Toughening agent with self-assembled nano-scale anti-epoxy resin cracking and preparation method thereof

By using liquid polybutadiene and SBS block copolymer in epoxy resin to construct an emulsion system, a self-assembled nano-scale toughening agent is formed, which solves the problem of insufficient toughness after curing of epoxy resin and achieves efficient toughening effect and light colors, suitable for mass production.

CN116694025BActive Publication Date: 2024-11-01EVERSUN POLYCARBON SCI&TECH CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310795985.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-01
Publication Date
2024-11-01
Estimated Expiration
2043-07-01

AI Technical Summary

Technical Problem

The three-dimensional mesh structure formed after curing of epoxy resin leads to its low impact strength, low peeling strength, poor fatigue resistance, and easy cracking. The existing toughening agent usually loses the bending strength and bending modulus while increasing the impact strength, or This results in the product color not suitable for widespread applications.

Method used

The emulsion system is constructed under the action of organic solvents and emulsifiers by using liquid polybutadiene and SBS block copolymers. The reaction is promoted by catalysts to form epoxidized liquid polybutadiene and epoxidized SBS block copolymers, and self-assembled into The nanoparticles are compatible with the epoxy resin to form a toughener to achieve toughening of the epoxy resin, while controlling the reaction conditions to maintain low viscosity and high solids content to ensure production efficiency and cost.

Benefits of technology

The impact strength and fracture toughness of epoxy resin are significantly improved, while maintaining the light color and the amount of toughening agent added is low, which can significantly improve the performance of epoxy resin cured products and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116694025B_ABST
    Figure CN116694025B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of epoxy resin toughening agents, and in particular to a toughening agent with self-assembled nano-level anti-epoxy resin cracking and a preparation method thereof. The toughening agent comprises the following materials: a solvent, an emulsifier, a liquid polybutadiene, an SBS block copolymer, a catalyst, an epoxidizing agent, an epoxy resin and water. Constructing an emulsion system under the action of an organic solvent and an emulsifier is conducive to maintaining the reaction process under a low viscosity condition and is conducive to increasing the solid content of the emulsified system to more than 35%; the obtained epoxidized liquid polybutadiene and epoxidized SBS block copolymer are completely compatible with epoxy resin, and the formed toughening agent is used for epoxy resin toughening modification, and the addition amount is low. When the epoxy resin curing reaction occurs, the epoxidized liquid polybutadiene and the epoxidized SBS self-assemble into nanoparticles and disperse in the epoxy resin system, which play a toughening role, and the formed epoxy resin cured product has strong impact strength and fracture toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy resin toughening agents, and in particular to a toughening agent with self-assembled nano-level anti-epoxy resin cracking function and a preparation method thereof. Background Art

[0002] Epoxy resin refers to a polymer compound with two or more epoxy groups in the molecule and aliphatic, alicyclic or aromatic chain segments as the skeleton. Under appropriate curing conditions, such as amine, imidazole, anhydride or phenolic resin, it can form a three-dimensional cross-linked network of cured polymers. After curing, epoxy resin has a high cross-linking density and high strength. It has a wide range of uses in many fields, such as carbon fiber composite materials, PCB copper-clad boards, wind turbine blades, adhesives for strengthening bridge structures, LED encapsulation glue, potting glue, epoxy floor paint, anti-corrosion paint and automotive primer, etc.

[0003] However, since epoxy resin forms a three-dimensional network structure macromolecule after curing, the movement of the molecular main chain is restricted, the internal stress is large, and it is easy to become brittle, resulting in low impact strength, low peel strength, poor fatigue resistance, low fracture toughness coefficient, and easy cracking of epoxy resin.

[0004] In order to solve the above-mentioned problems existing in epoxy resin, a toughening agent is usually added to the epoxy resin system to improve the toughness of the epoxy resin cured product.

