A temperature-compensated surface acoustic wave resonator and a method for preparing the same

By introducing lateral structural changes of the suspended metal layer in the surface acoustic wave resonator and optimizing the mass loading effect at the ends of the interdigital electrode fingers, the problem of difficult clutter suppression in the traditional temperature-compensated surface acoustic wave filter is solved and the electrical efficiency is improved. performance and process stability, achieving better clutter suppression effect.

CN116667808BActive Publication Date: 2024-10-22深圳新声半导体有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310960840.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-02
Publication Date
2024-10-22
Estimated Expiration
2043-08-02

AI Technical Summary

Technical Problem

Traditional temperature-compensated surface acoustic wave filters have limitations in clutter suppression. Limited by the accuracy of the photolithography machine and process stability, it is difficult to effectively suppress clutter, resulting in poor electrical performance.

Method used

By introducing lateral structural changes of the suspended metal layer in the surface acoustic wave resonator, the width of the suspended metal layer changes with the continuous wavelength of the apodization area of ​​the resonator, optimizing the mass loading effect at the ends of the interdigitated electrode fingers, forming a better hybrid Wave suppression effect.

Benefits of technology

It improves the performance of the resonator, enhances the clutter suppression effect, increases the Q value and roll-off steepness of the filter, simplifies the preparation process, and facilitates industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116667808B_ABST
    Figure CN116667808B_ABST
Patent Text Reader

Abstract

The present invention provides a temperature-compensated surface acoustic wave resonator and a preparation method thereof, and belongs to the technical field of TC-SAW filters. The present invention provides a temperature-compensated surface acoustic wave resonator, comprising a substrate layer, a forked electrode metal layer, a first temperature compensation layer, a suspended metal layer, and a second temperature compensation layer stacked in sequence, wherein the width of the suspended metal layer is 0.6 to 1 times the wavelength of the temperature-compensated surface acoustic wave resonator. The present invention utilizes the lateral structural change of the suspended metal layer, and the width of the suspended metal layer changes with the continuous wavelength change of the resonator apodization region. By changing the mass loading effect at the end of the forked electrode finger strip, a sound velocity difference is generated between the end region of the finger strip and the middle region, thereby forming a better clutter suppression effect, thereby improving the performance of the resonator and the filter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of TC-SAW filters, and in particular to a temperature-compensated surface acoustic wave resonator and a preparation method thereof. Background Art

[0002] Surface acoustic wave (SAW) filters have become an indispensable key component in radio frequency (RF) front-end applications due to their small size, good performance and low cost. In the 4G communication era, since the frequency of surface acoustic wave filters is greatly affected by the operating temperature, thin film bulk acoustic wave filters have gradually become the mainstream choice in the market. Considering the cost advantage of surface acoustic waves, temperature-compensated surface acoustic wave filters (TC-SAW) came into being, that is, thick SiO2 and other materials are made on the surface of conventional SAW devices as a temperature compensation layer. Since this temperature compensation layer forms a lower surface combined with metal fingers and a free upper surface, when the surface acoustic wave device is working, there will be noise propagating in the device, causing the bandwidth to narrow and the out-of-band suppression to have a bulge, which ultimately makes the device electrical performance poor. Therefore, it is necessary to suppress the noise.

[0003] The traditional method of suppressing clutter in temperature compensated surface acoustic wave filter (TC-SAW) is to adjust the duty factor at the end of the interdigitated electrode finger, the mass loading effect at the end of the finger, or to set a number of through holes or blind holes in the temperature compensation layer, such as Chinese patent CN114244304A. However, the above-mentioned clutter suppression methods all have certain limitations. For example, adjusting the duty factor at the end of the interdigitated electrode finger and setting a number of through holes or blind holes in the temperature compensation layer are limited by the accuracy of the lithography machine and have high requirements on the accuracy and stability of the process. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a temperature compensated surface acoustic wave resonator and a preparation method thereof. The temperature compensated surface acoustic wave resonator of the present invention forms a better clutter suppression effect by changing the lateral structure of the suspended metal layer, and the width of the suspended metal layer changes with the continuous wavelength of the resonator apodization area.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a temperature-compensated surface acoustic wave resonator, comprising a substrate layer, an interdigitated electrode metal layer, a first temperature compensation layer, a suspended metal layer and a second temperature compensation layer stacked in sequence, wherein the width of the suspended metal layer is 0.6 to 1 times the wavelength of the temperature-compensated surface acoustic wave resonator.

