A light-shielding composite film and its preparation method and application

Through the dual curing system of aqueous acrylate, isocyanate and amino resin, the problem of easy shedding and poor temperature resistance of the light-shielding composite film coating is solved, and better adhesion and durability are achieved, ensuring the stability of optical performance and Easy to operate.

CN116655979BActive Publication Date: 2024-12-03ZHONGSHAN YONGXIN ELECTRONIC TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310671255.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-07
Publication Date
2024-12-03
Estimated Expiration
2043-06-07

AI Technical Summary

Technical Problem

The coating of the existing light-shielding composite film is prone to fall off and deform, and has poor wear resistance, high temperature resistance and chemical reagent resistance.

Method used

A polyurethane system formed by aqueous acrylate and isocyanate is used, and a double curing crosslinking system combined with an amino resin is formed to form a light-shielding composite film with good adhesion and alkali resistance, wear resistance, high temperature and high humidity resistance, and chemical reagent resistance.

Benefits of technology

The adhesion, alkali resistance, wear resistance and high temperature and high humidity resistance of the light-shielding film are improved, the stability and operational convenience of the light-shielding composite film are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004273034470000051
    Figure BDA0004273034470000051
  • Figure BDA0004273034470000061
    Figure BDA0004273034470000061
  • Figure BDA0004273034470000071
    Figure BDA0004273034470000071
Patent Text Reader

Abstract

The invention discloses a shading composite film and a preparation method and application thereof, comprising a first black matte layer, a carrier base film and a second black matte layer stacked in sequence from top to bottom; the raw materials for preparing the first black matte layer and the second black matte layer include matte ink; the matte ink includes component A and component B; component A includes the following raw materials in parts by weight: 30-60 parts of water-based acrylic resin and 10-32 parts of amino resin; component B includes the following raw materials in parts by weight: 8-22 parts of isocyanate curing agent. The polyurethane system formed by acrylate and isocyanate cooperates with the amino resin to give the coating good adhesion, heat resistance, alkali resistance, wear resistance, chemical resistance, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of light-shielding films, and in particular relates to a light-shielding composite film and a preparation method and application thereof. Background Art

[0002] With the widespread use of portable communication camera equipment (such as mobile phones, video cameras, digital cameras, wearable devices, etc.), the demand for light-shielding materials for optical lenses is becoming more and more extensive, and the performance requirements for light-shielding materials are becoming higher and higher. In order to suppress the adverse effects of external light on camera quality such as halo and ghosting, the current solution is to use polyester film with matte ink on the surface as light-shielding material in optical components.

[0003] In the shading composite film formed by the existing method, the coating of the shading film is prone to fall off and deformation, and has poor wear resistance and high temperature resistance.

[0004] Therefore, it is urgent to solve the problems that the coating of the current shading composite film is prone to falling off and deformation, and has poor wear resistance, chemical resistance and high temperature resistance. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a light-shielding composite film, wherein the polyurethane system formed by acrylate and isocyanate has good wear resistance and good adhesion, and the dual-curing cross-linking system formed by the amino resin has better resistance to high temperature and humidity, chemical reagents and thermal shock.

[0006] The second aspect of the present invention provides a method for preparing the above-mentioned light-shielding composite film.

[0007] The third aspect of the present invention provides an application of the above-mentioned light-shielding composite film in an optical instrument.

[0008] A light-shielding composite film according to an embodiment of the first aspect of the present invention comprises a first black matte layer, a carrier base film and a second black matte layer stacked in sequence from top to bottom;

[0009] The matte ink comprises component A and component B;

[0010] The component A comprises the following raw materials in parts by weight: 30-60 parts of water-based acrylic resin and 10-32 parts of amino resin;

[0011] The component B comprises the following raw materials in parts by weight: 8 to 22 parts of isocyanate curing agent.

