A kind of gradient carbon paper and preparation method thereof
By using the alternating compression characteristic structure of gradient carbon paper in the hydrogen fuel cell, the problems of membrane electrode damage and low energy conversion efficiency caused by gas pressure differences in the hydrogen fuel cell are solved, and the gas transmission performance and the overall battery system are improved. efficiency.
Patent Information
- Application Number
- CN202310954687.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-08-01
AI Technical Summary
In existing hydrogen fuel cells, the large pressure difference between the inlet and outlet gases causes membrane electrode damage and reduced energy conversion efficiency.
Gradient carbon paper is used, which has a gradient structure of alternating compression characteristics along the in-plane direction. The gas transmission path is adjusted through the difference in compression ratio in different areas, avoiding gas channel blockage, and improving the porous structure and conductivity of the carbon fiber base paper.
It effectively reduces gas flow resistance, prevents the reduction of porosity, improves gas diffusion performance, reduces membrane electrode damage and energy loss, and improves the energy conversion efficiency of hydrogen fuel cells.
Smart Images

Figure CN116695488B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fuel cells, and in particular to a gradient carbon paper and a preparation method thereof. Background Art
[0002] Hydrogen energy is a clean energy source, fuel cells are a very important technology for the application of hydrogen energy, and carbon paper is a core material in hydrogen fuel cells. Improving the performance characteristics of carbon paper through design optimization is of great significance to the application of hydrogen energy.
[0003] During the operation of the fuel cell, the transmission and diffusion of gas on the membrane electrode has a great influence on the effective performance output. For carbon paper, the factors affecting gas transmission are mainly reflected in the pore structure after compression, and the gas inlet and outlet pressure difference caused by the blockage of the gas channel caused by the pressure sinking into the flow channel. Since the pressure conditions of the carbon paper in the flow channel area and the sub-ridge area on the bipolar plate are different, the compression deformation of the sub-ridge area is greater than the compression deformation of the flow channel area, resulting in excessive gas pressure difference and obstruction of the gas transmission path.
[0004] At the same time, during the operation of hydrogen fuel cells, if the gas pressure difference between the inlet and outlet is too large, it is easy to cause damage to the membrane electrode, and the high-pressure resistance requirements of other auxiliary materials in the stack system will also increase accordingly, resulting in an increase in material costs. In addition, due to the large pressure difference, additional energy loss will be caused, resulting in a decrease in the energy conversion efficiency of the hydrogen fuel cell system. Summary of the invention
[0005] Based on this, it is necessary to provide a gradient carbon paper and its preparation method and its preparation method, aiming to solve the technical problems in the prior art of damage to the membrane electrode and reduced energy conversion efficiency of the hydrogen fuel cell system due to the large inlet and outlet gas pressure difference.
[0006] A gradient carbon paper, wherein the raw materials for preparing the gradient carbon paper include:
[0007] Carbon fiber 18~100 parts;
[0008] Conductive carbon powder 20~150 parts;
[0009] 20 to 150 parts of a binder; and
[0010] 70-300 parts of solvent;
[0011] The gradient carbon paper has a gradient compression characteristic along the in-plane direction. In the in-plane direction, the gradient carbon paper is divided into n regions, and the compression rates of the n regions are ξ1 and / or ξ2. The difference between ξ1 and ξ2 ranges from 5% to 20%. The compression rates of adjacent regions are different, and n≥4.
[0012] Preferably, the widths of the n regions are respectively 0.1 mm to 1 mm.
[0013] The present invention also provides a method for preparing the gradient carbon paper as described above, comprising the steps of:
[0014] The carbon fiber is prepared into a carbon fiber base paper having a porous structure;
[0015] The conductive carbon powder, the binder and the solvent are mixed to prepare a first slurry; the carbon fiber base paper is placed in the first slurry for a first immersion and drying;
[0016] The carbon fiber base paper after the first impregnation is subjected to a first heating and rolling operation, and then subjected to a first heat treatment operation to obtain carbon fiber carbon paper;
[0017] The conductive carbon powder, the binder and the solvent are mixed to prepare a second slurry, the second slurry is poured into a mold, and the carbon fiber carbon paper is impregnated again with the mold and dried. During the impregnation process, after one side of the carbon fiber carbon paper is bonded to the second slurry, the second slurry is adsorbed to the other side of the carbon fiber carbon paper; in the mold, there are areas corresponding to a compression rate of ξ1 and areas corresponding to a compression rate of ξ2, and the area corresponding to ξ1 and the area corresponding to ξ2 have a depth difference;
[0018] The carbon fiber carbon paper after the second impregnation is heated and rolled for a second time, and then subjected to a second heat treatment operation to obtain the gradient carbon paper.