[0007] Preferably, the suspended metal layer is a single-layer suspended metal layer or a double-layer suspended metal layer.

[0008] Preferably, the material of the suspended metal layer includes one or more of copper, platinum, tantalum and tungsten.

[0009] Preferably, the single suspended metal layer is located vertically above the ends of the fingers of the interdigitated electrode metal layer.

[0010] Preferably, the single suspended metal layers vertically above the ends of adjacent fingers are connected by metal.

[0011] Preferably, the single-layer suspended metal layer is located vertically above the ends and front ends of the fingers of the interdigitated electrode metal layer, and the single-layer suspended metal layers vertically above adjacent fingers do not touch each other.

[0012] Preferably, the double-layer suspended metal layer is located vertically above the end and front end of the fingers of the interdigitated electrode metal layer, and the double-layer suspended metal layers vertically above adjacent fingers are in contact.

[0013] Preferably, the substrate layer is made of lithium niobate.

[0014] Preferably, the cutting angle of the lithium niobate is 128 degrees.

[0015] The present invention also provides a method for preparing the temperature-compensated surface acoustic wave resonator described in the above technical solution, comprising the following steps:

[0016] A lift-off process is used to grow an interdigital electrode metal layer on the surface of the substrate layer, a first temperature compensation layer is sputtered on the interdigital electrode metal layer, a suspended metal layer is formed on the first temperature compensation layer by a lift-off process, and a second temperature compensation layer is deposited on the suspended metal layer to obtain the temperature compensated surface acoustic wave resonator.

[0017] The present invention provides a temperature-compensated surface acoustic wave resonator, comprising a substrate layer, an interdigitated electrode metal layer, a first temperature compensation layer, a suspended metal layer and a second temperature compensation layer stacked in sequence, wherein the width of the suspended metal layer is 0.6 to 1 times the wavelength of the temperature-compensated surface acoustic wave resonator.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention utilizes the lateral structural change of the suspended metal layer. The width of the suspended metal layer changes with the continuous wavelength of the resonator's track change area. By changing the mass loading effect at the end of the interdigitated electrode finger strips, the width and thickness of the suspended metal layer are optimized to reduce the sound velocity in the end area of ​​the finger strips, so that a sound velocity difference is generated between the end area of ​​the finger strips and the middle area, forming a better clutter suppression effect, thereby improving the performance of the resonator.

[0020] Furthermore, the present invention limits the suspended metal layer to a single-layer suspended metal layer or a double-layer suspended metal layer. By changing the longitudinal structure of the suspended metal layer and adopting a double-layer suspended metal layer structure of the same material or different materials, the effect of suppressing clutter is further improved, so that the resonator obtains a higher Q value and the filter has a better roll-off steepness.

[0021] The present invention also provides a method for preparing the temperature-compensated surface acoustic wave resonator described in the above technical solution. The method of the present invention is simple and easy to realize industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic structural diagram of a temperature compensation type surface acoustic wave resonator in which the suspended metal layer is a single-layer suspended metal layer structure;

[0023] Figure 2 A schematic diagram of the structure of a temperature compensation surface acoustic wave resonator in which the suspended metal layer is a double-layer suspended metal layer structure;

[0024] Figure 3 It is a schematic diagram of a structure in which a single-layer suspended metal layer is located vertically above the ends of the fingers of the interdigitated electrode metal layer;

[0025] Figure 4 A top view showing a single suspended metal layer located vertically above and connected to the ends of the fingers of the interdigitated electrode metal layer;

[0026] Figure 5 A top view showing a single suspended metal layer located vertically above the ends and front ends of the fingers of the interdigitated electrode metal layer;