[0012] The embodiments according to the first aspect of the present invention have at least the following beneficial effects:

[0013] After the shading film is die-cut, the die-cut surface needs to be alkaline matted, so the shading coating needs to have good alkali resistance. The present invention adopts a water-based dual-cure system to increase the adhesion, alkali resistance, wear resistance, chemical reagent resistance, high and low temperature impact resistance, high temperature and high humidity resistance and weather resistance of the coating. The polyurethane system formed by water-based acrylic resin and isocyanate has good toughness, wear resistance, good adhesion and alkali resistance, and the dual-cure cross-linking system formed by the amino resin system has better high temperature and humidity resistance, chemical reagent resistance and thermal shock resistance; amino resin has good surface hydrophobicity, and the dual-cure system of the matting ink ensures the optical performance and ease of operation of the shading composite film after being corroded by alkaline matting.

[0014] According to some embodiments of the present invention, the water-based acrylic resin includes at least one of a water-based acrylic polyol and a water-based acrylic modified polyester.

[0015] According to some embodiments of the present invention, the acid value of the water-based acrylic modified polyester is 30-80 mgKOH / g.

[0016] According to some embodiments of the present invention, the water-based acrylic resin comprises: At least one of 1753, JT-202, AA-8662S and AA-8672S.

[0017] According to some embodiments of the present invention, the amino resin includes at least one of methyl etherified melamine resin and glycoluril resin.

[0018] According to some embodiments of the present invention, the amino resin is more preferably a highly methylated melamine resin.

[0019] According to some embodiments of the present invention, the amino resin includes AA-9077, CYMEL 303LF and CYMEL TM At least one of 1172.

[0020] According to some embodiments of the present invention, the isocyanate curing agent includes an aliphatic isocyanate curing agent.

[0021] According to some embodiments of the present invention, the aliphatic isocyanate curing agent includes at least one of water-soluble blocked isocyanate curing agent 125, Baihaidu XP 2547, YC-820, F-70D and CH100.

[0022] According to some embodiments of the present invention, the raw materials for preparing the carrier base film include at least one of black polyester film, transparent polyester film, black polycarbonate film, transparent polycarbonate film, black polyimide film, transparent polyimide film, brown polyimide film, black polyamideimide film and transparent polyamideimide film.

[0023] According to some embodiments of the present invention, the raw materials for preparing component A further include: matting powder.

[0024] According to some embodiments of the present invention, the matting powder includes at least one of an organic matting powder and an inorganic matting powder.

[0025] According to some embodiments of the present invention, the organic matting powder polymer particles include AK-800TR.

[0026] According to some embodiments of the present invention, the particle size of the organic matting powder is 2-8 μm.

[0027] According to some embodiments of the present invention, the inorganic matting powder includes silicon dioxide.

[0028] According to some embodiments of the present invention, the particle size of the silicon dioxide is 1 to 5 μm.

[0029] According to some embodiments of the present invention, the silicon dioxide includes at least one of water-based silicon dioxide WE1011 and GS-402 matting powder.

[0030] The micron-sized silica matting powder used in the present invention is easy to disperse and has a significant matting effect. It can also improve the hardness of the ink coating and the abrasion resistance of the coating. In addition, silica has a certain hydrophobicity. During the cleaning process after die cutting and the cleaning process after corrosion matting, the surface is not easily contaminated with dirt to affect the optical properties.

[0031] According to some embodiments of the present invention, the raw materials for preparing component A further include: carbon black.

[0032] According to some embodiments of the present invention, the carbon black includes at least one of high-pigment carbon black and conductive carbon black.

[0033] According to some embodiments of the present invention, the high pigment carbon black comprises waterborne carbon black coating high pigment carbon black.

[0034] According to some embodiments of the present invention, the conductive carbon black includes at least one of conductive carbon black super P, high conductive carbon black ZC800 and Hi-Black 420B.

[0035] According to some embodiments of the present invention, the particle size of the carbon black is 10-100 nm.

[0036] The conductive carbon black of the invention reduces the surface resistance of the light-shielding composite film and improves the antistatic property of the light-shielding composite film.

