller kiln for firing at a temperature of 1150°C. The strength of the bisque fired porcelain body is 51Mpa.
[0046] ⑸ Dust removal and heating: the surface of the unglazed porcelain tile blank is dusted and sent to an infrared drying kiln for heating to obtain an unglazed porcelain blank with a certain temperature. The temperature of the unglazed porcelain blank after heating is 150°C and the heating time is 6 minutes;
[0047] ⑹ Base glaze spraying: the heated unglazed porcelain body is decorated with base glaze high pressure spraying. The base glaze spraying pressure is 10 bar, the base glaze specific gravity is 1.50, and the glaze amount is 350g / m 2 , the average particle size D50 of the base glaze slurry is controlled to be 6.7μm, and the glossiness of the base glaze is 8°;
[0048] The base glaze formula is composed of the following raw material components by weight: 51 parts of frit A, 29 parts of frit B, 11 parts of zirconium silicate, 9 parts of kaolin, 10 parts of fixing agent, 0.25 parts of methyl, and 0.5 parts of sodium tripolyphosphate;
[0049] The base glaze formula is composed of the following chemical components by weight: SiO2: 51.94wt%, Al2O3: 11.81wt%, Fe2O3: 0.17wt%, K2O: 3.19wt%, Na2O: 1.29wt%, CaO: 7.86wt%, MgO: 0.76wt%, ZnO: 9.05wt%, ZrO2: 7.04wt%, B2O3: 1.18wt%, BaO: 4.68wt%, loss on ignition: 1.03wt%;
[0050] The frit A is composed of the following raw material components by weight: 11 parts of zinc oxide, 11 parts of barium carbonate, 13 parts of aluminum oxide, 31 parts of quartz, 23 parts of wollastonite, 1.5 parts of magnesium oxide, 1.5 parts of boron oxide, 3.5 parts of sodium carbonate, and 4.5 parts of potassium carbonate;
[0051] The frit A consists of the following chemical components by weight: SiO2 49.83wt%, Al2O3 13.15wt%, Fe2O3 0.19wt%, K2O 2.89wt%, Na2O 1.80wt%, CaO 9.13wt%, MgO 1.34wt%, ZnO 11.38wt%, B2O3 1.60wt%, BaO 8.64wt%, and loss on ignition 0.05wt%.
[0052] The frit B is composed of the following raw material components by weight: 11 parts of zinc oxide, 1 part of barium carbonate, 7 parts of aluminum oxide, 39 parts of quartz, 28 parts of wollastonite, 1.5 parts of boron oxide, 2.5 parts of sodium carbonate, and 10 parts of potassium carbonate;
[0053] The frit B is composed of the following chemical components by weight: SiO2 61.21wt%, Al2O3 7.05wt%, Fe2O3 0.14wt%, K2O 5.63wt%, Na2O 1.25wt%, CaO 11.03wt%, MgO 0.25wt%, ZnO 11.20wt%, B2O3 1.24wt%, BaO 0.95wt%, and ignition loss 0.05wt%;
[0054] The frit A and frit B are prepared by mixing raw materials according to a formula ratio, calcining and melting them at 1600°C to form a melt, and then adding them into water for rapid cooling to obtain a block of glassy frit, which is crushed and sieved for use, and the crushing and sieve mesh is controlled to be 120 mesh;
[0055] The fixing agent is a water bubble, which is prepared by mixing and grinding sodium carboxymethyl cellulose and water in a ratio of 15:85;
[0056] ⑺ Glaze drying: the bricks after the base glaze is dried by infrared, the drying temperature is 150℃, and the drying time is 4min;
[0057] ⑻ Pattern decoration: pattern decoration according to product effect requirements;
[0058] ⑼ Brick heating: The bricks with pattern decoration are subjected to electric infrared heating at a temperature of 200°C for 10 minutes. The temperature of the bricks after heating is 90°C to ensure that the decorative pattern is completely dry;