[0027] Figure 6 It is a schematic diagram of a structure in which a double-layer suspended metal layer is located vertically above the ends of the fingers of the interdigitated electrode metal layer;

[0028] Figure 7 A top view of a double-layer suspended metal layer located vertically above the end and front end of the fingers of the interdigitated electrode metal layer;

[0029] Figures 1 to 7 100 is a substrate layer, 110 is an interdigitated electrode metal layer, 120 is a first temperature compensation layer, 130 is a single-layer suspended metal layer, 140 is a double-layer suspended metal layer, and 150 is a second temperature compensation layer. DETAILED DESCRIPTION

[0030] The present invention provides a temperature-compensated surface acoustic wave resonator, comprising a substrate layer, an interdigitated electrode metal layer, a first temperature compensation layer, a suspended metal layer and a second temperature compensation layer stacked in sequence, wherein the width of the suspended metal layer is 0.6 to 1 times the wavelength of the temperature-compensated surface acoustic wave resonator.

[0031] In the present invention, the suspended metal layer is preferably a single-layer suspended metal layer or a double-layer suspended metal layer.

[0032] Figure 1 The schematic diagram of the structure of the temperature compensation surface acoustic wave resonator with a single-layer suspended metal layer is shown in FIG. Figure 2 The structure diagram of the temperature compensation type surface acoustic wave resonator with a double-layer suspended metal layer is shown below. Figure 1 and 2 Provide explanation.

[0033] The temperature-compensated surface acoustic wave resonator provided by the present invention includes a substrate layer 100 .

[0034] In the present invention, the material of the substrate layer 100 is preferably lithium niobate (abbreviated as LN).

[0035] In the present invention, the cutting angle of the lithium niobate is preferably 128 degrees.

[0036] In the present invention, the thickness of the substrate layer is preferably 350 or 200 μm.

[0037] The temperature-compensated surface acoustic wave resonator provided by the present invention includes an interdigital electrode metal layer 110 .

[0038] In the present invention, the material of the interdigitated electrode metal layer 110 preferably includes one or more of Ti, Cu and Ag. In a specific embodiment of the present invention, the interdigitated electrode metal layer 110 is preferably Ti / Cu or Ti / Ag / Cu, wherein the Ti / Cu refers to a stacked structure of titanium + copper, and the Ti / Ag / Cu refers to a stacked structure of titanium + silver + copper. The Ti / Cu and Ti / Ag / Cu can improve the power handling capacity of the resonator.

[0039] The temperature-compensated surface acoustic wave resonator provided by the present invention includes a first temperature compensation layer 120 .

[0040] In the present invention, the material of the first temperature compensation layer 120 is preferably silicon dioxide (SiO 2 ).

[0041] The temperature-compensated surface acoustic wave resonator provided by the present invention includes a suspended metal layer, and the width of the suspended metal layer is preferably 0.8 times the wavelength of the temperature-compensated surface acoustic wave resonator. The present invention preferably patterns the pattern of the suspended metal layer according to the design parameters of the resonator. According to different resonator design parameters, the width of the suspended metal layer changes accordingly.

[0042] The temperature-compensated surface acoustic wave resonator provided by the present invention preferably includes a single-layer suspended metal layer 130 .

[0043] In the present invention, the material of the suspended metal layer preferably includes one or more of copper, platinum, tantalum and tungsten.

[0044] In the present invention, the single-layer suspended metal layer 130 is preferably located vertically above the ends of the fingers of the interdigitated electrode metal layer, such as Figure 3 shown.

[0045] In the present invention, the single-layer suspended metal layer 130 vertically above the ends of the adjacent fingers is preferably connected by metal, and the metal connection is preferably achieved by the single-layer suspended metal layer 130, such as Figure 4 As shown, Figure 4 W1~W4 correspond to the width of the suspended metal layer at the end of the finger strip.

[0046] In the present invention, the single-layer suspended metal layer 130 is preferably located vertically above the end and front end of the finger of the interdigitated electrode metal layer, and the single-layer suspended metal layer 130 vertically above adjacent fingers does not touch, such as Figure 5 As shown, Figure 5 W1~W6 in the figure correspond to the width of the suspended metal layer at the end of the finger strip.