[0037] According to some embodiments of the present invention, the raw materials for preparing component A further include: at least one of a dispersant, a cross-linking agent, a leveling agent, a wax powder and an adhesion promoter.

[0038] According to some embodiments of the present invention, the dispersant includes at least one of dispersant DH-6601S and aqueous dispersant W1152.

[0039] According to some embodiments of the present invention, the cross-linking agent includes aziridine cross-linking agent HP-100.

[0040] According to some embodiments of the present invention, the promoter includes A-830 water-based adhesion promoter.

[0041] According to some embodiments of the present invention, the wax powder includes at least one of polypropylene wax, polyethylene wax and polytetrafluoroethylene wax.

[0042] According to some embodiments of the present invention, the wax powder includes SGW-102.

[0043] The wax powder of the present invention has fine particle size and has the functions of hardening, improving wear resistance, scratch resistance and hydrophobicity, effectively improving the surface scratch resistance of the shading composite film, reducing the surface roughness of the shading composite film, and improving the hydrophobicity of the surface of the shading composite film.

[0044] In the present invention, the above-mentioned dispersant, leveling agent, wax powder and cross-linking agent are auxiliary agents.

[0045] According to some embodiments of the present invention, the component A comprises the following preparation raw materials in parts by weight:

[0046] 30-60 parts of water-based acrylic resin, 10-32 parts of amino resin, 3-12 parts of matting powder, and 5-20 parts of carbon black.

[0047] According to some embodiments of the present invention, the component B further comprises a sulfonic acid catalyst.

[0048] According to some embodiments of the invention, the sulfonic acid catalyst includes DH-7356N.

[0049] According to some embodiments of the present invention, the component B comprises the following preparation raw materials in parts by weight:

[0050] 8 to 22 parts of isocyanate curing agent and 0.2 to 2 parts of sulfonic acid catalyst.

[0051] According to some embodiments of the present invention, the carrier base film has a thickness of 4-200 μm.

[0052] According to some embodiments of the present invention, the thickness of the first black matte layer and the second black matte layer is 2-20 μm.

[0053] The shading composite film of the present invention has the performance of strong alkali resistance, meets the matting corrosion process, has good adhesion, no deformation, and no change in reflectivity and optical density; the surface is hydrophobic and non-adhesive after matting corrosion, which is beneficial to optical stability and convenient operation.

[0054] According to a second aspect of the present invention, a method for preparing a light-shielding composite film is provided, comprising:

[0055] A first black matte layer is coated on one surface of the carrier base film, and a second black matte layer is coated on the other surface.

[0056] According to some embodiments of the present invention, the method for preparing the light-shielding composite film comprises: coating a first black matte layer on one surface of a carrier base film, drying it, and then coating a second black matte layer on the other surface of the carrier base film, drying it, and aging it to obtain a light-shielding composite film for optical instruments.

[0057] According to some embodiments of the present invention, the drying temperature is 60-120°C.

[0058] According to some embodiments of the present invention, the drying time is 2 to 5 minutes.

[0059] The above baking time and temperature can avoid the coating sticking after winding and curing due to incomplete solvent volatilization, which affects the appearance and optical properties.

[0060] According to some embodiments of the present invention, the aging temperature is 25-65°C.

[0061] According to some embodiments of the present invention, the aging temperature is 55°C.

[0062] According to some embodiments of the present invention, the aging time is 20 to 60 hours.

[0063] According to some embodiments of the present invention, the aging time is 48 hours.

[0064] According to some embodiments of the present invention, the coating method includes at least one of extrusion coating, micro-dimple coating, doctor blade coating and screen roller coating.

[0065] According to some preferred embodiments of the present invention, the coating method includes at least one of slot extrusion coating and micro-dimple coating.

[0066] According to some preferred embodiments of the present invention, the coating method comprises dimple coating.

[0067] According to some embodiments of the present invention, the method for preparing the first black matte layer and the second black matte layer includes: mixing the component A and the component B to obtain a matte ink.

[0068] According to a third aspect of the present invention, an embodiment of the present invention provides an application of the light-shielding composite film in an optical instrument.