[0005] At present, the main toughening methods include adding rubber elastomers, thermotropic liquid crystal polymers, inorganic nanoparticles, core-shell polymer toughening, etc., mainly by adjusting the crosslinking density of epoxy resin to achieve toughening. Existing epoxidized SBS is applied to epoxy resin system, and the impact strength of epoxy resin cured product can be improved by 3-4 times when 1phr is added, but the organic solvent system used in the process, the solid content of SBS is relatively low, and gel is easily generated in the epoxidation process. The patent publication number is CN 104725782A, which is a combination of one or more toughening modified epoxy resins using carboxyl nitrile elastic nanoparticles, nitrile elastic nanoparticles, carboxyl styrene elastic nanoparticles, styrene-butadiene elastic nanoparticles, while improving the impact strength, but the bending strength and bending modulus are lost. The patent publication number is CN 107698733 A, which is a scheme using synthetic polyurethane modified epoxy resin, which is usually formed by using polyurethane and epoxy resin to form an interpenetrating network polymer, increasing the toughness of the system, but the elastic modulus of the material is generally lost and the color of the modified object is darker. The scheme of patent publication number CN 103396536 A is to synthesize toughening agent by the method of polyester polyol, and apply it to epoxy resin and anhydride curing system, which improves the flexibility of epoxy resin, but the hydroxyl in polyester polyol has low reaction activity with epoxy resin, and the color of the product is brown, which is not conducive to wide application. The scheme of patent publication number CN115160515A is to use monomer polyethylene glycol methyl ether methacrylate and monomer biphenyl liquid crystal monomer block copolymer to toughen epoxy resin, and use the different solubility of two blocks in epoxy resin to produce microscopic phase separation, improve impact resistance, but the prepared copolymer lacks reactive functional groups and is prone to macroscopic phase separation. The scheme of patent publication number CN 107383366A is to prepare polyamide curing agent to cure epoxy resin, which is usually an effective method to improve the toughness of epoxy resin, but the color of the cured product is too dark and not suitable for wide application.Existing literature [(Guo Qipeng, Wang Ke, Chen Ling, et al. Phase behavior, crystallization, and nanostructures in thermoset blends of epoxy resin and amphiphilic star-shaped block copolymers [J]. Journal of Polymer Science: Part B. Polymer Physics, 2006, 44 (6): 975-985)] discloses a toughened epoxy resin, which utilizes the solubility characteristics of polypropylene oxide (PPO) and polyethylene oxide (PEO) in epoxy resin and selects polyether toughened epoxy resin formed by block copolymerization of the two. Since the polyether precipitates to form a dispersed phase during the resin curing process, it also shows a good toughening effect. However, the modified product has not yet formed a chemical bond with the epoxy resin substrate, but is only combined with the epoxy resin substrate by secondary bonds, so the toughening effect is limited. Summary of the invention

[0006] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a self-assembled nano-scale toughening agent for preventing epoxy resin cracking, which has a controllable structure and a small addition ratio, and participates in the epoxy resin curing reaction. During the curing process, the toughening agent can self-assemble to form nano-scale particles and be evenly dispersed in the epoxy resin system, thereby achieving the purpose of toughening the epoxy resin, and at the same time has the characteristic of light color after curing.

[0007] Another object of the present invention is to provide a method for preparing a self-assembled nano-scale toughening agent for preventing epoxy resin cracking. The method has simple operation, convenient control, high production efficiency, low production cost, and can be used for large-scale production.

[0008] The purpose of the present invention is achieved by the following technical solution: A self-assembled nano-scale toughening agent for preventing epoxy resin cracking, comprising the following materials in parts by weight:

[0009]