[0047] The temperature compensation surface acoustic wave resonator provided by the present invention preferably includes a double-layer suspended metal layer 140, and the structural schematic diagram is shown in FIG. Figure 6 As shown, the double-layer suspended metal layer 140 includes a first suspended metal layer and a second suspended metal layer which are stacked.

[0048] In the present invention, the width of the first suspended metal layer is preferably 0.8 times the wavelength and is continuous rather than a disconnected structure, and the width of the second suspended metal layer is preferably less than 0.8 times the wavelength, and its main function is to adjust the mass loading effect at the end of the finger.

[0049] In the present invention, the double-layer suspended metal layer 140 is preferably located vertically above the end and front end of the fingers of the interdigitated electrode metal layer, and the double-layer suspended metal layer 140 vertically above adjacent fingers is in contact, such as Figure 7 As shown, Figure 7 W1~W6 in the figure correspond to the width of the suspended metal layer at the end of the finger strip.

[0050] In the present invention, the widths of the first suspended metal layer and the second suspended metal layer of the double suspended metal layer 140 are preferably the same.

[0051] In the present invention, the materials of the first suspension metal layer and the second suspension metal layer of the double-layer suspension metal layer 140 are independently preferably one or more of copper, platinum, tantalum and tungsten.

[0052] The temperature-compensated surface acoustic wave resonator provided by the present invention includes a second temperature compensation layer 150 .

[0053] In the present invention, the material of the second temperature compensation layer 150 is preferably silicon dioxide (SiO 2 ).

[0054] The present invention also provides a method for preparing the temperature-compensated surface acoustic wave resonator described in the above technical solution, comprising the following steps:

[0055] A lift-off process is used to grow an interdigitated electrode metal layer 110 on the surface of the substrate layer 100, a first temperature compensation layer 120 is sputtered on the interdigitated electrode metal layer 110, a suspended metal layer is formed on the first temperature compensation layer by a lift-off process, and a second temperature compensation layer 150 is deposited on the suspended metal layer to obtain the temperature compensated surface acoustic wave resonator.

[0056] The present invention has no particular limitation on the specific methods of the lift-off process, sputtering and deposition, and methods familiar to those skilled in the art may be used.

[0057] In the present invention, the deposition preferably includes CVD (Chemical Vapor Deposition) and / or PVD (Physical Vapor Deposition).

[0058] After obtaining the second temperature compensation layer 150 , the present invention preferably performs surface planarization polishing to obtain the temperature compensation type surface acoustic wave resonator.

[0059] In the present invention, the surface planarization polishing is preferably chemical mechanical polishing (CMP), preferably chemical mechanical polishing until the in-plane consistency is within ±150 nm.

[0060] In order to further illustrate the present invention, the temperature-compensated surface acoustic wave resonator and the preparation method thereof provided by the present invention are described in detail below in conjunction with examples, but they should not be construed as limiting the protection scope of the present invention.

[0061] Example 1

[0062] Step 1: Using lithium niobate (LN) with a cutting angle of 128 degrees as the substrate layer 100 material;

[0063] Step 2: growing the interdigital electrode metal layer 110 on the substrate layer 100 by using a lift-off process, the material of which is Ti / Cu;

[0064] Step 3: Sputtering and growing silicon dioxide on the interdigital electrode metal layer 110 as the first temperature compensation layer 120;

[0065] Step 4: A single-layer suspended metal layer 130 is formed on the first temperature compensation layer 120 by a lift-off process. The material is copper. The single-layer suspended metal layer 130 is located vertically above the ends of the fingers of the interdigitated electrode metal layer. The single-layer suspended metal layers 130 vertically above the ends of adjacent fingers are connected. Figure 4 As shown, Figure 4 W1~W4 in the middle correspond to the width of the suspended metal layer at the end of the finger strip;

[0066] Step 5: Chemical vapor deposition of silicon dioxide as the second temperature compensation layer 150 is performed on the single-layer suspension metal layer 130 and chemical mechanical polishing is performed to make the surface flat.