[0069] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0071] Figure 1 It is a schematic diagram of the structure of the light-shielding composite film of Example 1 of the present invention. DETAILED DESCRIPTION

[0072] Embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.

[0073] Main raw material brands and manufacturers:

[0074] Waterborne Acrylic Polyols: 1753 (hydroxyl value 138mgKOH / g Allnex Resin (China) Co., Ltd.), JT-202 water-based acrylic modified polyester resin (Foshan Juntu New Materials Co., Ltd.), AA-8662S (acid value 70mgKOH / g Suzhou Qingtian New Materials Co., Ltd.), AA-8672S (acid value 50mgKOH / g Suzhou Qingtian New Materials Co., Ltd.);

[0075] Amino resin: AA-9077 (Suzhou Qingtian New Materials Co., Ltd.), CYMEL 303LF (U.S. Cytec Industries, Inc.);

[0076] Matting powder polymer particles AK-800TR (particle size 6um, Negami Industry Co., Ltd.), water-based silica wood paint additive WE1011 (particle size; 4.2 microns, Tosoh Corporation), GS-402 matting powder (particle size 1.8um, Foshan Shangjin Chengzhan New Material Technology Co., Ltd.);

[0077] Water-based carbon black coatings high pigment carbon black (Jinan DeLan Chemical Co., Ltd.), water-soluble conductive carbon black super P (particle size 20 nanometers, Tianjin Tianyi Century Chemical Products Technology Development Co., Ltd.), high conductive carbon black ZC800 (Tianjin Huayuan Chemical Technology Co., Ltd.), Hi-Black 420B (Olilong Engineering Carbon Group);

[0078] Water-based leveling agent: KMT-5510S leveling agent (Foshan Koning New Materials Co., Ltd.);

[0079] Dispersant DH-6601S (Suzhou Qingtian New Materials Co., Ltd.), water-based dispersant W1152 (Shenzhen Qiming Chemical Additives Co., Ltd.), aziridine crosslinker HP-100 (Guangzhou Huipu New Materials Co., Ltd.), A-830 water-based adhesion promoter (Foshan Juntu New Materials Co., Ltd.);

[0080] SGW-102 synthetic wax powder (Foshan Shangjin Chengzhan New Material Technology Co., Ltd.);

[0081] Curing agent: water-soluble blocked isocyanate curing agent 125 (Guangzhou Hangeng New Materials Co., Ltd.), Baihaidu XP2547 (Covestro), water-soluble blocked isocyanate curing agent H-125 (water-soluble blocked isocyanate curing agent 125), YC-820 (Anhui Yuanchen New Materials Technology Co., Ltd.), F-70D (Wuhan Shiquanxing New Materials Technology Co., Ltd.), CH100 (Guangzhou Changhao Trading Co., Ltd.);

[0082] Catalyst: Environmentally friendly fully enclosed sulfonic acid catalyst DH-7356N (Suzhou Qingtian New Materials Co., Ltd.).

[0083] Example 1

[0084] This embodiment discloses a light-shielding composite film and a preparation method thereof, and the specific steps are as follows:

[0085] S1: Mix water-based acrylic resin, amino resin, carbon black, matting powder and additives as shown in Table 1 below, sand grind them 3 times with a sand grinder, and then add curing agent and catalyst and stir evenly;

[0086] S2: Select a carrier base film, apply a first black matte layer of matte ink on one surface of the carrier base film, dry it at 110°C for 3 minutes, then apply the second black matte layer materials on the other opposite surface of the carrier base film, dry it at 110°C for 3 minutes, and mature it at 55°C for 48 hours to obtain a light-shielding composite film for optical instruments.

[0087] The structural schematic diagram of the light-shielding composite film of Example 1 is as follows Figure 1 As shown;

[0088] The amounts of the components of the matte ink of Example 1 are shown in Table 1;

[0089] Table 1. Amount of each component

[0090]

[0091]

[0092]

[0093] Example 2

[0094] This embodiment discloses a light-shielding composite film and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the contents of the components of the light-shielding composite film matting ink are as shown in Table 2, and the other conditions are the same as those in embodiment 1.

