A preparation method of a hydrophobic composite polyelectrolyte and its application in preparing oil-absorbing gel
By preparing hydrophobic composite polyelectrolyte [DEMA-TD][TPB], the problem of insufficient swelling ability of traditional oil-absorbing gels with organic solvents is solved, the absorption performance is significantly improved, and the efficiency is maintained during recycling, solving the current problem of There are limitations on the type and cost of polyelectrolyte preparation methods.
Patent Information
- Application Number
- CN202310711110.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-06-15
AI Technical Summary
Traditional oil-absorbing gels have insufficient swelling capacity for organic solvents and cannot cost-effectively absorb and separate organic solvents in water. Moreover, existing polyelectrolyte preparation methods limit the types of soluble organic solvents and are costly.
A hydrophobic composite polyelectrolyte is prepared by mixing tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone, adding anhydrous ether to precipitate, drying in a vacuum, and then Sodium tetraphenylborate reacts with deionized water to prepare hydrophobic composite polyelectrolyte [DEMA-TD][TPB], which is used to prepare oil-absorbing gel.
The oil-absorbing gel's absorption performance of n-heptane, toluene and methylene chloride is significantly improved, and the swelling rate of the material is only reduced by 3.3% during recycling, proving its high efficiency and reusability.
Smart Images

Figure CN116731057B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a polyelectrolyte. Background Art
[0002] Gel is an organic polymer soft material with a three-dimensional network structure formed by the mutual polymerization and cross-linking of one or more organic monomers through chemical reactions or physical actions. Due to the existence of the cross-linked network, there are a large number of pores in its spatial structure, so it has the function of adsorbing and storing liquid and gaseous substances (solutes). In addition, a large number of pores also give this type of material sufficient deformation space, so this type of material also has excellent elasticity and compressibility. According to the type of adsorbed substance, gel can be divided into hydrogel, aerogel and oil-absorbing gel. Among them, since oil-absorbing gel has the characteristics of absorbing a variety of organic solvents, it is used to absorb organic pollutants in water, such as offshore oil and organic matter leakage, organic sewage purification and kitchen wastewater treatment.
[0003] Although oil-absorbing gels can absorb organic solvents, they generally have the characteristics of low absorption rate, few types of absorbable organic solvents, and low reuse rate. There are three main reasons for the above problems. First, the adsorption process of the material is a dynamic physical action. For oil-absorbing gels, the adsorption power comes from the intermolecular force between the gel constituent monomers and the adsorbed organic matter, that is, the van der Waals force; the desorption power comes from the concentration difference of the organic matter and the rebound force generated by the expansion of the gel network structure. Since the van der Waals force is a weak force in chemistry, the positive adsorption power provided is small, resulting in a low adsorption rate of organic solvents. In addition, the polarity between materials is different. For the same gel constituent monomer, as the polarity difference between it and the adsorbed organic solvent increases, the intermolecular force becomes smaller, resulting in a decrease in adsorption power and adsorption rate, which is reflected in the different adsorption rates of different organic solvents from a macroscopic level. At the same time, since the constituent monomers of the oil-absorbing gel are only connected by covalent bonds, the structural strength is smaller than that of the hydrogel composed of multiple forces, and the material as a whole is more easily destroyed during use. In order to solve the above problems, introducing one or more forces into the traditional oil-absorbing gel structure is the main research direction in current related research.
[0004] Polyelectrolytes are organic salts formed by two oppositely charged polymerizable organic substances through ionic bonds or complex reactions, and have physical properties similar to those of inorganic salts. However, unlike inorganic salts, polyelectrolytes can usually be ionized in one or more organic solvents because the anions and cations that constitute the polyelectrolytes are lipophilic. Depending on the different charges carried by the organic substances after ionization, polyelectrolytes can be divided into anionic polyelectrolytes, cationic polyelectrolytes, and composite polyelectrolytes. By introducing polyelectrolytes into the oil-absorbing gel structure, the corresponding charge can be given to the oil-absorbing gel structure by relying on its ionization characteristics, thereby introducing electromagnetic repulsion characteristics into the gel, providing new impetus for the positive adsorption of the solution. In addition, depending on the organic solvents that the polyelectrolyte can ionize and the solubility, its electromagnetic repulsion characteristics show selectivity. In addition, the new electromagnetic force provides higher strength for the structure.