[0019] Preferably, the solid content of the first slurry is 10% to 30%, and the viscosity is 10 Pa•s to 100 Pa•s.
[0020] Preferably, the second slurry has a solid content of 10% to 30% and a viscosity of 10 Pa•s to 100 Pa•s.
[0021] Preferably, the heating temperature of the first heating and rolling is 25°C~150°C, and the rolling pressure is 0.5 MPa~5MPa, and the heating temperature of the second heating and rolling is 25°C~150°C, and the rolling pressure is 0.5 MPa~5MPa.
[0022] Preferably, the temperature of the first heat treatment is 300°C to 450°C, and the temperature of the second heat treatment is 300°C to 450°C.
[0023] Preferably, in the mold, the area corresponding to ξ1 is 0.05 mm to 0.3 mm wider than the area corresponding to ξ2.
[0024] Preferably, the diameter of the carbon fiber is 5 μm to 15 μm.
[0025] Preferably, the thickness of the carbon fiber base paper is 0.1 mm to 3 mm.
[0026] Beneficial effects of the present invention
[0027] Through the alternating in-plane compression characteristic gradient structure, the problem of increased gas flow resistance caused by excessive compression deformation due to pressure on the sub-ridge area of the bipolar plate, which causes the carbon fiber base paper in the flow channel area to sink into the flow channel, can be effectively reduced.
[0028] The alternating in-plane compression characteristic gradient structure can effectively prevent the porosity from decreasing due to compression, thereby reducing the gas diffusion coefficient of the carbon fiber base paper and affecting mass transfer. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0030] Figure 1 A plane diagram of a gradient carbon paper in one embodiment;
[0031] Figure 2 A schematic diagram of a mold in an embodiment;
[0032] Figure 3 A plane diagram of a gradient carbon paper in one embodiment;
[0033] Figure 4 A schematic diagram of a mold in an embodiment;
[0034] Figure 5 1 is a pressure-thickness curve of the gradient carbon paper of Example 1 and the non-gradient carbon paper of Comparative Example 1;
[0035] Figure 6 It is a pressure-in-plane air permeability coefficient curve of the gradient carbon paper of Example 1 and the non-gradient carbon paper of Comparative Example 1. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0038] In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, "and / or" in the full text includes three solutions. Taking A and / or B as an example, it includes technical solution A, technical solution B, and technical solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0039] A gradient carbon paper, wherein the raw materials for preparing the gradient carbon paper include, by weight:
[0040] 18-100 parts of carbon fiber, 20-150 parts of conductive carbon powder, 20-150 parts of binder and 70-300 parts of solvent; the conductive carbon powder includes at least one of graphite, carbon black, carbon nanotube and carbon fiber powder, the binder is at least one of cellulose, polyurethane, pyrrolidone and polyvinyl alcohol, and the solvent includes at least one of water, ethanol and methanol.
[0041] The gradient carbon paper has a gradient compression characteristic along the in-plane direction. In the in-plane direction, the gradient carbon paper is divided into n regions, and the compression rates of the n regions are ξ1 and / or ξ2. The difference between ξ1 and ξ2 is in the range of 5% to 20%. The compression rates of adjacent regions are different, and n≥4. Specifically, the thickness of the carbon paper before compression is T0, and the thickness after compression is T1, then the compression rate is ξ=(T0~T1) / T0*100%.
[0042] Preferably, the widths of the n regions are respectively 0.1 mm to 1 mm.