[0010] The self-assembled nano-scale toughening agent for preventing epoxy resin cracking of the present invention uses liquid polybutadiene and SBS block copolymer as main reaction raw materials, constructs an emulsion system under the action of an organic solvent and an emulsifier, is conducive to maintaining a reaction process under a relatively low viscosity condition, avoids the influence of high viscosity of a traditional solvent system on heat transfer, mass transfer and transmission, and is conducive to increasing the solid content of the emulsified system to more than 20% or even more than 35%. Under the action of a catalyst, the liquid polybutadiene and the SBS block copolymer react with an epoxidizing agent to obtain epoxidized liquid polybutadiene and epoxidized SBS block copolymer, which are completely compatible with epoxy resin. When the formed toughening agent is used for toughening and modification of epoxy resin, the addition amount is low. When the epoxy resin curing reaction occurs, the epoxidized liquid polybutadiene and the epoxidized SBS self-assemble into nanoparticles and are dispersed in the epoxy resin system to play a toughening role. The formed epoxy resin cured product has relatively strong impact strength and fracture toughness. Moreover, polybutadiene has a high double bond content, which can regulate the double bond content in the PB+SBS system, thereby regulating the content of epoxy groups after epoxidation.

[0011] Preferably, the organic solvent is a non-polar solvent with a boiling point of 60-120°C.

[0012] More preferably, the organic solvent is at least one of cyclohexane, 120# solvent, benzene and toluene.

[0013] Preferably, the HLB value of the emulsifier is 8-14.

[0014] More preferably, the emulsifier is at least one of OP-10, NP-9, SDS, SDBS, isomeric tridecanol polyoxyethylene ether and tritonX-100.

[0015] Preferably, the number average molecular weight of the liquid polybutadiene is 1000-100000; the number average molecular weight of the SBS block copolymer is 1000-200000.

[0016] Preferably, the catalyst is phosphotungstic heteropoly acid.

[0017] More preferably, the preparation method of the phosphotungstic heteropoly acid comprises the following steps:

[0018] (R1), take tungstic acid, hydrogen peroxide, phosphoric acid, and methyl trioctyl ammonium chloride-dichloromethane solution and set aside;

[0019] (R2), stir tungstic acid and hydrogen peroxide at 60-70°C until the solution changes from yellow to colorless, and filter and take the filtrate;

[0020] (R3) Add phosphoric acid to the filtrate and stir for 10-20 minutes, then drop methyl trioctyl ammonium chloride-dichloromethane solution, continue stirring for 3-8 minutes, then stand to separate the layers, take the lower layer solution and distill under reduced pressure at 45°C to obtain a phosphotungstic heteropoly acid catalyst.

[0021] The catalyst prepared by adopting the above technical scheme is a peroxide phosphotungstic heteropoly acid phase transfer catalyst, which is a colorless transparent viscous body. In the process of producing toughening agent, it is the key to the epoxidation of liquid polybutadiene and SBS block copolymer, and can be recycled and reused. Furthermore, the weight ratio of each part of tungstic acid, hydrogen peroxide, phosphoric acid, and methyl trioctyl ammonium chloride-dichloromethane solution is 6-8:30-40:1-3:120-150. In the methyl trioctyl ammonium chloride-dichloromethane solution, the mass concentration of methyl trioctyl ammonium chloride is 3-5%; the mass concentration of hydrogen peroxide is 30%, and the mass volume concentration of phosphoric acid is 40%.

[0022] Preferably, the epoxidizing agent is hydrogen peroxide; and the epoxy resin is bisphenol A epoxy resin.

[0023] Another object of the present invention is achieved by the following technical solution: The preparation method of the above-mentioned toughening agent with self-assembled nano-scale anti-epoxy resin cracking comprises the following steps:

[0024] (S1), taking a solvent, an emulsifier, a liquid polybutadiene, an SBS block copolymer, a catalyst, an epoxidizing agent, an epoxy resin and water according to weight parts for later use;

[0025] (S2), adding liquid polybutadiene and SBS block copolymer to a portion of the organic solvent, heating to 60-80° C. and stirring to dissolve, to obtain a solution;

[0026] (S3), after the dissolved liquid is cooled, an emulsifier and water are added, and emulsified at a rotation speed of 300-800 rpm to form an emulsion;

[0027] (S4), adding a catalyst to the emulsion, raising the temperature to 50-90° C., adding an epoxidizing agent dropwise for 1-6 hours, keeping the temperature for 1-3 hours, and cooling to obtain a reaction product;

[0028] (S5), adding the remaining organic solvent to the reaction product, standing to separate the layers, taking the upper organic phase, washing it with water for multiple times, adding epoxy resin, and distilling it under normal pressure to obtain a toughening agent with self-assembled nano-scale anti-epoxy resin cracking.