[0005] Although the introduction of polyelectrolytes provides an effective solution for improving the performance of oil-absorbing gels, the preparation of polyelectrolytes is still in its infancy. How to prepare polyelectrolytes with higher solubility, a wider range of organic solvents that can be dissolved, and lower costs is the main problem currently faced. Summary of the invention
[0006] The purpose of the present invention is to solve the problem that traditional oil-absorbing gel materials have insufficient swelling capacity for organic solvents, cannot absorb and separate organic solvents in water economically and effectively, and the oil-absorbing gel prepared using existing polyelectrolytes has few types of organic solvents that can be dissolved, and to provide a method for preparing a hydrophobic composite polyelectrolyte and its application in preparing oil-absorbing gel.
[0007] A method for preparing a hydrophobic composite polyelectrolyte is specifically completed by the following steps:
[0008] 1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]:
[0009] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed and stirred for a period of time at the experimental temperature and in a nitrogen atmosphere to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, and the precipitate was collected and then vacuum dried to remove the solvent to obtain an anionic polyelectrolyte [DEMA-TD][Br], which was recorded as DTB;
[0010] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is (1-2):1:(0.01-0.09):(3-6);
[0011] 2. Preparation of composite polyelectrolyte:
[0012] DTB, sodium tetraphenylborate and acetone were mixed and stirred for a period of time at the experimental temperature and nitrogen atmosphere to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at the experimental temperature and stirred for a certain period of time to obtain a white precipitate; the white precipitate was rinsed and finally vacuum dried to remove the residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], which was recorded as DTT;
[0013] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step 2 is 1:(1-2):(10-20):(30-60).
[0014] A hydrophobic composite polyelectrolyte is used to prepare oil-absorbing gel.
[0015] Advantages of the present invention:
[0016] (1) Compared with the oil-absorbing gel without adding polyelectrolyte, the hydrophobic composite polyelectrolyte prepared by the present invention can effectively improve the swelling performance of the oil-absorbing gel. Compared with the oil-absorbing gel used in the control group, the absorption performance of n-heptane under the test conditions is improved by 52.44% to 120.01%, the absorption performance of toluene is improved by 92.22% to 190.36%, and the absorption performance of dichloromethane is improved by 139.27% to 453.90%;
[0017] (2) The oil-absorbing gel prepared by the hydrophobic composite polyelectrolyte prepared by the present invention can be recycled by adsorption-desorption. Benzene is used as the absorption target. After 10 adsorption-desorption experiments, the swelling rate of the material is only reduced by 3.3%. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the nuclear magnetic resonance hydrogen spectrum characterization spectrum of the anionic polyelectrolyte [DEMA-TD][Br] prepared in step 1 of Example 1;
[0019] Figure 2 This is the nuclear magnetic resonance hydrogen spectrum characterization spectrum of the hydrophobic composite polyelectrolyte [DEMA-TD][TPB] prepared in step 2 of Example 1;
[0020] Figure 3 The following are the swelling test results of the comparative example and application tests 1, 2 and 3 in different organic solvents. DETAILED DESCRIPTION
[0021] Specific implementation method 1: This implementation method is a method for preparing a hydrophobic composite polyelectrolyte, which is specifically completed by the following steps:
[0022] 1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]:
[0023] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed and stirred for a period of time at the experimental temperature and in a nitrogen atmosphere to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, and the precipitate was collected and then vacuum dried to remove the solvent to obtain an anionic polyelectrolyte [DEMA-TD][Br], which was recorded as DTB;
[0024] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is (1-2):1:(0.01-0.09):(3-6);
[0025] 2. Preparation of composite polyelectrolyte:
[0026] DTB, sodium tetraphenylborate and acetone were mixed and stirred for a period of time at the experimental temperature and nitrogen atmosphere to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at the experimental temperature and stirred for a certain period of time to obtain a white precipitate; the white precipitate was rinsed and finally vacuum dried to remove the residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], which was recorded as DTT;
[0027] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step 2 is 1:(1-2):(10-20):(30-60).