[0059] ⑽Apply protective glaze: spray the heated brick with transparent protective glaze at high pressure. The spraying pressure of transparent protective glaze is 10 bar, the specific gravity of transparent protective glaze is 1.50, and the glaze amount is 150g / m 2 , the average particle size D50 of the transparent protective glaze is controlled to be 7.2μm, and the glossiness of the transparent protective glaze is controlled to be 90°;
[0060] The transparent protective glaze formula is composed of the following raw material components by weight: 85 parts of glossy transparent frit, 10 parts of matte transparent frit, 5 parts of kaolin, 0.25 parts of methyl, and 0.5 parts of sodium tripolyphosphate;
[0061] The transparent protective glaze formula consists of the following chemical components by weight: SiO2 47.61wt%, Al2O3 5.62wt%, Fe2O3 0.13wt%, K2O 0.86wt%, Na2O 8.20wt%, CaO 1.77wt%, MgO 0.23wt%, ZnO 3.72wt%, B2O3 22.99wt%, BaO 8.03wt%, SrO 0.25wt%, and ignition loss 0.59wt%;
[0062] The bright transparent frit is composed of the following raw material components by weight: 4 parts of zinc oxide, 12 parts of barium carbonate, 2.5 parts of aluminum oxide, 29 parts of quartz, 4 parts of wollastonite, 24 parts of boron oxide, 23 parts of sodium carbonate, and 1.5 parts of potassium carbonate;
[0063] The bright transparent frit is composed of the following chemical components by weight: SiO2 47.01wt%, Al2O3 2.75wt%, Fe2O3 0.16wt%, K2O 0.98wt%, Na2O 9.14wt%, CaO 1.65wt%, MgO 0.10wt%, ZnO 4.38wt%, B2O3 24.35wt%, BaO 9.45wt%, and ignition loss 0.03wt%;
[0064] The matte transparent frit formula is composed of the following raw material components by weight: 15 parts of aluminum oxide, 40 parts of quartz, 8 parts of wollastonite, 22 parts of boron oxide, 1.5 parts of magnesium oxide, 9 parts of sodium carbonate, 0.5 parts of potassium carbonate, and 4 parts of strontium carbonate;
[0065] The matte transparent frit is composed of the following chemical components by weight: SiO2 48.92wt%, Al2O3 15.80wt%, Fe2O3 0.08wt%, K2O 0.28wt%, Na2O 4.33wt%, CaO 3.67wt%, MgO 1.43wt%, B2O3 22.96wt%, SrO 2.48wt%, and ignition loss 0.05wt%;
[0066] The bright transparent frit and the matte transparent frit are obtained by mixing raw materials according to the formula ratio, calcining and melting at 1500°C to form a melt, and then adding it into water for rapid cooling to obtain a block glass frit. The block glass frit is crushed and sieved for standby use, and the crushing and screening mesh is controlled to be 90 meshes;
[0067] ⑾ Hot bending and firing: the ceramic tile blanks with transparent protective glaze are sent into a shuttle kiln for firing. The hot bending temperature is controlled at 950°C and the firing time is 380 minutes to obtain a semi-finished curved ceramic plate. The semi-finished curved ceramic plate is polished and edge-ground to finally obtain a finished curved ceramic plate (see Figure 2).
[0068] Example 2
[0069] See also Figure 1 As shown, the curved ceramic plate is composed of a base glaze and a transparent glaze protective glaze constituting a composite layer. The ceramic hot bending process of the curved ceramic plate includes the following steps:
[0070] ⑴ Preparation of powder: ball milling according to the proportion of raw materials in the formula, and spray powdering to obtain green body powder and store it for aging;
[0071] (2) Pressing and forming, feeding the obtained powder into a press for pressing to obtain a ceramic green body with a green body thickness of 9.7 mm, a width of 1720 mm, and a length of 3390 mm;
[0072] ⑶ Drying of green body: sending the formed ceramic green body into roller kiln for drying;
[0073] (4) Primary biscuit firing: the dried body is sent to a roller kiln for firing at a temperature of 1200°C. The biscuit strength is 55 MPa.