[0067] Example 2

[0068] Step 1: Using lithium niobate (LN) with a cutting angle of 128 degrees as the substrate layer 100 material;

[0069] Step 2: growing the interdigital electrode metal layer 110 on the substrate layer 100 by using a lift-off process, the material of which is Ti / Cu;

[0070] Step 3: Sputtering and growing silicon dioxide on the interdigital electrode metal layer 110 as the first temperature compensation layer 120;

[0071] Step 4: A single-layer suspended metal layer 130 is formed on the first temperature compensation layer 120 by a lift-off process. The material is copper. The single-layer suspended metal layer 130 is located vertically above the end and front end of the finger of the interdigitated electrode metal layer, and the single-layer suspended metal layer vertically above adjacent fingers does not touch each other. Figure 5 As shown, Figure 5 W1~W6 in the middle correspond to the width of the suspended metal layer at the end of the finger strip;

[0072] Step 5: Chemical vapor deposition of silicon dioxide as the second temperature compensation layer 150 is performed on the single-layer suspension metal layer 130 and chemical mechanical polishing is performed to make the surface flat.

[0073] Example 3

[0074] Step 1: Using lithium niobate (LN) with a cutting angle of 128 degrees as the substrate layer 100 material;

[0075] Step 2: growing the interdigital electrode metal layer 110 on the substrate layer 100 by using a lift-off process, the material of which is Ti / Cu;

[0076] Step 3: Sputtering and growing silicon dioxide on the interdigital electrode metal layer 110 as the first temperature compensation layer 120;

[0077] Step 4: A double-layer suspended metal layer 140 is formed on the first temperature compensation layer 120 by a lift-off process. The material is copper. The double-layer suspended metal layer 140 is located vertically above the end and front end of the finger electrode metal layer, and the double-layer suspended metal layer 140 vertically above adjacent finger strips is connected, such as Figure 7 As shown, Figure 7 W1~W6 in the middle correspond to the width of the suspended metal layer at the end of the finger strip;

[0078] Step 5: Chemical vapor deposition of silicon dioxide as the second temperature compensation layer 150 is performed on the single-layer suspension metal layer 130 and chemical mechanical polishing is performed to make the surface flat.

[0079] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A temperature-compensated surface acoustic wave resonator, characterized in that: Specifically, it comprises a substrate layer, an interdigitated electrode metal layer, a first temperature compensation layer, a suspended metal layer, and a second temperature compensation layer which are stacked in sequence; The suspended metal layer is a double-layer suspended metal layer; The double-layer suspended metal layer is located vertically above the end and front end of the fingers of the interdigitated electrode metal layer, and the double-layer suspended metal layers vertically above adjacent fingers are in contact; The double-layer suspended metal layer includes a first suspended metal layer and a second suspended metal layer which are stacked; the width of the first suspended metal layer is 0.8 times the wavelength and is continuous rather than a disconnected structure, and the width of the second suspended metal layer is less than 0.8 times the wavelength and greater than or equal to 0.6 times the wavelength; The material of the suspended metal layer includes one or more of copper, platinum, tantalum and tungsten; The thickness of the substrate layer is 350 μm or 200 μm.

2. The temperature-compensated surface acoustic wave resonator according to claim 1, characterized in that: The material of the substrate layer is lithium niobate.

3. The temperature-compensated surface acoustic wave resonator according to claim 2, characterized in that: The cutting angle of the lithium niobate is 128 degrees.

4. A method for preparing a temperature-compensated surface acoustic wave resonator according to any one of claims 1 to 3, characterized in that: The following steps are involved: A lift-off process is used to grow an interdigital electrode metal layer on the surface of the substrate layer, a first temperature compensation layer is sputtered on the interdigital electrode metal layer, a suspended metal layer is formed on the first temperature compensation layer by a lift-off process, and a second temperature compensation layer is deposited on the suspended metal layer to obtain the temperature compensated surface acoustic wave resonator.