[0028] Specific implementation method 2: The difference between this implementation method and specific implementation method 1 is that: the experimental temperature described in step 1 is 35℃~55℃; the stirring time is 12h~36h; the stirring speed is 100r / min~800r / min; the experimental temperature described in step 2 is 15℃~35℃; in step 2, DTB, sodium tetraphenylborate and acetone are mixed, stirred for 2h~6h at 15℃~35℃ and nitrogen atmosphere, and the stirring speed is 100r / min~800r / min to obtain a light yellow opaque liquid; in step 2, a certain mass of deionized water is added to the light yellow opaque liquid at the experimental temperature, and then stirred for 4h~12h, and the stirring speed is 100r / min~800r / min to obtain a white precipitate; the white precipitate is rinsed with deionized water 3 times~5 times. The other steps are the same as those in specific implementation method 1.
[0029] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1:1:0.01:3; the molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step 2 is 1:1:10:30. The other steps are the same as those in specific embodiment 1 or 2.
[0030] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the experimental temperature described in step 1 is 35°C; the stirring time is 36h; the stirring speed is 800r / min; the experimental temperature described in step 2 is 15°C; in step 2, DTB, sodium tetraphenylborate and acetone are mixed, stirred for 6h at 15°C and nitrogen atmosphere, and the stirring speed is 800r / min to obtain a light yellow opaque liquid; in step 2, a certain mass of deionized water is added to the light yellow opaque liquid at the experimental temperature, and then stirred for 12h at a stirring speed of 800r / min to obtain a white precipitate; the white precipitate is rinsed with deionized water for 3 to 5 times. The other steps are the same as those of specific embodiments 1 to 3.
[0031] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1.5:1:0.05:4.5; the molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step 2 is 1:1.5:15:45. The other steps are the same as those in specific embodiments 1 to 4.
[0032] Specific implementation six: This implementation is different from specific implementations one to five in that: the experimental temperature described in step one is 45°C; the stirring time is 24h; the stirring speed is 450r / min; the experimental temperature described in step two is 25°C; in step two, DTB, sodium tetraphenylborate and acetone are mixed, stirred for 4h at 25°C and nitrogen atmosphere, and the stirring speed is 450r / min to obtain a light yellow opaque liquid; in step two, a certain mass of deionized water is added to the light yellow opaque liquid at the experimental temperature, and then stirred for 8h at a stirring speed of 450r / min to obtain a white precipitate; the white precipitate is rinsed with deionized water for 3 to 5 times. The other steps are the same as those of specific implementations one to five.
[0033] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 2:1:0.09:6; the molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step 2 is 1:2:20:60. The other steps are the same as those in specific embodiments 1 to 6.
[0034] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the experimental temperature described in step one is 55°C; the stirring time is 12h; the stirring speed is 100r / min; the experimental temperature described in step two is 35°C; in step two, DTB, sodium tetraphenylborate and acetone are mixed, stirred at 35°C and nitrogen atmosphere for 2h, and the stirring speed is 100r / min to obtain a light yellow opaque liquid; in step two, a certain mass of deionized water is added dropwise to the light yellow opaque liquid at the experimental temperature, and then stirred for 4h, and the stirring speed is 100r / min to obtain a white precipitate; the white precipitate is rinsed with deionized water for 3 to 5 times. The other steps are the same as specific embodiments one to seven.
[0035] Specific embodiment 9: This embodiment is a hydrophobic composite polyelectrolyte used to prepare oil-absorbing gel.