[0029] Among them, adding the remaining organic solvent to the reaction product is beneficial to adjusting the density of the organic phase.

[0030] The beneficial effects of the present invention are:

[0031] (1) The present invention has a self-assembled nano-scale toughening agent for preventing epoxy resin cracking. The preparation process uses an emulsion system to achieve epoxidation, which reduces the viscosity of the reaction system. The viscosity of the emulsified system is less than 100 cp (25° C.), while under the same conditions, if a pure solvent system is used, the viscosity is as high as thousands of centipoises;

[0032] (2) The present invention has a self-assembled nano-scale toughening agent for preventing epoxy resin cracking. The solid content of the emulsified system can be above 35%, and the viscosity is not large, which does not affect the heat transfer, mass transfer and transmission of the system. However, the solvent system can only reach a maximum of 20%, and the viscosity is too high to be produced;

[0033] (3) An emulsion system was constructed during the preparation of the toughening agent, and the epoxidation reaction occurred at the oil-water interface, which was beneficial for controlling side reactions such as the ring opening of the epoxy group;

[0034] (4) Both the liquid polybutadiene and the SBS block copolymer react with an epoxidizing agent to obtain epoxidized liquid polybutadiene and epoxidized SBS block copolymers, which are completely compatible with epoxy resins. When the epoxy resin curing reaction occurs, the epoxidized liquid polybutadiene and epoxidized SBS self-assemble into nanoparticles and disperse in the epoxy resin system, playing a toughening role;

[0035] (5) During the preparation of the toughening agent, the catalyst can be recovered and reused;

[0036] (6) The amount of toughening agent added to epoxy resin modification is low, and 1phr can significantly improve the impact strength and fracture toughness of epoxy resin cured products. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic diagram of the epoxidation reaction of liquid polybutadiene and SBS block copolymer in Example 1 of the present invention;

[0038] Figure 2 is a transmission electron micrograph of an ultrathin section of a modified epoxy resin cured product obtained by applying the toughening agent of Example 1 to epoxy resin;

[0039] Figure 3 This is a scanning electron micrograph of the fracture surface of a modified epoxy resin cured product obtained by applying the toughening agent of Example 1 to epoxy resin. DETAILED DESCRIPTION

[0040] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments and drawings. The contents mentioned in the implementation modes are not intended to limit the present invention.

[0041] Example 1

[0042] Preparation of catalyst: 7.56g tungstic acid and 35ml hydrogen peroxide (mass concentration 30%) were stirred at 65°C until the solution changed from yellow to colorless, filtered, 1.9ml phosphoric acid aqueous solution (mass volume concentration 40%) was added to the filtrate, stirred for 15 minutes, and 132g methyl trioctyl ammonium chloride (mass concentration 3.8%) dichloromethane solution was added dropwise, stirred for 5 minutes, and allowed to stand for stratification. The lower layer solution was removed and subjected to reduced pressure distillation at 45°C to obtain a peroxide tungstic phosphotungstic heteropoly acid phase transfer catalyst.

