A kind of heat insulation flame retardant coating and preparation method thereof

Prepared by the chemical grafting method of nano-metal oxide and other components, the problem of existing transparent heat-insulating coatings being ineffective in shielding infrared and ultraviolet rays is solved, and efficient heat-insulating and flame-retardant properties are achieved, making it suitable for industrial production.

CN116751492BActive Publication Date: 2024-10-15ZHUHAI TAIRAN TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310867345.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-14
Publication Date
2024-10-15
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

Existing transparent thermal insulation coatings have limited effectiveness in shielding infrared and ultraviolet rays, and the nanoparticles have poor dispersion and poor stability during the preparation process, resulting in poor thermal insulation effect and flame retardant performance, and are not suitable for industrial mass production.

Method used

Using nanometer metal oxide, silane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, vinyl methacrylate, glycidyl methacrylate, methacrylic acid Ethylized caged silsesquioxane, azobisisobutyronitrile, nano-antimony-doped tin oxide, nano-lanthanum hexaboride and other components are used to prepare heat-insulating and flame-retardant coatings through chemical grafting methods to achieve UV protection. and near-infrared light shielding.

Benefits of technology

It achieves effective shielding of ultraviolet and near-infrared light, improves the transparency, mechanical properties and thermal insulation and flame retardant properties of the coating, reduces the energy consumption of the production process, and is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116751492B_ABST
    Figure CN116751492B_ABST
Patent Text Reader

Abstract

The invention discloses a heat-insulating flame-retardant coating and a preparation method thereof, wherein the coating comprises nano metal oxide, silane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, vinyl methacrylate, glycidyl methacrylate, methacrylate ethylated cage-shaped silsesquioxane, azobisisobutyronitrile, nano antimony-doped tin oxide, nano lanthanum hexaboride, and an organic solvent. The preparation method comprises polymerizing nano metal oxide and silane coupling agent to obtain suspension A; polymerizing 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and vinyl methacrylate to obtain solution B; reacting glycidyl methacrylate and methacrylate ethylated cage-shaped silsesquioxane with suspension A and solution B; adding nano antimony-doped tin oxide and nano lanthanum hexaboride for dispersion and mixing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coating materials, and particularly relates to a heat-insulating flame-retardant coating and a preparation method thereof. Background Art

[0002] As the earth's environmental temperature continues to rise and energy is increasingly depleted, healthy, environmentally friendly, heat-insulating and energy-saving coatings are becoming more and more popular. At the same time, modern building materials or other industries also put forward high requirements on the flame retardant properties of coatings. Therefore, it is of great significance to develop coatings with both heat-insulating and flame-retardant functions. Under sunlight, some large open-air equipment will produce various losses due to excessive temperature. For example, aviation fuel storage tanks will produce aviation fuel evaporation losses due to excessive temperature, and the safe operation of civil aviation has high requirements for the fire retardancy of structural materials used in aviation fuel storage areas. Therefore, the development of a coating that can be applied on the outer surface of aviation fuel storage tank equipment and has good heat-insulating and flame-retardant properties not only helps to reduce the evaporation loss of aviation fuel, but also can enhance the fire resistance limit of the storage tank structure, and further improve the fire safety of aviation fuel storage. Not only that, this type of heat-insulating and flame-retardant coating also has a relatively broad application prospect in related fields such as large buildings, pipelines, bridges, etc.

[0003] The radiation band from the sun to the ground ranges from about 200 to 2500nm, of which 200 to 400nm is ultraviolet light, 400 to 800nm ​​is visible light, and 800 to 2500nm is near infrared light, which can be divided into short-wave near infrared (800 to 1100nm) and long-wave near infrared (1100 to 2500nm). The human eye can only directly perceive visible light. Therefore, in order to achieve the purpose of heat insulation and energy saving while making the material transparent, it is necessary to shield infrared and ultraviolet light as much as possible and only allow visible light to pass through.