[0036] Specific embodiment 10: The difference between this embodiment and specific embodiment 9 is that a hydrophobic composite polyelectrolyte is used to prepare an oil-absorbing gel in accordance with the following steps:
[0037] Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone are added into a sealable container and stirred at 25°C to 40°C for 1 hour, nitrogen is filled into the container and sealed, and constant temperature heating is performed at the experimental temperature to finally obtain a reaction product, and the product is vacuum dried to remove acetone to obtain an oil-absorbing gel;
[0038] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone is (1-5):(1-5):(0.03-0.15):(0.06-0.3):(0.2-0.6):(3-9); the experimental temperature range is 70°C-80°C; the constant temperature heating time is 8h-12h. The other steps are the same as those in the ninth embodiment.
[0039] The following examples are used to verify the beneficial effects of the present invention:
[0040] Embodiment 1: A method for preparing a hydrophobic composite polyelectrolyte, characterized in that the preparation method is specifically completed according to the following steps:
[0041] 1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]:
[0042] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed, stirred at 35°C and nitrogen atmosphere for 36 hours at a stirring speed of 800 r / min to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, the precipitate was collected, and the precipitate was vacuum dried to remove the solvent to obtain anionic polyelectrolyte [DEMA-TD][Br], recorded as DTB;
[0043] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1:1:0.01:3;
[0044] 2. Preparation of composite polyelectrolyte:
[0045] DTB, sodium tetraphenylborate and acetone were mixed, stirred at 15°C and nitrogen atmosphere for 6 hours at a stirring speed of 800 r / min to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at 15°C, and stirred for another 12 hours at a stirring speed of 800 r / min to obtain a white precipitate; the white precipitate was rinsed with deionized water for 5 times, and finally vacuum dried to remove residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], denoted as DTT;
[0046] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water described in step 2 is 1:1:10:30.
[0047] Embodiment 2: A method for preparing a hydrophobic composite polyelectrolyte, characterized in that the preparation method is specifically completed according to the following steps:
[0048] 1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]:
[0049] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed, stirred at 45°C and nitrogen atmosphere for 24 hours at a stirring speed of 450 r / min to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, the precipitate was collected, and the precipitate was vacuum dried to remove the solvent to obtain anionic polyelectrolyte [DEMA-TD][Br], recorded as DTB;
[0050] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1.5:1:0.05:4.5;
[0051] 2. Preparation of composite polyelectrolyte:
[0052] DTB, sodium tetraphenylborate and acetone were mixed, stirred at 25°C and nitrogen atmosphere for 4 hours at a stirring speed of 450 r / min to obtain a light yellow opaque liquid; a certain mass of deionized water was added dropwise to the light yellow opaque liquid at 25°C, and stirred for another 8 hours at a stirring speed of 450 r / min to obtain a white precipitate; the white precipitate was rinsed with deionized water for 5 times, and finally vacuum dried to remove residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], denoted as DTT;
[0053] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step 2 is 1:1.5:15:45.
[0054] Embodiment 3: A method for preparing a hydrophobic composite polyelectrolyte, characterized in that the preparation method is specifically completed according to the following steps:
[0055] 1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]:
[0056] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed and stirred at 55°C in a nitrogen atmosphere for 12 hours at a stirring speed of 100 r / min to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, and the precipitate was collected and then vacuum dried to remove the solvent to obtain an anionic polyelectrolyte [DEMA-TD][Br], which was recorded as DTB;
[0057] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 2:1:0.09:6;
[0058] 2. Preparation of composite polyelectrolyte:
[0059] DTB, sodium tetraphenylborate and acetone were mixed, stirred at 35°C and nitrogen atmosphere for 2 hours at a stirring speed of 100 r / min to obtain a light yellow opaque liquid; a certain mass of deionized water was added dropwise to the light yellow opaque liquid at 35°C, and stirred for another 4 hours at a stirring speed of 100 r / min to obtain a white precipitate; the white precipitate was rinsed with deionized water for 5 times, and finally vacuum dried to remove the residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], denoted as DTT;
[0060] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water described in step 2 is 1:2:20:60.