[0043] In a 1000 ml reactor equipped with a condenser, a stirrer and a temperature control device, 155.5 g of toluene and 38.9 g of a cyclohexane mixed solvent were added, followed by 168 g of liquid polybutadiene and 42 g of a thermoplastic elastomer SBS792, heated to 65° C., stirred for 1 hour to form a viscous liquid; then 9 g of NP-9 surfactant and 3 g of sodium dodecyl sulfate SDS were added, stirred well, and cooled to room temperature, 159 g of deionized water was added, and the speed was adjusted to 600 rpm until a white emulsion was formed; then 2.4 g of a catalyst was added, and then the temperature was raised to 60° C., and 25 g of a hydrogen peroxide solution with a mass concentration of 4.8% was added dropwise by a peristaltic pump, and the addition was continued for 2 hours, and the reaction was kept warm for 2 hours. The reaction process was as follows: Figure 1 As shown, the temperature was lowered to room temperature; 144 g of toluene and 36 g of cyclohexane mixture was added to the reactor, stirred thoroughly, allowed to stand for stratification, and the aqueous phase was recovered by filtration. The upper organic phase was washed with water three times, 30 g of water each time, and then 840 g of 128 epoxy resin was added, and the solvent was removed by atmospheric distillation to obtain a self-assembled nano-scale anti-epoxy resin cracking toughening agent with a solid content of 20%.

[0044] Example 2

[0045] Preparation of catalyst: 7.56g tungstic acid and 35ml hydrogen peroxide (mass concentration 30%) were stirred at 65°C until the solution changed from yellow to colorless, filtered, 1.9ml phosphoric acid aqueous solution (mass volume concentration 40%) was added to the filtrate, stirred for 15 minutes, and 132g methyl trioctyl ammonium chloride (mass concentration 3.8%) dichloromethane solution was added dropwise, stirred for 5 minutes, and allowed to stand for stratification. The lower layer solution was removed and subjected to reduced pressure distillation at 45°C to obtain a peroxide tungstic phosphotungstic heteropoly acid phase transfer catalyst.

[0046] A 1000ml reactor equipped with a condenser, a stirrer and a temperature control device was added with a mixed solvent of 145.8g toluene and 48.6g cyclohexane, followed by 168g liquid polybutadiene and 42g thermoplastic elastomer SBS792, heated to 65°C, stirred for 1 hour to form a viscous liquid; then 9g NP-9 surfactant and 3g sodium dodecyl sulfate SDS were added, stirred evenly and cooled to room temperature, 159g deionized water was added, the speed was adjusted to 600 rpm, until a white emulsion was formed; then 2.4g catalyst was added, the temperature was raised to 60°C, 25g of a 4.8% hydrogen peroxide solution was dripped by a peristaltic pump, dripped for 2 hours, kept warm for reaction for 2 hours, and cooled to room temperature; then 145.8g toluene and 48.6g cyclohexane mixed solution were added to the reactor, stirred thoroughly, allowed to stand for stratification, and filtered to recover the water phase. The upper organic phase was washed with water three times, 30 g of water each time, and then 840 g of 128 epoxy resin was added, and the solvent was removed by atmospheric distillation to obtain a toughening agent with a solid content of 20% and having self-assembled nano-scale anti-epoxy resin cracking properties.

[0047] Example 3

[0048] Preparation of catalyst: 7.56g tungstic acid and 35ml hydrogen peroxide (mass concentration 30%) were stirred at 65°C until the solution changed from yellow to colorless, filtered, 1.9ml phosphoric acid aqueous solution (mass volume concentration 40%) was added to the filtrate, stirred for 15 minutes, and 132g methyl trioctyl ammonium chloride (mass concentration 3.8%) dichloromethane solution was added dropwise, stirred for 5 minutes, and allowed to stand for stratification. The lower layer solution was removed and subjected to reduced pressure distillation at 45°C to obtain a peroxide tungstic phosphotungstic heteropoly acid phase transfer catalyst.

