A method for back sealing of silicon wafers
By adding an LTO layer to the silicon wafer back-sealing process to wrap a POLY layer, the edge SRP abnormality problem caused by metal impurity diffusion was solved, and the uniformity of silicon wafer resistivity and SRP characteristics were improved.
Patent Information
- Application Number
- CN202310685375.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-12
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-06-12
AI Technical Summary
In existing silicon wafer back-sealing processes, metal impurities diffuse to the edge of the front side of the silicon wafer during high-temperature processes, causing abnormal edge SRP tests and resulting in poor resistivity uniformity.
The process employs LTO+POLY+LTO, which adds an LTO film to the existing super back-sealing process to wrap the POLY layer and prevent the diffusion of metal impurities. The specific steps include depositing an LTO film, a POLY film, and a second LTO film on the back of the silicon wafer.
It effectively prevents the diffusion of metal impurities during high-temperature epitaxy, solves the edge SRP anomaly problem, improves the uniformity of resistivity within the silicon wafer, and ensures that the SRP characteristic curve is normal.
Smart Images

Figure CN116741623B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and more particularly to a method for back-sealing silicon wafers. Background Technology
[0002] In the semiconductor manufacturing field, edge SRP testing of silicon wafers typically refers to SRP (Spreading Resistance Profile) testing of the silicon wafer edges. This is a method for measuring electrical parameters such as diffusion resistance, resistivity, and carrier concentration distribution of semiconductor materials at relatively high resolution. On epitaxial wafers, it is generally used to measure electrical parameters such as surface resistance, substrate resistance, and transition region resistance curves on semiconductors or (EPI) substrate materials, helping to determine whether the silicon wafer meets quality standards and manufacturing requirements.
[0003] Due to process specifications, some silicon wafer processing products typically require a super back-sealing process (i.e., LTO+POLY) for back sealing. The drawback is that the outermost structure of this process is a POLY layer. If there is metal contamination (especially boron and phosphorus metals) beneath the POLY layer during deposition, these contaminants will gradually diffuse from the POLY layer towards the front edge of the silicon wafer during epitaxy at high temperatures. This leads to abnormal surface resistivity (SRP) tests at the front edge of the wafer and poor overall in-plane resistivity uniformity. Since cleanrooms in silicon wafer processing cannot currently guarantee the complete absence of boron and phosphorus metals, products using super back sealing are highly susceptible to edge SRP anomalies caused by metal contamination after epitaxy.
[0004] Therefore, in view of the above shortcomings, a new method is needed to solve the existing problems. Summary of the Invention
[0005] The technical problem to be solved by this invention is the abnormal SRP collapse at the edge of the existing silicon wafer back sealing process. In view of the defects in the prior art, this invention provides a method for silicon wafer back sealing.
[0006] To address the aforementioned technical problems, this invention provides a method for back-sealing a silicon wafer, the method comprising the following steps:
[0007] (1) Deposit an LTO film on the back of the silicon wafer;
[0008] (2) A POLY film is deposited on the LTO film surface from step (1);
[0009] (3) Deposit an LTO film on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0010] The existing silicon wafer super back-sealing process structure is LTO (silicon dioxide) + POLY (polycrystalline silicon). The outermost POLY film is a polycrystalline silicon structure composed of many smaller silicon crystals. Because current cleanrooms in silicon wafer processing cannot guarantee the complete absence of metal elements such as boron (B) and phosphorus (Ph), if there are metal impurities (especially B and Ph) under the POLY layer during the POLY film deposition process, these impurities will gradually diffuse from the interior of the POLY layer towards the edge of the silicon wafer during epitaxy at high temperatures. This leads to abnormal SRP (Surface Resistivity) tests at the edge of the silicon wafer, resulting in poor overall in-plane resistivity uniformity. The closer to the edge of the silicon wafer, the more pronounced the SRP collapse. (See attached image) Figure 1 As shown, the SRP (Surface Reinforced Polymer) in the central region of the silicon wafer hardly collapses, slight SRP collapse occurs 10mm from the edge, and severe SRP collapse occurs 3mm from the edge. Taking the presence of P contamination under the POLY layer of the super back seal as an example, as shown in the attached diagram... Figure 2 As shown ( Figure 2 In the context of EPI (Extravitational Phase I), during the high-temperature epitaxial process, P will move from the position below the POLY layer to the edge of the POLY layer and diffuse to the front edge of the silicon wafer, causing a deviation in the resistivity of the silicon wafer edge and triggering an abnormal SRP collapse at the edge.