[0095] Table 2. Amount of each component

[0096]

[0097]

[0098] Example 3

[0099] This embodiment discloses a light-shielding composite film and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the contents of the components of the light-shielding composite film matte ink are as shown in Table 3, and the other conditions are the same as those in embodiment 1.

[0100] Table 3. Amount of each component

[0101]

[0102]

[0103] Example 4

[0104] This embodiment discloses a light-shielding composite film and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the contents of the components of the light-shielding composite film matting ink are as shown in Table 4, and the other conditions are the same as those in embodiment 1.

[0105] Table 4. Amount of each component

[0106]

[0107]

[0108] Example 5

[0109] This embodiment discloses a light-shielding composite film and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the contents of the components of the light-shielding composite film matte ink are as shown in Table 5, and the other conditions are the same as those in embodiment 1.

[0110] Table 5. Amount of each component

[0111]

[0112]

[0113] Example 6

[0114] This embodiment discloses a light-shielding composite film and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the contents of the components of the light-shielding composite film matte ink are as shown in Table 6, and the other conditions are the same as those in embodiment 1.

[0115] Table 6. Dosage of each component

[0116]

[0117]

[0118] Comparative Example 1

[0119] This comparative example discloses a shading composite film and a preparation method thereof. The difference between this comparative example and Example 1 is that the amount of the water-based acrylic resin in the matte ink component is 20 parts. 1753, and the other conditions are the same as those in Example 1.

[0120] Comparative Example 2

[0121] This comparative example discloses a light-shielding composite film and a preparation method thereof. The difference between this comparative example and Example 1 is that the amount of amino resin added in the matte ink component is 5 parts of CYMEL 303LF, and the other conditions are the same as those in Example 1.

[0122] Comparative Example 3

[0123] This comparative example discloses a shading composite film and a preparation method thereof. The difference between this comparative example and Example 1 is that the amount of the water-based curing agent added to the matte ink component is 3 parts of a water-soluble blocked isocyanate curing agent 125, and the other conditions are the same as those in Example 1.

[0124] Comparative Example 4

[0125] This comparative example discloses a light-shielding composite film and a preparation method thereof. The difference between this comparative example and Example 1 is that no catalyst is added to the matte ink component. The contents of each component of the light-shielding composite film are shown in Table 2, and the other conditions are the same as Example 1.

[0126] Comparative Example 5

[0127] This comparative example discloses a light-shielding composite film and a preparation method thereof. The difference between this comparative example and Example 1 is that no conductive carbon black is added to the matte ink component. The contents of each component of the light-shielding composite film are shown in Table 2, and the other conditions are the same as those in Example 1.

[0128] Test method:

[0129] In the present invention, various tests are performed on the shading composite films prepared according to the following different preparation conditions to verify their performance in terms of optical density, glossiness, surface resistance, surface roughness, coating scratch resistance, coating adhesion, high temperature and high humidity reliability, etc. The test results are shown in Table 7.

[0130] For the above characteristics, the test method is as follows:

[0131] 1. Optical density

[0132] Optical density is a characteristic measure of the absorption of light by an object, that is, the ratio of the amount of incident light to the amount of reflected light or transmitted light. It is usually expressed as the decimal logarithm of the reciprocal of transmittance or reflectance. It is an important parameter to characterize the light-shielding performance of the light-shielding composite film. The transmittance of the cured light-shielding composite film is tested and calculated using a Hitachi 4100 spectrometer. The greater the optical density, the smaller the light transmittance, and the better the light-shielding performance of the light-shielding composite film. Take the average value of the 5 test points, and record it as ○ if it is greater than 6, record it as △ if it is greater than 4 and less than 6, and record it as × if it is less than 4.