[0049] A 1000ml reactor equipped with a condenser, a stirrer and a temperature control device was added with 145.8g of toluene and 48.6g of a cyclohexane mixed solvent, followed by 150g of liquid polybutadiene and 60g of a thermoplastic elastomer SBS791, heated to 65°C, stirred for 1 hour to form a viscous liquid; then 9g of an OP-10 surfactant and 3g of sodium dodecyl sulfate SDS were added, stirred evenly, and then cooled to room temperature, 159g of deionized water was added, and the speed was adjusted to 600 rpm until a white emulsion was formed; 2.4g of a catalyst was added, and then the temperature was raised to 60°C, and 25g of a hydrogen peroxide solution with a mass concentration of 4.8% was dripped through a peristaltic pump, dripped for 2 hours, kept warm for reaction for 2 hours, and cooled to room temperature; 145.8g of a mixed solution of toluene and 48.6g of cyclohexane was added to the reactor, stirred sufficiently, allowed to stand for stratification, and filtered to recover the water phase. The upper organic phase was washed with water three times, 30 g of water each time, and then 840 g of E51 epoxy resin was added. The solvent was removed by atmospheric distillation to obtain a toughening agent with a solid content of 20% and having self-assembled nano-scale anti-epoxy resin cracking properties.

[0050] Example 4

[0051] Preparation of catalyst: 7.56g tungstic acid and 35ml hydrogen peroxide (mass concentration 30%) were stirred at 65°C until the solution changed from yellow to colorless, filtered, 1.9ml phosphoric acid aqueous solution (mass volume concentration 40%) was added to the filtrate, stirred for 15 minutes, and 132g methyl trioctyl ammonium chloride (mass concentration 3.8%) dichloromethane solution was added dropwise, stirred for 5 minutes, and allowed to stand for stratification. The lower layer solution was removed and subjected to reduced pressure distillation at 45°C to obtain a peroxide tungstic phosphotungstic heteropoly acid phase transfer catalyst.

[0052] A 1000ml reactor equipped with a condenser, a stirrer and a temperature control device is provided with a mixed solvent of 145.8g toluene and 48.6g cyclohexane, followed by 168g liquid polybutadiene and 42g thermoplastic elastomer SBS792, which are heated to 65°C and stirred for 1 hour to form a viscous liquid; 9g isomeric tridecanol polyoxyethylene ether surfactant and 3g sodium dodecylbenzene sulfonate SDBS are then added, stirred evenly and then cooled to room temperature, 159g deionized water is added, the speed is adjusted to 600 rpm, until a white emulsion is formed; 2.4g of a catalyst is then added, the temperature is then raised to 70°C, 25g of a hydrogen peroxide solution with a mass concentration of 4.8% is dripped through a peristaltic pump, the temperature is dripped for 2 hours, the temperature is kept for reaction for 2 hours, and the temperature is cooled to room temperature; 145.8g toluene and 48.6g cyclohexane mixed solution are then added to the reactor, stirred sufficiently, allowed to stand for stratification, and the aqueous phase is filtered and recovered. The upper organic phase was washed with water three times, 30 g of water each time, and then 840 g of 128 epoxy resin was added, and the solvent was removed by atmospheric distillation to obtain a toughening agent with a solid content of 20% and having self-assembled nano-scale anti-epoxy resin cracking properties.

[0053] Example 5

[0054] Preparation of catalyst: 7.56g tungstic acid and 35ml hydrogen peroxide (mass concentration 30%) were stirred at 65°C until the solution changed from yellow to colorless, filtered, 1.9ml phosphoric acid aqueous solution (mass volume concentration 40%) was added to the filtrate, stirred for 15 minutes, and 132g methyl trioctyl ammonium chloride (mass concentration 3.8%) dichloromethane solution was added dropwise, stirred for 5 minutes, and allowed to stand for stratification. The lower layer solution was removed and subjected to reduced pressure distillation at 45°C to obtain a peroxide tungstic phosphotungstic heteropoly acid phase transfer catalyst.