[0004] Existing transparent heat insulation technologies mostly use ITO and ATO as shielding materials, but these two materials can only shield long-wave near-infrared, and have no obvious barrier to short-wave near-infrared and ultraviolet rays, so the energy-saving effect is limited. Most of the thermal insulation coatings on the market are prepared by physically blending thermal insulation nanomaterials with different polymer film-forming agents (such as water-based polyurethane and water-based polyacrylate). These blending systems have problems such as poor dispersion and stability of nanoparticles and easy agglomeration, resulting in poor thermal insulation effect of the coatings. In addition, the moldability and adhesion of water-based coatings are poor, and the energy consumption is high during use, which is not suitable for large-scale industrial production. Chinese invention patent CN102746781A discloses a fully infrared and ultraviolet shielding polyurethane nano transparent heat-insulating coating and its preparation method. The coating has a basic formula of 40% to 80% polyurethane resin, 5% to 30% nano ATO dispersion, 1% to 10% nano LaB6 dispersion, 1% to 15% nano WO3 dispersion, 0.5% to 3% additive and 5% to 20% solvent by weight percentage. The coating can shield long-wave near-infrared, but the transmittance of the coating to visible light between 400 to 500nm and 700 to 800nm ​​is less than 30%. The preparation process adopts a physical blending method, which has poor dispersibility and stability, high haze after film formation, and poor transparency and mechanical properties. In addition, the heat-insulating and flame-retardant effect of the coating is not good, which has certain restrictions on its application field. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a heat-insulating flame-retardant coating which can shield infrared rays and ultraviolet rays and has high transparency.

[0006] The technical solution adopted by the present invention is:

[0007] A heat-insulating flame-retardant coating comprises the following components: nano metal oxide, silane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, vinyl methacrylate, glycidyl methacrylate, ethyl methacrylate cage-shaped silsesquioxane, azobisisobutyronitrile, nano antimony-doped tin oxide, nano lanthanum hexaboride and organic solvent.

[0008] Furthermore, the molar ratio of the nano metal oxide, the silane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, vinyl methacrylate, glycidyl methacrylate, and ethyl methacrylate cage-shaped silsesquioxane is 2:2:2:2:2:1.

[0009] Furthermore, the mass fractions of azobisisobutyronitrile, nano antimony-doped tin oxide, and nano lanthanum hexaboride are 0.05%, 1.5%, and 1.5%, respectively.

[0010] Furthermore, the nano metal oxide is a mixture of any one or more of nano zinc oxide, nano titanium dioxide, nano vanadium oxide, nano aluminum oxide, and nano iron oxide in any proportion.

[0011] Furthermore, the silane coupling agent is a mixture of any one or more of KH-570, KH-A172, A151, and KH171 in any proportion.

[0012] Furthermore, the particle size of the nano metal oxide is 15 to 30 nm.

[0013] A method for preparing a thermal insulation coating comprises the following steps:

[0014] (1) Dispersing nano-metal oxide in an anhydrous ethanol solution, adding a silane coupling agent, heating to T1 and stirring at a constant temperature until the ethanol is completely evaporated, washing the obtained nanoparticles to remove impurities, and then adding them to anhydrous ethanol for dispersion to obtain a suspension A.

[0015] (2) Add flame retardant 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) to an appropriate amount of organic solvent, heat and stir under nitrogen protection until DOPO is completely dissolved, add vinyl methacrylate, and react for a period of time. After cooling to room temperature, remove the solvent by evaporation, then add anhydrous ethanol, heat to T2 and stir at a constant temperature to obtain solution B.

[0016] (3) Glycidyl methacrylate and ethyl methacrylate cage-shaped silsesquioxane are dissolved in anhydrous ethanol, and then the suspension A and solution B are added and stirred thoroughly. Azobisisobutyronitrile is added and stirred continuously. The solution obtained after the polymerization reaction is recorded as solution C.

[0017] (4) Add nano antimony-doped tin oxide and nano lanthanum hexaboride to solution C, and stir at room temperature until they are completely dispersed to obtain a heat-insulating flame-retardant coating.

[0018] The constant temperature stirring temperature T1 in step (1) is 45°C.

[0019] The organic solvent in step (2) is a mixture of equal volumes of xylene and tetrahydrofuran.

[0020] The constant temperature stirring temperature T2 in step (2) is 60°C.

[0021] The order of step (1) and step (2) can be swapped without any impact on the preparation process, cost and performance of the final prepared coating.

[0022] The heat-insulating flame-retardant coating provided by the present invention shields the ultraviolet light through nano metal oxides, and simultaneously introduces nano antimony-doped tin oxide and nano lanthanum hexaboride to achieve a nearly complete shielding effect on the near-infrared light region (short wave and long wave).