[0074] ⑸ Dust removal and heating: the surface of the unglazed porcelain tile blank is dusted and sent to an infrared drying kiln for heating to obtain an unglazed porcelain blank with a certain temperature. The temperature of the unglazed porcelain blank after heating is 110°C and the heating time is 7 minutes;
[0075] ⑹ Base glaze spraying: the heated unglazed porcelain body is decorated with base glaze high pressure spraying. The base glaze spraying pressure is 12 bar, the base glaze specific gravity is 1.50, and the glaze amount is 360g / m 2 , the average particle size D50 of the base glaze slurry is controlled to be 6.7μm, and the glossiness of the base glaze is 6°;
[0076] The base glaze formula is composed of the following raw material components by weight: 25 parts of frit A, 57 parts of frit B, 12 parts of zirconium silicate, 6 parts of kaolin, 15 parts of fixing agent, 0.25 parts of methyl, and 0.5 parts of sodium tripolyphosphate;
[0077] The base glaze formula is composed of the following chemical components by weight: SiO2 53.93wt%, Al2O3 10.55wt%, Fe2O3 0.13wt%, K2O 3.93wt%, Na2O 1.16wt%, CaO 8.57wt%, MgO 0.48wt%, ZnO 9.23wt%, ZrO2 7.61wt%, B2O3 1.11wt%, BaO 2.70wt%, and ignition loss 0.60wt%;
[0078] The frit A is composed of the following raw material components by weight: 12 parts of zinc oxide, 11 parts of barium carbonate, 11 parts of aluminum oxide, 31 parts of quartz, 24 parts of wollastonite, 1.5 parts of magnesium oxide, 1.5 parts of boron oxide, 3.5 parts of sodium carbonate, and 4.5 parts of potassium carbonate;
[0079] The frit A consists of the following chemical components by weight: SiO2 49.83wt%, Al2O3 13.15wt%, Fe2O3 0.19wt%, K2O 2.89wt%, Na2O 1.80wt%, CaO 9.13wt%, MgO 1.34wt%, ZnO11.38wt%, B2O3 1.60wt%, BaO 8.64wt%, and loss on ignition 0.05wt%.
[0080] The frit B is composed of the following raw material components by weight: 11 parts of zinc oxide, 1 part of barium carbonate, 7 parts of aluminum oxide, 39 parts of quartz, 28 parts of wollastonite, 1.5 parts of boron oxide, 2.5 parts of sodium carbonate, and 10 parts of potassium carbonate;
[0081] The frit B described in this embodiment is composed of the following chemical components by weight: SiO2 61.21wt%, Al2O37.05wt%, Fe2O3 0.14wt%, K2O 5.63wt%, Na2O 1.25wt%, CaO11.03wt%, MgO 0.25wt%, ZnO 11.20wt%, B2O3 1.24wt%, BaO 0.95wt%, and ignition loss 0.05wt%;
[0082] The frit A and frit B are prepared by mixing raw materials in a formula ratio, calcining and melting them at 1600° C. to form a melt, and then adding them into water for rapid cooling to obtain a block glass frit. The block glass frit is crushed and sieved for standby use, and the crushing and sieve mesh size is controlled to be 120 meshes.
[0083] The fixing agent is composed of water bubbles, a suspending agent, and super-plastic ball clay, wherein the water bubbles are prepared by mixing and grinding sodium carboxymethyl cellulose and water in a ratio of 15:85; the suspending agent is composed of the following raw materials by weight: 20 parts of methyl glycol, 20 parts of sodium carboxymethyl cellulose, 20 parts of polymethylsiloxane, 1 part of sodium metaphosphate, 0.4 parts of sodium dodecylbenzene sulfonate, and 0.6 parts of dodecyltrimethylammonium bromide; and 38 parts of deionized water;
[0084] ⑺ Glaze drying: the bricks after base glaze application are infrared dried at a temperature of 200°C for 4 minutes;
[0085] ⑻ Pattern decoration: pattern decoration according to product effect requirements;
[0086] ⑼ Heating the bricks: subject the bricks decorated with patterns to flame burning heating treatment at a temperature of 280°C for 8 minutes. The temperature of the bricks after heating is 95°C to ensure that the decorative patterns are completely dry;
[0087] ⑽Apply protective glaze: spray the heated brick with transparent protective glaze at high pressure. The spraying pressure of transparent protective glaze is 12 bar, the specific gravity of transparent protective glaze is 1.30, and the glaze amount is 210g / m 2 , the average particle size D50 of the transparent protective glaze is controlled to 7.2μm, and the glossiness of the transparent protective glaze is controlled to 10°;
[0088] The transparent protective glaze formula is composed of the following raw material components by weight: 20 parts of bright transparent frit, 75 parts of matte transparent frit, 5 parts of kaolin, 0.25 parts of methyl, and 0.5 parts of sodium tripolyphosphate;
[0089] The transparent protective glaze is composed of the following chemical components by weight: SiO2 48.83wt%, Al2O3 14.10wt%, Fe2O3 0.11wt%, K2O 0.41wt%, Na2O 5.08wt%, CaO 3.11wt%, MgO1.06wt%, ZnO 0.88wt%, B2O3 22.09wt%, BaO 1.89wt%, SrO 1.86wt%, and ignition loss 0.58wt%;
[0090] The bright transparent frit is composed of the following raw material components by weight: 4 parts of zinc oxide, 12 parts of barium carbonate, 2.5 parts of aluminum oxide, 29 parts of quartz, 4 parts of wollastonite, 24 parts of boron oxide, 23 parts of sodium carbonate, and 1.5 parts of potassium carbonate.