[0055] A 1000ml reactor equipped with a condenser, a stirrer and a temperature control device was added with 145.8g of toluene and 48.6g of a cyclohexane mixed solvent, followed by 168g of liquid polybutadiene and 42g of a thermoplastic elastomer SBS791, heated to 75°C, stirred for 1 hour to form a viscous liquid; then 9g of NP-9 surfactant and 3g of sodium dodecyl sulfate SDS were added, stirred evenly, and then cooled to room temperature, 159g of deionized water was added, and the speed was adjusted to 600 rpm until a white emulsion was formed; 2.4g of a catalyst was added, and then the temperature was raised to 80°C, and 25g of a hydrogen peroxide solution with a mass concentration of 4.8% was dripped through a peristaltic pump, dripped for 2 hours, kept warm for reaction for 1 hour, and cooled to room temperature; 145.8g of a mixed solution of toluene and 48.6g of cyclohexane was added to the reactor, stirred thoroughly, allowed to stand for stratification, and filtered to recover the water phase. The upper organic phase was washed with water three times, 30 g of water each time, and then 840 g of 828 epoxy resin was added, and the solvent was removed by atmospheric distillation to obtain a self-assembled nano-scale toughening agent for preventing epoxy resin cracking with a solid content of 20%.

[0056] Comparative Example 1

[0057] A toughening agent is a long-chain aliphatic compound CMP-410 containing polypropylene glycol diglycidyl ester.

[0058] Comparative Example 2

[0059] The difference between this comparative example and Example 1 is:

[0060] A 1000ml reactor equipped with a condenser, a stirrer and a temperature control device was added with 155.5g of toluene and 38.9g of a cyclohexane mixed solvent, followed by 168g of liquid polybutadiene and 42g of a thermoplastic elastomer SBS792, heated to 65°C, stirred for 1 hour to form a viscous liquid; then 9g of NP-9 surfactant and 3g of sodium dodecyl sulfate SDS were added, stirred evenly, and then cooled to room temperature, 159g of deionized water was added, and the speed was adjusted to 600 rpm until a white emulsion was formed; then the temperature was raised to 60°C, 25g of a 4.8% hydrogen peroxide solution was added dropwise by a peristaltic pump, added dropwise for 2 hours, kept warm for 2 hours, and cooled to room temperature; then 144g of toluene and 36g of a cyclohexane mixed solution were added to the reactor, stirred thoroughly, allowed to stand for stratification, and filtered to recover the water phase. The upper organic phase was washed with water three times, 30 g of water each time, and then 840 g of 128 epoxy resin was added, and the solvent was removed by atmospheric distillation to obtain a toughening agent.

[0061] Example 6

[0062] Application of toughening agent in toughening modification of epoxy resin:

[0063] The preparation method of the modified epoxy resin cured product comprises the following steps: taking 5 parts by weight of a toughening agent, adding 95 parts by weight of an E51 epoxy resin, stirring evenly, adding a DDM curing agent (the stoichiometric ratio of epoxy groups to active hydrogen is 1), and after complete dissolution, vacuum degassing to obtain a modified epoxy resin;

[0064] Pour the modified epoxy resin into a silicone mold, heat and cure it, and cool it to room temperature to obtain a modified epoxy resin cured product;

[0065] The curing conditions are as follows: heating to 50°C and keeping the temperature for 2 hours, then heating to 80°C and keeping the temperature for 3 hours, and then heating to 140°C and keeping the temperature for 3 hours.

[0066] Performance Testing:

[0067] I. Take the toughening agent of Example 1, and prepare a modified epoxy resin cured product according to the preparation method of Example 6, and then perform transmission electron microscopy test and fracture scanning electron microscopy test on it. The test results are as follows: Figure 2 and Figure 3 shown by Figure 2 It can be seen that the epoxidized liquid polybutadiene and epoxidized SBS self-assemble into nanoparticles dispersed in the modified epoxy resin cured product. Figure 3 It can be seen that in the scanning electron microscope image of the fracture of the modified epoxy resin cured product, the fracture showed a ductile fracture phenomenon, proving that the toughening agent in Example 1 played a toughening role.

[0068] II. Preparation of samples of epoxy resin cured products and testing of mechanical properties:

[0069] Preparation of the control group: 95 parts by weight of E51 epoxy resin was added with DDM curing agent (the ratio of epoxy group to active hydrogen was 1), mixed well, heated and cured, and cooled to room temperature to obtain epoxy resin cured product;

[0070] The curing conditions are as follows: heating to 50°C and keeping the temperature for 2 hours, then heating to 80°C and keeping the temperature for 3 hours, and then heating to 140°C and keeping the temperature for 3 hours.