[0023] The heat-insulating flame-retardant coating provided by the present invention has a simple production process and low energy consumption. The chemical grafting method is adopted to form a high molecular polymer material by linking double bonds of nano zinc oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), and ethyl methacrylate cage-shaped silsesquioxane respectively for nano-modification and then grafting copolymerization. The nanoparticles have good dispersibility and stability, and the material has excellent light transmission, flame retardant and heat insulation properties, and the film forming degree and mechanical properties of the material are better; DOPO has flame retardancy, but the addition of DOPO will increase the haze of the coating after film formation, resulting in a decrease in the transparency of the material. The coating of the present invention is added with DOPO to link double bonds with vinyl methacrylate, and then grafted with double bonds in other components of the coating to polymerize, so that the material has flame retardancy and can also enhance the mechanical properties of the material. The heat-insulating flame-retardant coating provided by the present invention can make the glass have a selective transmission function for the spectrum, and can block infrared light, far infrared light, ultraviolet light, and heat radiation while being able to transmit most of the visible light without affecting the lighting. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram comparing the ultraviolet-visible-infrared transmission spectra of the coating formed after the heat-insulating flame-retardant coating is coated on the glass according to the embodiment of the present invention and the original glass without coating.

[0025] Figure 2 It is a schematic diagram comparing the heat release rate curves of the PU foam coated with the heat-insulating flame-retardant coating according to an embodiment of the present invention and the original PU foam without coating.

[0026] Figure 3 It is a schematic diagram comparing the total heat release curves of the PU foam coated with the heat-insulating flame-retardant coating according to an embodiment of the present invention and the original PU foam without coating.

[0027] Figure 4 It is a comparative schematic diagram of adhesion test between the heat-insulating flame-retardant paint coating according to an embodiment of the present invention and the paint coating prepared by the physical blending method. DETAILED DESCRIPTION

[0028] The specific implementation of the present invention is described in detail below in conjunction with specific implementation examples, but the present invention is not limited to the given examples.

[0029] A heat-insulating flame-retardant coating comprises the following components: 0.1 mol of nano zinc oxide, 0.1 mol of silane coupling agent KH-570, 0.1 mol of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 0.1 mol of vinyl methacrylate, 0.1 mol of glycidyl methacrylate, 0.05 mol of ethyl methacrylate cage-shaped silsesquioxane, azobisisobutyronitrile, nano antimony-doped tin oxide, nano lanthanum hexaboride and an appropriate amount of solvent.

[0030] The specific preparation method of the heat-insulating flame-retardant coating provided by the present invention is as follows:

[0031] (1) Take 0.1 mol of nano ZnO (particle size: 15-30 nm) and disperse it in an appropriate amount of anhydrous ethanol, then add 0.1 mol of silane coupling agent KH-570, and stir evenly under a constant temperature of 45°C until the ethanol is completely evaporated. The obtained nano KH-570@ZnO particles are rinsed with deionized water 3 times and anhydrous ethanol once. Then the nanoparticles are added to 100 ml of anhydrous ethanol and ultrasonically dispersed for 30 minutes to obtain a nanoparticle suspension, which is recorded as solution A.

[0032] (2) Take 0.1 mol of flame retardant 9,10-dihydro-9-11.2-oxa-10-phosphaphenanthrene-10-oxide (DOPO), add 30 ml of xylene and 30 ml of tetrahydrofuran as solvent. After heating to 80°C and stirring under a nitrogen atmosphere until DOPO is completely dissolved, add 0.1 mol of vinyl methacrylate and keep the reaction mixture at this temperature for 20 hours. After cooling to room temperature, remove the solvent by vacuum rotary evaporation. Then add 100 ml of anhydrous ethanol and stir thoroughly at 60°C until dissolved to obtain solution B.

[0033] (3) Dissolve 0.1 mol of glycidyl methacrylate and 0.05 mol of ethyl methacrylate cage-shaped silsesquioxane in 100 ml of anhydrous ethanol, add solution A and solution B, and stir thoroughly. Add 0.05 wt% of azobisisobutyronitrile to the resulting solution, and continue stirring at 45° C. for 2 hours. The solution obtained after the polymerization reaction is recorded as solution C.

[0034] (4) Weigh 1.5 wt% of nano antimony-doped tin oxide and 1.5 wt% of nano lanthanum hexaboride, which are equivalent to the weight of solution C, and add them to solution C. Stir at room temperature until they are completely dispersed to obtain the final coating.

[0035] After adding 10-15 wt% of curing agent hexamethylenediamine to the above coating, the coating was sprayed on the glass surface to form a heat-insulating and flame-retardant transparent coating. The optical properties, heat-insulating properties and flame-retardant properties of the coating were then tested respectively.

[0036] (1) Optical performance test of coating

[0037] The optical properties (UV, near infrared shielding and visible light transmission) of the coating were tested using a UV-Vis / NIR spectrophotometer (UV-Vis / NIR, Shimadzu, Japan, UV-3600i Plus). The transmittance of the original glass sample (Pristine glass) and the coated glass sample (Coated glass) was tested in the wavelength range of 200-2200nm.