[0061] The anionic polyelectrolyte [DEMA-TD][Br] prepared in step 1 of Example 1 was subjected to H-NMR testing, and the characterization spectrum is shown in Figure 1 As shown;
[0062] from Figure 1 It can be seen that DTB has a total of 10 absorption peaks, which represent the resonance absorption of 10 hydrogen nuclei in the molecular structure. The position of each hydrogen nucleus and its corresponding peak has been marked in the figure. The above test results prove the successful synthesis of DTB.
[0063] The hydrophobic composite polyelectrolyte [DEMA-TD][TPB] prepared in step 2 of Example 1 was subjected to H-NMR test, and the characterization spectrum is shown in Figure 2 As shown;
[0064] from Figure 2 It can be seen that compared with Figure 1 , the H-NMR test results of DTT showed three new absorption peaks, which represent the three hydrogen nuclei on the tetraphenylboryl group. The positions of each hydrogen nucleus and its corresponding peaks are marked in the figure. The above test results prove the successful synthesis of DTT.
[0065] Application test 1: A hydrophobic composite polyelectrolyte prepared in Example 1 was used to prepare an oil-absorbing gel, which was specifically completed by the following steps:
[0066] Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone are added to a sealable container, and then stirred at 25°C for 1 hour, nitrogen is filled into the container, and then the container is sealed, and heated at a constant temperature of 70°C for 12 hours in a nitrogen atmosphere to finally obtain a reaction product, and the product is vacuum dried to remove acetone to obtain an oil-absorbing gel;
[0067] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone is 5:1:0.03:0.3:0.2:3.
[0068] Application Test 2: A hydrophobic composite polyelectrolyte prepared in Example 1 was used to prepare an oil-absorbing gel, which was specifically completed by the following steps:
[0069] Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone are added to a sealable container, and then stirred at 25°C for 1 hour, nitrogen is filled into the container, and then the container is sealed, and heated at a constant temperature of 75°C for 10 hours in a nitrogen atmosphere to finally obtain a reaction product, and the product is vacuum dried to remove acetone to obtain an oil-absorbing gel;
[0070] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone is 3:3:0.09:0.18:0.4:4.5.
[0071] Application test 3: A hydrophobic composite polyelectrolyte prepared in Example 1 was used to prepare an oil-absorbing gel, which was specifically completed by the following steps:
[0072] Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone are added to a sealable container, and then stirred at 25°C for 1 hour, nitrogen is filled into the container, and then the container is sealed, and heated at a constant temperature of 80°C for 8 hours in a nitrogen atmosphere to finally obtain a reaction product, and the product is vacuum dried to remove acetone to obtain an oil-absorbing gel;
[0073] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone is 1:5:0.15:0.06:0.6:6.
[0074] Comparative Example:
[0075] Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide and acetone are added into a sealable container in a mass ratio of 1:5:0.15:0.06:6, and then stirred at 25°C for 1 hour; nitrogen is filled into the container, and then the container is sealed, and heated at a constant temperature of 80°C for 8 hours under a nitrogen atmosphere to finally obtain a reaction product. The product is vacuum dried to remove acetone, thereby obtaining an oil-absorbing gel.
[0076] In order to test the absorption capacity of the oil-absorbing gel prepared by the hydrophobic composite polyelectrolyte [DEMA-TD][TPB] prepared by the present invention for organic solvents, the gel was placed in different organic solvents (the material can absorb a wide variety of organic solvents, and only n-heptane, toluene and dichloromethane were selected for the absorption capacity test in this test), and the mass change of the gel before and after the experiment was measured after immersion at 25°C for 24 hours, so as to calculate the mass change rate.