[0133] 2. Glossiness

[0134] Glossiness is used to characterize the degree of reflection of visible light on the matte coating surface of the shading composite film, and is a parameter that characterizes the matte effect of the shading composite film. According to the GB / T9754-2007 standard, the surface glossiness of the shading composite film is tested when the incident angle of visible light is 60°. The lower the glossiness, the better the matte property. The average value is taken from the test of 5 points.

[0135] 3. Surface resistance

[0136] Surface resistance is an important parameter to measure the antistatic effect of shading composite film. According to ASTM D-257 standard, when testing, just place two weights on the surface of shading composite film and press the test button. The instrument will display the surface resistance value of the measured object, and take the average value of 5 test points.

[0137] 4. Surface roughness

[0138] Surface roughness refers to the unevenness of the small spacing and tiny peaks and valleys on the surface of the shading composite film. The distance (wave distance) between two wave crests or two wave valleys is very small (below 1mm), which belongs to the microscopic geometric shape error. The smaller the surface roughness, the smoother the surface. According to the GB / T131-2006 standard, after calibrating the test probe with a standard test piece before testing, place the probe on the surface of the shading composite film to test the surface roughness Ra, and test 5 points to get the average value.

[0139] 5. Scratch resistance

[0140] The surface scratch resistance of the shading composite film is an important parameter to characterize the reliability of the shading composite film during die-cutting, assembly and use of optical devices. According to the GB / T 9279-2015 standard, a circular scratching needle is used at a speed of 5 mm / s and a load of 200 g. If no scratches are caused on the surface of the shading composite film after 5 times of measurement, it is ○, otherwise it is ×.

[0141] 6. Contact angle

[0142] Poor hydrophobicity on the surface of the shading composite film will cause the shading composite film to stick after cleaning after die-cutting and cleaning and drying after alkaline solution matting, affecting the shading effect and assembly operation efficiency of the shading composite film. According to the GB / T 30693-2014 standard, the water contact angle on the surface of the shading composite film is tested, and the average value is taken from 10 test points. When the surface water contact angle of the shading composite film is greater than 90°, the surface of the shading composite film is a hydrophobic surface, which is marked as ○, otherwise it is marked as ×.

[0143] 7. Lubricity

[0144] In order to study the surface lubricity of the shading composite film, the surface dynamic friction coefficient (μ d ) and static friction coefficient (μ s ), dynamic friction coefficient (μ d ) and static friction coefficient (μ s ) are all less than 0.3, which is ○; greater than 0.3, which is ×.

[0145] 8. Coating Adhesion

[0146] According to GB / T9286-2021 standard, the initial adhesion of the black matte layer of the shading composite film was tested by the white grid knife method. In order to study the adhesion of the coating after the shading composite film was matted with alkali solution, the shading composite film was immersed in a 50% concentration of NaOH solution at 80°C for 30 minutes. The edges of the cuts made by the white grid knife test of the black matte coating on both sides of the shading film were smooth, and there was no shedding of the grid edge, which was ○, otherwise it was ×.

[0147] 9. Chemical resistance test of matt layer

[0148] According to GB / T 23989-2009 standard, a dust-free cloth was soaked with alcohol and acetone respectively, and then the matte layer was wiped back and forth three times with a force of 1000g. If there was no discoloration or shedding of the matte layer in the wiped area, it was marked as ○, otherwise it was marked as ×.

[0149] / 10. High temperature and high humidity reliability test.

[0150] The shading composite film was placed in a high temperature and high humidity box at a temperature of 85°C and a relative humidity of 85% for 120 hours, and then taken out and placed at room temperature for 2 hours. If there was no detachment, white spots, black spots, etc. on the surface of the shading composite film, it was marked as ○, otherwise it was marked as ×.