[0011] This invention introduces a novel back-sealing process: LTO+POLY+LTO. Building upon existing super-sealing (LTO+POLY) processes, an additional LTO film is deposited for back sealing. This encapsulates the exposed POLY film layer, preventing metal impurities adsorbed within the POLY layer from diffusing even at high temperatures. This solves the problem of edge SRP abnormalities caused by metal contamination that easily occurs in super-sealed products after epitaxy. This invention is highly innovative and practical. (See attached diagram.) Figure 3 As shown ( Figure 3 In this context, CVD stands for Chemical Vapor Deposition.
[0012] Specifically, taking the presence of P contamination beneath the POLY layer of a super-sealed product as an example, as shown in the attached... Figure 4 As shown ( Figure 4 In this context, EPI stands for epitaxy. Based on the original LTO+POLY layer super back-sealing process, an additional LTO layer is added to protect the POLY layer, i.e., LTO+POLY+LTO process. Even after a high-temperature epitaxial process, the phosphorus element under the POLY layer can only diffuse through the POLY film and cannot penetrate the outermost LTO film. This process has a better back-sealing effect when there is phosphorus contamination in the silicon wafer and solves the problem of abnormal edge SRP after epitaxy of super back-sealed products.
[0013] Preferably, the thickness of the LTO film in step (1) is 4000 to 6000 angstroms, for example, it can be 4000 angstroms, 4500 angstroms, 5000 angstroms, 5500 angstroms or 6000 angstroms.
[0014] Preferably, the thickness of the POLY film in step (2) is 6500 to 9500 angstroms, for example, it can be 6500 angstroms, 7000 angstroms, 7500 angstroms, 8000 angstroms, 8500 angstroms or 9000 angstroms.
[0015] Preferably, the thickness of the LTO film in step (3) is 3500 to 5500 angstroms, for example, it can be 3500 angstroms, 4000 angstroms, 4500 angstroms, 5000 angstroms or 5500 angstroms.
[0016] In this invention, the main purpose of step (3) is to wrap the inner POLY layer, which will reduce the thickness without affecting the effect, thus reducing the cost.
[0017] Preferably, the deposition method described in steps (1), (2), and (3) is chemical vapor deposition.
[0018] Implementing this invention has the following beneficial effects:
[0019] This invention proposes an LTO+POLY+LTO process for silicon wafer back sealing. Even after a high-temperature epitaxial process, the phosphorus element under the POLY layer can only diffuse through the POLY film and cannot penetrate the outermost LTO film. This process has a better back sealing effect when there is phosphorus contamination in the silicon wafer. It solves the problem of abnormal SRP at the edge after epitaxy of super-sealed products. After the silicon wafer products are sent to the customer for epitaxy, the uniformity of resistivity in the silicon wafer surface is 2% to 4%, and there are no abnormalities in the SRP characteristic curve. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of SRP collapse at the edge of a silicon wafer using existing back-sealing technology.
[0021] Figure 2 This is a schematic diagram of the diffusion of phosphorus (P) under the POLY layer in the silicon wafer epitaxial process using existing back-sealing technology.
[0022] Figure 3 This is a schematic diagram comparing the existing back sealing process with the new back sealing process provided by this invention.
[0023] Figure 4 This is a schematic diagram of the diffusion of P element under the POLY layer during the epitaxial process after the back sealing process provided by the present invention. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] Example 1
[0026] This embodiment provides a back-sealed silicon wafer.
[0027] (1) A layer of LTO film with a thickness of 5000 angstroms is deposited on the back side of the silicon wafer;
[0028] (2) A POLY film with a thickness of 7500 angstroms is deposited on the LTO film surface in step (1);
[0029] (3) A layer of LTO film with a thickness of 4500 angstroms is deposited on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0030] Example 2
[0031] This embodiment provides a back-sealed silicon wafer.