[0071] Preparation of experimental group 1-5 and comparative group 1-2: Take the toughening agents of Examples 1-5 and Comparative Examples 1-2, and prepare the modified epoxy resin cured product by the preparation method of Example 6 above.

[0072] The mechanical properties of the samples in the experimental groups 1-5, the comparative groups 1-2 and the control group were tested, and the test results are shown in Table 1:

[0073] Table 1

[0074]

[0075] As shown in Table 1 above, the impact strength and fracture toughness of the modified epoxy resin cured products of the experimental groups 1-5 are greatly improved compared with the control group, and the toughening effect is better than that of the comparative groups 1 and 2. In the case of the toughening agent in the comparative group 2 without the addition of phosphotungstic heteropoly acid, the overall mechanical properties of the epoxy cured product are reduced, the epoxidation degree of the toughening agent is low, the compatibility with the epoxy resin is poor, and the toughening effect is limited.

[0076] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A self-assembled nano-scale toughening agent for preventing epoxy resin from cracking. It is characterized in that The composition comprises the following materials in parts by weight: The organic solvent is at least one of cyclohexane, 120# solvent, benzene and toluene; The emulsifier is at least one of OP-10, NP-9, SDS, SDBS, isomeric tridecanol polyoxyethylene ether and triton X-100; The number average molecular weight of the liquid polybutadiene is 1000-100000; the number average molecular weight of the SBS block copolymer is 1000-200000.

2. The toughening agent having self-assembled nano-scale anti-epoxy resin cracking according to claim 1, Features: The catalyst is phosphotungstic heteropoly acid.

3. The toughening agent having self-assembled nano-scale anti-epoxy resin cracking according to claim 2, Features: The preparation method of the phosphotungstic heteropoly acid comprises the following steps: (R1), taking tungstic acid, hydrogen peroxide, phosphoric acid, and methyl trioctyl ammonium chloride-dichloromethane solution and setting aside; (R2), stirring tungstic acid and hydrogen peroxide at 60-70°C until the solution changes from yellow to colorless, filtering and taking the filtrate; (R3) Add phosphoric acid to the filtrate and stir for 10-20 minutes, then drop methyl trioctyl ammonium chloride-dichloromethane solution, continue stirring for 3-8 minutes, then stand to separate the layers, take the lower layer solution and distill under reduced pressure at 45°C to obtain a phosphotungstic heteropoly acid catalyst.

4. The toughening agent having self-assembled nano-scale anti-epoxy resin cracking according to claim 1, Features: The epoxidizing agent is hydrogen peroxide; and the epoxy resin is bisphenol A epoxy resin.

5. A method for preparing a toughening agent having self-assembled nano-scale anti-epoxy resin cracking as claimed in any one of claims 1 to 4, It is characterized in that The steps include: (S1), taking a solvent, an emulsifier, a liquid polybutadiene, an SBS block copolymer, a catalyst, an epoxidizing agent, an epoxy resin and water according to weight parts for later use; (S2), adding liquid polybutadiene and SBS block copolymer to a portion of the organic solvent, heating to 60-80° C. and stirring to dissolve, to obtain a solution; (S3), after the dissolved liquid is cooled, an emulsifier and water are added, and emulsified at a rotation speed of 300-800 rpm to form an emulsion; (S4), adding a catalyst to the emulsion, raising the temperature to 50-90° C., adding an epoxidizing agent dropwise for 1-6 hours, keeping the temperature for 1-3 hours, and cooling to obtain a reaction product; (S5), adding the remaining organic solvent to the reaction product, standing to separate the layers, taking the upper organic phase, washing it with water for multiple times, adding epoxy resin, and distilling it under normal pressure to obtain a toughening agent with self-assembled nano-scale anti-epoxy resin cracking.