[0151] Table 7 Performance test results of shading composite film samples of embodiments and comparative examples

[0152]

[0153]

[0154] According to the above test results, it can be seen that the light-shielding film prepared with the matte ink of the above Examples 1 to 6 as raw materials has good comprehensive performance. The main difference between Example 4 and Example 1 is that the amount of matte powder added is less, the matte effect of the matte ink is relatively low, and the glossiness of the prepared light-shielding film is relatively large, but still within the allowable range. The main difference between Example 5 and Example 1 is that the amount of high-pigment carbon black and high-conductivity carbon black added is less, the matte ink has a poor light-shielding effect, a slightly higher glossiness, and a larger surface resistance, but still has good optical properties and antistatic properties.

[0155] The test results of Comparative Example 1 show that when the amount of water-based acrylic resin added is insufficient, the resin content is low, the adhesion is poor, and the chemical resistance and high temperature and high humidity resistance are poor. The test results of Comparative Example 3 show that the amount of curing agent added is insufficient, the ink cannot be completely cured, and the ink has poor adhesion, scratch resistance, chemical resistance and high temperature and high humidity resistance. In Comparative Example 2, the amount of amino resin added is small, and the prepared shading film has poor chemical resistance. In Comparative Example 4, no catalyst was added, the amino resin and water-based acrylic resin were not completely cured and cross-linked, and the prepared shading film had poor scratch resistance and chemical resistance and could not meet application requirements. In Comparative Example 5, no high-conductive carbon black was added, and the surface resistance of the prepared shading film was large, and it did not have an antistatic effect.

[0156] In summary, the present invention provides a light-shielding composite film and a preparation method thereof. The present invention utilizes a dual-curing system of water-based acrylate, isocyanate and amino resin, and then reasonably combines ingredients such as matting powder, carbon black and additives to effectively improve the adhesion and high temperature and high humidity resistance of the matting ink.

[0157] The embodiments of the present invention are described in detail with reference to the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A light-shielding composite film, characterized in that: It includes a first black matte layer, a carrier base film and a second black matte layer which are sequentially stacked from top to bottom; The raw materials for preparing the first black matte layer and the second black matte layer include matte ink; The matte ink comprises component A and component B; The component A comprises the following raw materials in parts by weight: 30-60 parts of water-based acrylic resin and 10-32 parts of amino resin; The raw materials for preparing the component A also include: carbon black; The component B comprises the following raw materials in parts by weight: 8 to 22 parts of isocyanate curing agent and 0.2 to 2 parts of sulfonic acid catalyst; The water-based acrylic resin includes water-based acrylic acid polyol and acrylic acid-modified polyester resin; The amino resin includes at least one of methyl etherified melamine resin and glycoluril resin.

2. The light-shielding composite film according to claim 1, characterized in that: The carrier base film is prepared from raw materials including at least one of black polyester film, transparent polyester film, black polycarbonate film, transparent polycarbonate film, black polyimide film, transparent polyimide film, brown polyimide film, black polyamideimide film and transparent polyamideimide film.

3. The light-shielding composite film according to claim 1, characterized in that: The thickness of the carrier base film is 4-200 μm.

4. The light-shielding composite film according to claim 1, characterized in that: The thickness of the first black matte layer and the second black matte layer is 2-20 μm.

5. A method for preparing a light-shielding composite film according to any one of claims 1 to 4, characterized in that: include: A first black matte layer is coated on one surface of the carrier base film, and a second black matte layer is coated on the other surface.

6. The preparation method according to claim 5, characterized in that: The method for preparing the first black matte layer and the second black matte layer comprises: mixing raw materials for preparing the first black matte layer and the second black matte layer.

7. The preparation method according to claim 5, characterized in that: The coating method includes at least one of extrusion coating, micro-dimple coating, doctor blade coating and screen roll coating.

8. Use of the shading composite film according to any one of claims 1 to 4 in optical instruments.

Citation Information

Patent Citations

  • Coating method of adjustable-gloss extinction transparent electrophoretic coating

    CN108467656A

  • Shading composite film for optical instruments and preparation method thereof

    CN111675818A

  • Thermosetting adjustable matte gloss oil for metal printing and preparation method of thermosetting adjustable matte gloss oil

    CN115322662A

  • Water-based electronic component insulating paint and preparation method thereof

    CN115678403A