[0043] The present invention also provides a method for preparing the gradient carbon paper as described above, comprising the steps of:
[0044] S100, preparing carbon fiber into carbon fiber base paper with a porous structure.
[0045] S200, mixing the conductive carbon powder, the binder and the solvent to prepare a first slurry, wherein the solid content of the first slurry is 10% to 30% and the viscosity is 10 Pa•s to 100 Pa•s; placing the carbon fiber base paper in the first slurry for a first immersion and drying.
[0046] S300, heating and rolling the carbon fiber base paper after the first impregnation for the first time, and then performing a first heat treatment operation to obtain carbon fiber carbon paper, the heating temperature is 25°C~150°C, the rolling pressure is 0.5 MPa~5MPa, and the heat treatment temperature is 300°C~450°C.
[0047] S400, mixing the conductive carbon powder, the binder and the solvent to prepare a second slurry, pouring the second slurry into a mold, using the mold to impregnate the carbon fiber carbon paper again and dry it, during the impregnation process, after one side of the carbon fiber carbon paper is bonded to the second slurry, the second slurry is adsorbed to the other side of the carbon fiber carbon paper, and the adsorption is to make the slurry quickly penetrate through the carbon fiber carbon paper under the action of negative pressure airflow to fill the carbon fiber carbon paper; in the mold, there are respectively an area corresponding to a compression rate of ξ1 and an area corresponding to a compression rate of ξ2, the area corresponding to ξ1 and the area corresponding to ξ2 have a depth difference of 5-20mm, and the area corresponding to ξ1 is 0.05nm~0.3mm wider than the area corresponding to ξ2.
[0048] S500, heating and rolling the carbon fiber carbon paper after re-impregnation for a second time, and then performing a second heat treatment operation to obtain the gradient carbon paper, the heating temperature is 25°C~150°C, the rolling pressure is 0.5 MPa~5MPa, and the heat treatment temperature is 300°C~450°C.
[0049] Specifically, the thickness of the carbon paper before compression is T0, and the thickness after compression is T1, then the compression rate is ξ=(T0-T1) / T0*100%. When calculating ξ1 and ξ2, T0 is the thickness of the carbon fiber base paper before the first impregnation, and T1 is the thickness of the gradient carbon paper after the second heat treatment. The reason why ξ1 and ξ2 are different is the difference in the number of impregnations. The filling rate of the base paper after one impregnation is lower than the filling rate after two impregnations, so the compression rate after compression is different.
[0050] More specifically, the mold for the second impregnation is divided into an area corresponding to ξ1 and an area corresponding to ξ2, wherein the area corresponding to ξ1 is a solid part, and the surface is treated with polytetrafluoroethylene (Teflon) to make the surface of the mold area ξ1 hydrophobic to prevent the second slurry from entering the area that does not require secondary impregnation. The area corresponding to ξ1 cannot be impregnated for the second time, and the area corresponding to ξ2 is a hollow part that can be impregnated for the second time.
[0051] like Figure 1 As shown, in one embodiment, the gradient carbon paper is a plane diagram of a gradient compression characteristic of a parallel line type carbon paper, wherein the gray part is the area with a compression rate of ξ1, the white part is the area with a compression rate of ξ2, ξ2 corresponds to the area under the bipolar plate ridge, and ξ1 corresponds to the flow channel area. The corresponding mold schematic diagram in this embodiment is Figure 2 ,like Figure 2 As shown, the hollowed-out part corresponds to the area with a compression rate of ξ2.
[0052] like Figure 3 As shown, in one embodiment, the gradient carbon paper is a carbon paper plane diagram with gradient compression characteristics of wavy lines, wherein the black part is the area with a compression rate of ξ2, the gray part is the area with a compression rate of ξ1, ξ2 corresponds to the area under the ridge of the bipolar plate, and the area corresponding to ξ1 is the flow channel area.