[0091] The bright transparent frit consists of the following chemical components by weight: SiO2 7.01wt%, Al2O3 2.75wt%, Fe2O3 0.16wt%, K2O 0.98wt%, Na2O 9.14wt%, CaO 1.65wt%, MgO 0.10wt%, ZnO 4.38wt%, B2O3 24.35wt%, BaO 9.45wt%, and ignition loss 0.03wt%.
[0092] The matte transparent frit formula consists of the following raw material components by weight: 15 parts of aluminum oxide, 40 parts of quartz, 8 parts of wollastonite, 22 parts of boron oxide, 1.5 parts of magnesium oxide, 9 parts of sodium carbonate, 0.5 parts of potassium carbonate, and 4 parts of strontium carbonate.
[0093] The matte transparent frit is composed of the following chemical components by weight: SiO2 48.92wt%, Al2O3 15.80wt%, Fe2O3 0.08wt%, K2O 0.28wt%, Na2O 4.33wt%, CaO 3.67wt%, MgO 1.43wt%, B2O3 22.96wt%, SrO 2.48wt%, and loss on ignition 0.05wt%.
[0094] The bright transparent frit and the matte transparent frit are obtained by mixing raw materials according to the formula ratio, calcining and melting at 1500°C to form a melt, and then adding it into water for rapid cooling to obtain a block glass frit. The block glass frit is crushed and sieved for standby use, and the crushing and screening mesh is controlled to be 90 meshes;
[0095] ⑾ Hot bending and firing: the ceramic tile blanks with transparent protective glaze are sent into a shuttle kiln for firing. The hot bending temperature is controlled at 900°C and the firing time is 490 minutes to obtain a semi-finished curved ceramic plate. The semi-finished curved ceramic plate is polished and edge-ground to finally obtain a finished curved ceramic plate (see Figure 2).
[0096] Example 3
[0097] See also Figure 1 As shown, the curved ceramic plate is composed of a base glaze and a transparent glaze protective glaze constituting a composite layer. The ceramic hot bending process of the curved ceramic plate includes the following steps:
[0098] ⑴ Preparation of powder: ball milling according to the proportion of raw materials in the formula, and spray powdering to obtain green body powder and store it for aging;
[0099] (2) Pressing and forming, feeding the obtained powder into a press for pressing to obtain a ceramic green body with a green body thickness of 6.5 mm, a width of 1271 mm, and a length of 2754 mm;
[0100] ⑶ Drying of green body: sending the formed ceramic green body into roller kiln for drying;
[0101] (4) Primary biscuit firing: the dried body is sent to a roller kiln for firing at a temperature of 1200°C. The biscuit strength is 50 MPa.
[0102] ⑸ Dust removal and heating: the surface of the unglazed porcelain tile blank is dusted and sent to an infrared drying kiln for heating to obtain an unglazed porcelain blank with a certain temperature. The temperature of the unglazed porcelain blank after heating is 70°C and the heating time is 9 minutes;
[0103] ⑹ Base glaze spraying: the heated unglazed porcelain body is decorated with base glaze high pressure spraying. The base glaze spraying pressure is 12 bar, the base glaze specific gravity is 1.50, and the glaze amount is 300g / m 2 , the average particle size D50 of the base glaze slurry is controlled to be 6.7μm, and the glossiness of the base glaze is 6°;
[0104] The base glaze formula is composed of the following raw material components by weight: 25 parts of frit A, 57 parts of frit B, 12 parts of zirconium silicate, 6 parts of kaolin, 15 parts of fixing agent, 0.25 parts of methyl, and 0.5 parts of sodium tripolyphosphate;
[0105] The base glaze formula is composed of the following chemical components by weight: SiO2 53.93wt%, Al2O3 10.55wt%, Fe2O3 0.13wt%, K2O 3.93wt%, Na2O 1.16wt%, CaO 8.57wt%, MgO 0.48wt%, ZnO 9.23wt%, ZrO2 7.61wt%, B2O3 1.11wt%, BaO 2.70wt%, and ignition loss 0.60wt%;
[0106] The frit A is composed of the following raw material components by weight: 12 parts of zinc oxide, 11 parts of barium carbonate, 11 parts of aluminum oxide, 31 parts of quartz, 24 parts of wollastonite, 1.5 parts of magnesium oxide, 1.5 parts of boron oxide, 3.5 parts of sodium carbonate, and 4.5 parts of potassium carbonate;
[0107] The frit A consists of the following chemical components by weight: SiO2 49.83wt%, Al2O3 13.15wt%, Fe2O3 0.19wt%, K2O 2.89wt%, Na2O 1.80wt%, CaO 9.13wt%, MgO 1.34wt%, ZnO 11.38wt%, B2O3 1.60wt%, BaO 8.64wt%, and loss on ignition 0.05wt%.