[0077] The swelling rate variation trend of the oil-absorbing gel prepared in the comparative example and application tests 1, 2 and 3 in n-heptane, toluene and dichloromethane is shown in FIG. Figure 3 As shown;
[0078] Table 1 shows the swelling ratios obtained from the swelling experiments of the oil-absorbing gel prepared in the comparative example and the oil-absorbing gel prepared in the application tests 1, 2 and 3 in n-heptane, toluene and dichloromethane;
[0079] Table 1 Swelling ratio of the same gel in organic solvents
[0080]
[0081] The swelling test results show that with the addition of DTT, the gel's absorption capacity for three organic solvents is significantly improved. In n-heptane, compared with the control example, the swelling rate of application test 1 increased by 52.44%, the swelling rate of application test 2 increased by 120.01%, and the swelling rate of application test 3 increased by 78.17%; in toluene, compared with the control example, the swelling rate of application test 1 increased by 92.22%, the swelling rate of application test 2 increased by 193.36%, and the swelling rate of application test 3 increased by 155.64%; in dichloromethane, compared with the control example, the swelling rate of application test 1 increased by 139.27%, the swelling rate of application test 2 increased by 265.37%, and the swelling rate of application test 3 increased by 453.90%. The above test results prove that the addition of DTT can effectively improve the gel's absorption capacity for organic solvents.
[0082] In order to test the reusability of the oil-absorbing gel prepared by the present invention for organic solvents, multiple adsorption-desorption experiments were carried out with dichloromethane as the adsorption target. The initial mass of the gel was weighed and recorded as m0, and then an adsorption experiment was carried out. The experimental temperature was 25°C and the immersion time was 24 hours. Then the mass of the swollen gel m1 was weighed. The swelling rate R1 of the gel was calculated based on m0 and m1. The gel was then placed in a 60°C oven for 24 hours to remove the adsorbed dichloromethane, and the mass after desorption was weighed and recorded as m2. The mass change rate R2 of the gel was calculated based on m0 and m2. The above process was repeated 10 times, and the initial mass m was tested by the first test. 0-1 and the mass m after the tenth desorption 2-10 , calculate the cycle mass change rate R3; R1, R2 and R3 are calculated according to the following formulas 1, 2 and 3.
[0083]
[0084]
[0085]
[0086] Table 2 shows the results of 10 adsorption-desorption tests of the oil-absorbing gel prepared in Application Test 3 in benzene.
[0087] Table 2 Results of cyclic adsorption-desorption tests of oil-absorbing gels based on hydrophobic polyelectrolytes
[0088]
[0089] The results of the cyclic adsorption-desorption test show that the mass loss rate of the oil-absorbing gel prepared in the application test 3 is 3.3% after 10 cycles of testing; at the same time, the swelling rate change rate is almost unchanged. The above results prove that the oil-absorbing gel prepared based on the hydrophobic polyelectrolyte has the function of being reusable.
Claims
1. An application of a hydrophobic composite polyelectrolyte, characterized in that A hydrophobic composite polyelectrolyte is used to prepare an oil-absorbing gel, wherein the swelling rate of the oil-absorbing gel in n-heptane is 258.36%, the swelling rate in toluene is 559.84%, and the swelling rate in dichloromethane is 722.39%. The preparation method is specifically completed according to the following steps: Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone are added to a sealable container, and then stirred at 25°C for 1 hour, nitrogen is filled into the container, and then the container is sealed, and heated at a constant temperature of 70°C for 12 hours in a nitrogen atmosphere to finally obtain a reaction product, and the product is vacuum dried to remove acetone to obtain an oil-absorbing gel; The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone is 5:1:0.03:0.3:0.2:3; The preparation method of DTT is specifically completed according to the following steps:
1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]: Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed, stirred at 35°C and nitrogen atmosphere for 36 hours at a stirring speed of 800 r / min to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, the precipitate was collected, and the precipitate was vacuum dried to remove the solvent to obtain anionic polyelectrolyte [DEMA-TD][Br], recorded as DTB; The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1:1:0.01:3; 2. Preparation of composite polyelectrolyte: DTB, sodium tetraphenylborate and acetone were mixed, stirred at 15°C and nitrogen atmosphere for 6 hours at a stirring speed of 800 r / min to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at 15°C, and stirred for another 12 hours at a stirring speed of 800 r / min to obtain a white precipitate; the white precipitate was rinsed with deionized water for 5 times, and finally vacuum dried to remove residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], denoted as DTT; The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water described in step 2 is 1:1:10:
30.