[0053] Example 1
[0054] S100, using carbon fiber with a diameter of 6μm-9μm to prepare a carbon fiber base paper with a porous structure with a thickness of 0.25mm;
[0055] S200, using conductive carbon powder, binder, and solvent to mix and prepare a first slurry with a solid content of 20% and a viscosity of 20Pa•s according to a proportion, and the carbon fiber base paper is first impregnated in the first slurry and then dried. Among them, the conductive carbon powder is 10 parts by mass, the binder is 8 parts by mass, and the solvent is 72 parts by mass. The conductive carbon powder is graphite, the binder is polyvinyl pyrrolidone, and the solvent is water.
[0056] S300, heat the carbon fiber base paper after the first impregnation to 50°C, use a steel rod with a diameter of 0.5m to roll it at a pressure of 1MPa, and then heat treat the rolled carbon fiber base paper at 380°C for 10min.
[0057] S400, after the heat treatment is completed, the conductive carbon powder, the binder, and the solvent are mixed and prepared into a second slurry with a solid content of 15% and a viscosity of 20Pa•s according to a proportion, and poured into a mold, and the carbon fiber base paper after the first heat treatment is impregnated and filled with holes again using the mold, and the other side of the carbon fiber base paper is adsorbed during the impregnation process. Among them, the conductive carbon powder is 12 parts by mass, the binder is 8 parts by mass, and the solvent is 113 parts by mass. The conductive carbon powder is graphite, the binder is polyvinyl pyrrolidone, and the solvent is water.
[0058] The mold is divided into an area corresponding to ξ1 and an area corresponding to ξ2, wherein the area corresponding to ξ1 is a solid part, and the surface is treated with polytetrafluoroethylene (Teflon) to make the surface of the mold area ξ1 hydrophobic to prevent the second slurry from entering the area that does not require secondary impregnation. The area corresponding to ξ2 is a hollow part, the width of the ξ1 area is 0.3mm, and the depth is 0mm, the width of the ξ2 area is 0.15mm, and the depth is 5mm, and ξ1 and ξ2 are parallel direct current grooves.
[0059] S500, the carbon fiber base paper after being impregnated, filled and dried again is heated to 50°C, and rolled using a steel rod with a diameter of 0.5m at a pressure of 1MPa, and then the rolled carbon fiber base paper is heat treated at 380°C for 10min to obtain a gradient carbon paper with parallel lines.
[0060] Example 2
[0061] S100, using carbon fibers with a diameter of 6 μm-9 μm to prepare carbon fiber base paper with a porous structure and a thickness of 0.2 mm.
[0062] S200, using conductive carbon powder, binder, and solvent to mix, according to the proportion, to prepare a first slurry with a solid content of 20% and a viscosity of 20Pa•s, and then immersing the carbon fiber base paper in the slurry for the first time and drying it. Conductive carbon powder is 10 parts by mass, binder is 12 parts by mass, and solvent is 88 parts by mass. The conductive carbon powder is graphite, the binder is polyvinyl alcohol, and the solvent is water.
[0063] S300, heating the carbon fiber base paper after the first impregnation to 50°C, using a steel rod with a diameter of 0.5m to roll it at a pressure of 1MPa, and then heat treating the rolled carbon fiber base paper at 380°C for 10min to obtain carbon fiber carbon paper.
[0064] S400, after the heat treatment is completed, the conductive carbon powder, the binder, and the solvent are mixed, and the second slurry with a solid content of 15% and a viscosity of 20Pa•s is prepared according to the proportion and poured into the mold, and the carbon fiber carbon paper after the first heat treatment is impregnated and filled with holes again using the mold, and the other side of the carbon fiber base paper is adsorbed during the impregnation process. Among them, the conductive carbon powder is 8 parts by mass, the binder is 7 parts by mass, and the solvent is 85 parts by mass. The conductive carbon powder is graphite, the binder is polyvinyl alcohol, and the solvent is water.
[0065] Mould Figure 2 As shown, it is divided into the area corresponding to ξ1 and the area corresponding to ξ2, where the area corresponding to ξ1 is the solid part, and the surface is treated with Teflon, and the area corresponding to ξ2 is the hollow part. The width of the ξ1 area is 0.2mm, and the depth is 0mm. The width of the ξ2 area is 0.15mm, and the depth is 15mm. ξ1 and ξ2 are parallel straight grooves.