[0108] The frit B is composed of the following raw material components by weight: 11 parts of zinc oxide, 1 part of barium carbonate, 7 parts of aluminum oxide, 39 parts of quartz, 28 parts of wollastonite, 1.5 parts of boron oxide, 2.5 parts of sodium carbonate, and 10 parts of potassium carbonate;
[0109] The frit B described in this embodiment is composed of the following chemical components by weight: SiO2 61.21wt%, Al2O37.05wt%, Fe2O3 0.14wt%, K2O 5.63wt%, Na2O 1.25wt%, CaO11.03wt%, MgO 0.25wt%, ZnO 11.20wt%, B2O3 1.24wt%, BaO 0.95wt%, and ignition loss 0.05wt%;
[0110] The frit A and frit B are prepared by mixing raw materials in a formula ratio, calcining and melting them at 1600°C to form a melt, and then adding them into water for rapid cooling to obtain a block glass frit. The block glass frit is crushed and sieved for standby use, and the crushing and sieve mesh is controlled to be 80 meshes.
[0111] The fixing agent is composed of water bubbles, a suspending agent, and super-plastic ball clay, wherein the water bubbles are prepared by mixing and grinding sodium carboxymethyl cellulose and water in a ratio of 15:85; the suspending agent is composed of the following raw materials by weight: 20 parts of methyl glycol, 20 parts of sodium carboxymethyl cellulose, 20 parts of polymethylsiloxane, 1 part of sodium metaphosphate, 0.4 parts of sodium dodecylbenzene sulfonate, and 0.6 parts of dodecyltrimethylammonium bromide; and 38 parts of deionized water;
[0112] ⑺ Glaze drying: the bricks after the base glaze is dried by infrared, the drying temperature is 120℃, and the drying time is 5min;
[0113] ⑻ Pattern decoration: pattern decoration according to product effect requirements;
[0114] ⑼ Brick heating: The bricks with pattern decoration are subjected to electric infrared heating at a temperature of 150°C for 15 minutes. The temperature of the bricks after heating is 110°C to ensure that the decorative pattern is completely dry;
[0115] ⑽Apply protective glaze: spray the heated brick with transparent protective glaze at high pressure. The spraying pressure of transparent protective glaze is 12 bar, the specific gravity of transparent protective glaze is 1.30, and the glaze amount is 210g / m 2 , the average particle size D50 of the transparent protective glaze is controlled to 7.2μm, and the glossiness of the transparent protective glaze is controlled to 10°;
[0116] The transparent protective glaze formula is composed of the following raw material components by weight: 20 parts of bright transparent frit, 75 parts of matte transparent frit, 5 parts of kaolin, 0.25 parts of methyl, and 0.5 parts of sodium tripolyphosphate;
[0117] The transparent protective glaze is composed of the following chemical components by weight: SiO2 48.83wt%, Al2O3 14.10wt%, Fe2O3 0.11wt%, K2O 0.41wt%, Na2O 5.08wt%, CaO 3.11wt%, MgO1.06wt%, ZnO 0.88wt%, B2O3 22.09wt%, BaO 1.89wt%, SrO 1.86wt%, and ignition loss 0.58wt%;
[0118] The bright transparent frit is composed of the following raw material components by weight: 4 parts of zinc oxide, 12 parts of barium carbonate, 2.5 parts of aluminum oxide, 29 parts of quartz, 4 parts of wollastonite, 24 parts of boron oxide, 23 parts of sodium carbonate, and 1.5 parts of potassium carbonate.
[0119] The bright transparent frit consists of the following chemical components by weight: SiO2 47.01wt%, Al2O3 2.75wt%, Fe2O3 0.16wt%, K2O 0.98wt%, Na2O 9.14wt%, CaO 1.65wt%, MgO 0.10wt%, ZnO 4.38wt%, B2O3 24.35wt%, BaO 9.45wt%, and ignition loss 0.03wt%.
[0120] The matte transparent frit formula consists of the following raw material components by weight: 15 parts of aluminum oxide, 40 parts of quartz, 8 parts of wollastonite, 22 parts of boron oxide, 1.5 parts of magnesium oxide, 9 parts of sodium carbonate, 0.5 parts of potassium carbonate, and 4 parts of strontium carbonate.