2. An application of a hydrophobic composite polyelectrolyte, characterized in that A hydrophobic composite polyelectrolyte is used to prepare an oil-absorbing gel, wherein the swelling rate of the oil-absorbing gel in n-heptane is 372.87%, the swelling rate in toluene is 854.42%, and the swelling rate in dichloromethane is 1103.11%. The preparation method is specifically completed according to the following steps: Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone are added to a sealable container, and then stirred at 25°C for 1 hour, nitrogen is filled into the container, and then the container is sealed, and heated at a constant temperature of 80°C for 8 hours in a nitrogen atmosphere to finally obtain a reaction product, and the product is vacuum dried to remove acetone to obtain an oil-absorbing gel; The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone is 3:3:0.09:0.18:0.4:4.5; The preparation method of DTT is specifically completed according to the following steps:
1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]: Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed, stirred at 35°C and nitrogen atmosphere for 36 hours at a stirring speed of 800 r / min to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, the precipitate was collected, and the precipitate was vacuum dried to remove the solvent to obtain anionic polyelectrolyte [DEMA-TD][Br], recorded as DTB; The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1:1:0.01:3; 2. Preparation of composite polyelectrolyte: DTB, sodium tetraphenylborate and acetone were mixed, stirred at 15°C and nitrogen atmosphere for 6 hours at a stirring speed of 800 r / min to obtain a light yellow opaque liquid; a certain mass of deionized water was added dropwise to the light yellow opaque liquid at 15°C, and stirred for another 12 hours at a stirring speed of 800 r / min to obtain a white precipitate; the white precipitate was rinsed with deionized water for 5 times, and finally vacuum dried to remove residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], denoted as DTT; The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water described in step 2 is 1:1:10:
30.
3. An application of a hydrophobic composite polyelectrolyte, characterized in that A hydrophobic composite polyelectrolyte is used to prepare an oil-absorbing gel, wherein the swelling rate of the oil-absorbing gel in n-heptane is 301.97%, the swelling rate in toluene is 744.54%, the swelling rate in dichloromethane is 1672.34%, and the mass loss rate is 3.3% after 10 adsorption-desorption cycles in benzene; the preparation method is specifically completed according to the following steps: Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone are added to a sealable container, and then stirred at 25°C for 1 hour, nitrogen is filled into the container, and then the container is sealed, and heated at a constant temperature of 80°C for 8 hours in a nitrogen atmosphere to finally obtain a reaction product, and the product is vacuum dried to remove acetone to obtain an oil-absorbing gel; The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, benzoyl peroxide, DTT and acetone is 1:5:0.15:0.06:0.6:6; The preparation method of DTT is specifically completed according to the following steps:
1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]: Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed, stirred at 35°C and nitrogen atmosphere for 36 hours at a stirring speed of 800 r / min to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, the precipitate was collected, and the precipitate was vacuum dried to remove the solvent to obtain anionic polyelectrolyte [DEMA-TD][Br], recorded as DTB; The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1:1:0.01:3; 2. Preparation of composite polyelectrolyte: DTB, sodium tetraphenylborate and acetone were mixed, stirred at 15°C and nitrogen atmosphere for 6 hours at a stirring speed of 800 r / min to obtain a light yellow opaque liquid; a certain mass of deionized water was added dropwise to the light yellow opaque liquid at 15°C, and stirred for another 12 hours at a stirring speed of 800 r / min to obtain a white precipitate; the white precipitate was rinsed with deionized water for 5 times, and finally vacuum dried to remove residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], denoted as DTT; The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water described in step 2 is 1:1:10:30.