[0032] (1) A layer of LTO film with a thickness of 4000 angstroms is deposited on the back side of the silicon wafer;
[0033] (2) A POLY film with a thickness of 6500 angstroms is deposited on the LTO film surface in step (1);
[0034] (3) A layer of LTO film with a thickness of 3500 angstroms is deposited on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0035] Example 3
[0036] This embodiment provides a back-sealed silicon wafer.
[0037] (1) A layer of LTO film with a thickness of 6000 angstroms is deposited on the back side of the silicon wafer;
[0038] (2) A POLY film with a thickness of 9500 angstroms is deposited on the LTO film surface in step (1);
[0039] (3) Deposit an LTO film with a thickness of 5500 angstroms on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0040] Example 4
[0041] This embodiment provides a back-sealed silicon wafer.
[0042] (1) A layer of LTO film with a thickness of 4500 angstroms is deposited on the back side of the silicon wafer;
[0043] (2) A POLY film with a thickness of 8000 angstroms is deposited on the LTO film surface in step (1);
[0044] (3) Deposit an LTO film with a thickness of 4000 angstroms on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0045] Example 5
[0046] This embodiment provides a back-sealed silicon wafer.
[0047] (1) A layer of LTO film with a thickness of 5500 angstroms is deposited on the back side of the silicon wafer;
[0048] (2) A POLY film with a thickness of 9000 angstroms is deposited on the LTO film surface in step (1);
[0049] (3) Deposit an LTO film with a thickness of 5000 angstroms on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0050] Example 6
[0051] This embodiment provides a back-sealed silicon wafer.
[0052] (1) A layer of LTO film with a thickness of 3000 angstroms is deposited on the back side of the silicon wafer;
[0053] (2) A POLY film with a thickness of 5000 angstroms is deposited on the LTO film surface in step (1);
[0054] (3) A layer of LTO film with a thickness of 3000 angstroms is deposited on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0055] Example 7
[0056] This embodiment provides a back-sealed silicon wafer.
[0057] (1) A layer of LTO film with a thickness of 7000 angstroms is deposited on the back side of the silicon wafer;
[0058] (2) A POLY film with a thickness of 10,000 angstroms is deposited on the LTO film surface in step (1);
[0059] (3) An LTO film with a thickness of 8000 angstroms is deposited on the POLY film surface in step (2) to obtain a back-sealed silicon wafer.
[0060] Comparative Example 1
[0061] The only difference between this comparative example and Example 1 is that this comparative example does not include step (3), while the rest are the same as Example 1.
[0062] The silicon wafers provided in Examples 1-7 and Comparative Example 1 were subjected to tests on the in-plane resistivity uniformity and SRP characteristic curves.
[0063] Resistivity uniformity test method: The lateral resistivity of the epitaxial layer is measured using a four-probe method, with 9 points tested per wafer using a cross-hatching method. The resistivity uniformity is calculated from the resistivity values at these 9 points. Test standard: Resistivity uniformity RRG < 5%. Because there are differences in resistivity uniformity between each silicon wafer, the data obtained through this test refers to the resistivity uniformity value of an entire batch of products; therefore, RRG is a range value.
[0064] SRP testing method: Use an extended resistivity tester to test the longitudinal resistivity of the epitaxial layer; SRP testing standard: Observe the SRP characteristic curve for obvious bulges or collapses.
[0065] The results are shown in Table 1.
[0066] Table 1
[0067]
[0068] The data in the table shows that the back sealing process provided by this invention has good performance, with good uniformity of internal resistivity after silicon wafer epitaxy and no abnormalities in the SRP characteristic curve. Compared with existing processes, it has better performance.
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for back-sealing a silicon wafer, characterized in that: The method includes the following steps: (1) Deposit an LTO film on the back side of the silicon wafer; (2) A POLY film is deposited on the LTO film surface in step (1); (3) An LTO film is deposited on the POLY film surface in step (2) to obtain a back-sealed silicon wafer; the LTO film is used to seal the P impurities inside the POLY film layer inside the POLY film to eliminate the abnormal SRP collapse at the edge of the silicon wafer. The thickness of the LTO film in step (1) is 4000~6000 angstroms; the thickness of the POLY film in step (2) is 6500~9500 angstroms; the thickness of the LTO film in step (3) is 3500~5500 angstroms; The deposition method described in steps (1), (2), and (3) is chemical vapor deposition.
Citation Information
Patent Citations
Semiconductor device and preparation method thereof
CN115763386A