[0066] S500, the carbon fiber base paper after being impregnated, filled and dried again is heated to 50°C, and rolled using a steel rod with a diameter of 0.5m at a pressure of 1MPa, and then the rolled carbon fiber base paper is heat treated at 380°C for 10min to obtain a gradient carbon paper with parallel lines.
[0067] Example 3
[0068] S100, using carbon fibers with a diameter of 6 μm-9 μm to prepare carbon fiber base paper with a porous structure and a thickness of 1 mm.
[0069] S200, using conductive carbon powder, binder, and solvent to mix, according to the proportion, to prepare a first slurry with a solid content of 25% and a viscosity of 30Pa•s, and completely immersing the carbon fiber base paper in the first slurry and then drying it. Among them, the conductive carbon powder is 14 parts by mass, the binder is 11 parts by mass, and the solvent is 75 parts by mass. The conductive carbon powder is graphite, the binder is polyvinyl alcohol, and the solvent is water.
[0070] S300, heating the carbon fiber base paper after the first impregnation to 50°C, using a steel rod with a diameter of 0.5m to roll it at a pressure of 1.5MPa, and then heat treating the rolled carbon fiber base paper at 380°C for 10min to obtain carbon fiber carbon paper.
[0071] S400, after the heat treatment is completed, the conductive carbon powder, the binder, and the solvent are mixed and prepared into a second slurry with a solid content of 20% and a viscosity of 20Pa•s according to a proportion, and poured into a mold, and the carbon fiber carbon paper is impregnated and filled with holes again using the mold, and the other side of the carbon fiber base paper is adsorbed during the impregnation process. Among them, the conductive carbon powder is 10 parts by mass, the binder is 10 parts by mass, and the solvent is 80 parts by mass. The conductive carbon powder is graphite, the binder is polyvinyl alcohol, and the solvent is water.
[0072] Mould Figure 4 As shown, it is divided into the area corresponding to ξ1 and the area corresponding to ξ2, where the area corresponding to ξ1 is the solid part, and the surface is treated with Teflon, and the area corresponding to ξ2 is the hollow part. The width of the ξ1 area is 0.2mm, and the depth is 0mm. The width of the ξ2 area is 0.15mm, and the depth is 20mm. ξ1 and ξ2 are parallel wavy grooves.
[0073] S500, heating the carbon fiber carbon paper that has been impregnated, filled and dried again to 50°C, using a steel rod with a diameter of 0.5m to roll it at a pressure of 1MPa, and then heat-treating the rolled carbon fiber carbon paper at 380°C for 10min to obtain a gradient carbon paper with parallel wavy lines.
[0074] The pressure-thickness data tables of Example 2 and Example 3 are as follows Figure 1 As shown, the pressure-permeability coefficient data table of Example 2 and Example 3 is as follows Figure 2 shown.
[0075] Comparative Example 1 (non-gradient carbon paper)
[0076] The other steps are the same as those in Example 1. In step S400, no mold having a region corresponding to ξ1 and a region corresponding to ξ2 is used for impregnation to obtain a non-gradient carbon paper.
[0077] The thickness of the gradient carbon paper prepared in Example 1 and the non-gradient carbon paper prepared in Comparative Example 1 was tested to see whether it changes with pressure. The results are as follows: Figure 4 .
[0078] like Figure 4 As shown, under the same pressure, the thickness of the carbon paper after gradient treatment is greater than that of the carbon paper without gradient treatment, that is, the compression deformation is smaller.
[0079] The air permeability coefficient of the gradient carbon paper prepared in Example 1 and the non-gradient carbon paper prepared in Comparative Example 1 was tested to change with pressure. The results are as follows: Figure 5 .
[0080] like Figure 5 As shown, with the increase of pressure, the carbon paper after gradient treatment has a higher in-plane permeability coefficient, which means that the gradient treatment can effectively improve the problem of reduced permeability coefficient caused by compression and improve the gas transmission and diffusion performance.