[0121] The matte transparent frit is composed of the following chemical components by weight: SiO2 48.92wt%, Al2O3 15.80wt%, Fe2O3 0.08wt%, K2O 0.28wt%, Na2O 4.33wt%, CaO 3.67wt%, MgO 1.43wt%, B2O3 22.96wt%, SrO 2.48wt%, and loss on ignition 0.05wt%.
[0122] The bright transparent frit and the matte transparent frit are obtained by mixing raw materials according to the formula ratio, calcining and melting at a temperature of 1500°C to form a melt, and then adding the melt into water for rapid cooling to obtain a block glass frit. The block glass frit is crushed and sieved for standby use, and the crushing and sieving mesh is controlled to be 120 meshes;
[0123] ⑾ Hot bending and firing: the ceramic tile blanks with transparent protective glaze are sent into a shuttle kiln for firing. The hot bending temperature is controlled at 950°C and the firing time is 450 minutes to obtain a semi-finished curved ceramic plate. The semi-finished curved ceramic plate is edge-grinded to finally obtain a finished curved ceramic plate (see Figure 2).
[0124] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should fall within the scope of the claims of the present invention.
Claims
1. A ceramic hot bending process for a curved ceramic plate, characterized in that: The following steps are involved: ⑴ Preparation of powder: ball milling according to the proportion of raw materials in the formula, and spray powdering to obtain green body powder and store it for aging; (2) Pressing and forming, feeding the obtained powder into a press for pressing to obtain a ceramic green body, the green body thickness is controlled to be 6-10 mm, the width is controlled to be 600-1750 mm, and the length is controlled to be 1200-3500 mm; ⑶ Drying of green body: sending the formed ceramic green body into roller kiln for drying; (4) Primary biscuit firing: the dried body is sent to a roller kiln for firing at a temperature of 1100-1200°C. The strength of the biscuit-fired porcelain body is controlled to be 45-55 MPa. ⑸ Dust removal and heating: the surface of the unglazed porcelain tile blank is dusted and sent to the infrared drying kiln for heating to obtain an unglazed porcelain blank with a certain temperature. After heating, the temperature of the unglazed porcelain blank is controlled to be 65-150°C, and the heating time is 6-9 minutes; ⑹ Base glaze spraying: the heated unglazed porcelain body is decorated with base glaze under high pressure spraying. The base glaze spraying pressure is 6-15 bar, the base glaze specific gravity is 1.50±0.02, and the glaze application amount is 300-400 g / m 2 , the average particle size D50 of the base glaze slurry is controlled to be 6-8μm, and the glossiness of the base glaze is controlled to be 6-10°; ⑺ Glaze drying: the bricks after base glaze application are dried by infrared rays at a temperature of 120-240°C and a drying time of 3-5 minutes; ⑻ Pattern decoration: pattern decoration according to product effect requirements; ⑼ Heating the bricks: heating the bricks decorated with patterns, using electric infrared heating or flame burning heating, with a heating temperature of 150-300°C and a heating time of 8-15 minutes. The temperature of the bricks after heating is controlled at 70-120°C to ensure that the decorative patterns are completely dry; ⑽ Apply protective glaze: spray the heated bricks with transparent protective glaze at high pressure. The spraying pressure of the transparent protective glaze is 8-15 bar, the specific gravity of the transparent protective glaze is 1.30-1.60, and the glaze amount is 120-400g / m 2 , the average particle size D50 of the transparent protective glaze is controlled to be 6-8 μm, and the glossiness of the transparent protective glaze is controlled to be 10-95°; ⑾ Hot bending and firing: the ceramic tile blanks with transparent protective glaze are sent into a shuttle kiln for firing. The hot bending temperature is controlled at 900-950°C and the firing time is 350-500 minutes to obtain a semi-finished curved ceramic plate. The semi-finished curved ceramic plate is polished or not polished and edged to finally obtain a finished curved ceramic plate.
Citation Information
Patent Citations
High-curvature wide-color-gamut ceramic curved surface rock plate and preparation method and application thereof
CN113979738A
Ceramic glaze and preparation method thereof
CN107417117A
Sanitary ceramic sanitary appliance warm and humid glaze with soft impression and preparation process thereof
CN108455857A
Manufacturing method of soft-light glazed ceramic chip
CN111875415A
One-time firing process of curved surface ceramic rock plate
CN114702297A