[0081] Table 1 Pressure-thickness data of Example 2 and Example 3
[0082]
[0083] Table 2 Pressure-permeability coefficient data of Example 2 and Example 3
[0084]
[0085] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a gradient carbon paper, characterized in that: In parts by weight, the raw materials for preparing the gradient carbon paper include: Carbon fiber 18~100 parts; Conductive carbon powder 20~150 parts; 20 to 150 parts of a binder; and 70-300 parts of solvent; The gradient carbon paper has a gradient structure of compression characteristics along the in-plane direction. In the in-plane direction, the gradient carbon paper is divided into n regions, and the compression rates of adjacent regions of the n regions are ξ1 and ξ2 respectively, and the difference between ξ1 and ξ2 is in the range of 5% to 20%, and n≥4; The preparation method of the gradient carbon paper comprises the steps of: The carbon fiber is prepared into a carbon fiber base paper having a porous structure; The conductive carbon powder, the binder and the solvent are mixed to prepare a first slurry; the carbon fiber base paper is placed in the first slurry for a first immersion and drying; The carbon fiber base paper after the first impregnation is subjected to a first heating and rolling operation, and then subjected to a first heat treatment operation to obtain carbon fiber carbon paper; The conductive carbon powder, the binder and the solvent are mixed to obtain a second slurry, the second slurry is poured into a mold, and the carbon fiber carbon paper is impregnated again with the mold and dried. During the impregnation process, after one side of the carbon fiber carbon paper is bonded to the second slurry, the second slurry is adsorbed to the other side of the carbon fiber carbon paper, and the adsorption is to make the second slurry quickly penetrate through the carbon fiber carbon paper under the action of negative pressure airflow to fill the carbon fiber carbon paper; the mold has an area corresponding to ξ1 and an area corresponding to ξ2, the area corresponding to ξ1 is an area corresponding to the compression rate of ξ1 and does not require secondary impregnation, the area corresponding to ξ2 is a secondary impregnation area corresponding to the compression rate of ξ2, and the area corresponding to ξ1 and the area corresponding to ξ2 have a depth difference of 5-20mm; wherein the area corresponding to ξ1 is a solid part, and the surface is treated with a hydrophobic agent to make the surface of the area corresponding to ξ1 in the mold hydrophobic, so as to prevent the second slurry from entering the area corresponding to ξ1 that does not require secondary impregnation; The carbon fiber carbon paper after the second impregnation is heated and rolled for a second time, and then subjected to a second heat treatment operation to obtain the gradient carbon paper.
2. The method for preparing the gradient carbon paper according to claim 1, characterized in that: The widths of the n regions are respectively 0.1 mm to 1 mm.
3. The method for preparing the gradient carbon paper according to claim 1, characterized in that: The solid content of the first slurry is 10% to 30%, and the viscosity is 10 Pa•s to 100 Pa•s.
4. The method for preparing the gradient carbon paper according to claim 1, characterized in that: The second slurry has a solid content of 10% to 30% and a viscosity of 10 Pa•s to 100 Pa•s.
5. The method for preparing the gradient carbon paper according to claim 1, characterized in that: The heating temperature of the first heating and rolling is 25°C~150°C, and the rolling pressure is 0.5MPa~5MPa. The heating temperature of the second heating and rolling is 25°C~150°C, and the rolling pressure is 0.5MPa~5MPa.
6. The method for preparing the gradient carbon paper according to claim 1, characterized in that: The temperature of the first heat treatment is 300°C~450°C, and the temperature of the second heat treatment is 300°C~450°C.
7. The method for preparing the gradient carbon paper according to claim 1, characterized in that: In the mold, the area corresponding to ξ1 is 0.05 mm to 0.3 mm wider than the area corresponding to ξ2.
8. The method for preparing the gradient carbon paper according to claim 1, characterized in that: The diameter of the carbon fiber is 5 μm to 15 μm.
9. The method for preparing the gradient carbon paper according to claim 1, characterized in that: The thickness of the carbon fiber base paper is 0.1 mm to 3 mm.
Citation Information
Patent Citations
Gas diffusion layer of proton exchange membrane fuel cell
CN110112425A
Special-shaped fuel cell gas diffusion layer, preparation method, fuel cell and assembly method
CN111799475A