[0038] like Figure 1 As shown in the test of the original glass sample and the coating sample, it can be seen that the transmittance of the coated glass sample in the ultraviolet light region (200-400nm) and the near infrared light region (800-2200nm) is significantly lower than that of the original glass sample, which shows that after the modification of the coating, the ultraviolet and near infrared in the incident sunlight can be effectively shielded. For the visible light region (400-800nm), the average transmittance can be maintained above 75%, indicating that the coating does not affect the visualization of the glass.

[0039] (2) Thermal insulation performance test of coating

[0040] The thermal insulation performance of the coating is tested by infrared heating test. Specifically, by applying a constant power of 1kW infrared light (wavelength of about 950nm) on one side of the coated glass sample for 30 seconds, the temperature of the other side of the coated glass sample is continuously measured, and the initial temperature and peak temperature are measured. At the same time, the original sample is tested in the same way. The calculation of the heat barrier rate is based on the following formula:

[0041]

[0042] Where δT C is the difference between the temperature of the coated glass sample after the test and the temperature before the test, ΔT amb It is the difference between the air temperature after the test and the temperature before the test.

[0043] In the test device, the infrared lamp is located at the top and irradiates downward, the temperature sensor is at the bottom, and the initial temperature is 25.4°C. After 30 seconds of heating, the temperature in the air chamber rises to 48.1°C, and the temperature on the lower side of the coated glass sample rises to 27.2°C, and the insulation efficiency is about 92.14%.

[0044] (3) Flame retardant performance test of coating

[0045] Determination of Limit Oxygen Index (LOI): The Limit Oxygen Index refers to the volume fraction concentration of oxygen in a mixture of oxygen and nitrogen when the sample being tested is just able to support its combustion. It is an index that characterizes the combustion behavior of the material. The determination process is carried out using a Limit Oxygen Index instrument, and the selected test samples are the original polyurethane (PU) foam and the PU foam soaked in the coating. The test is carried out in accordance with GB / T2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method Part 2: Room Temperature Test" / ISO:4589-1.

[0046] Table 1. Determination of the limiting oxygen index.

[0047]

[0048] It is generally believed that materials with an oxygen index of less than 22% are flammable materials, materials with an oxygen index between 22% and 27% are combustible materials, and materials with an oxygen index of more than 27% are flame-retardant materials. The average limiting oxygen index of the coated PU foam reached 27.41%, which is in the flame-retardant category, indicating that the coating has good flame retardant properties.

[0049] Determination of Heat Release Rate (HRR): Heat release rate refers to the amount of heat released per unit time by a material when it burns under specified conditions. The determination process is carried out in a cone calorimeter. In this test, we also selected PU foam as the base material and measured the heat release rates of the original PU foam and the coated PU foam at different test times in the cone calorimeter test.

[0050] Determination of total heat release (THR): the integral value of the heat release rate within a specified time.

[0051] like Figure 2 As shown in the figure, the peak heat release rate of the PU foam sprayed with the coating is only 38% of that of the original PU foam, indicating that the coating can greatly reduce the speed of heat release during combustion and reduce the peak value of the rate, which can be specifically manifested as a lower total amount of heat release through integration. Figure 3 As shown, the total heat release of the spray-coated PU foam is significantly less than that of the original PU foam.

[0052] (4) Mechanical properties test of coating

[0053] The adhesion of the coating is tested according to ASTM D3359. The interval between each blade of the grid cutter is 1 mm, so the area of ​​each grid obtained by cutting is about 1 square millimeter. Place the center of the 3M tape at the intersection of the cut, smooth the tape in the cut area with your fingers, and roll it back and forth with a 2kg load to make the tape completely adhere to the sample. The color change of the transparent tape can represent whether the tape is in good contact with the sample. Within 90 seconds, grab one end of the tape and pull it away as quickly as possible at an angle of 180° to remove the tape. Then observe the shedding of the coating surface to evaluate the adhesion of the coating.

[0054] Conventional physical blending method for preparing coating: weigh 0.1mol nano ZnO (particle size: 15-30nm), 0.1mol silane coupling agent KH-570, 0.1mol flame retardant 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 0.1mol vinyl methacrylate, 0.05mol methacrylate ethyl ester cage-shaped silsesquioxane (ME-POSS) and dissolve in 300mL anhydrous ethanol, stir for 2 hours, weigh 1.5wt% nano antimony doped tin oxide (ATO) and 1.5wt% nano lanthanum hexaboride (LaB6) and add them to the solution, stir at room temperature until completely dispersed, and obtain the final coating. After adding 10-15wt% curing agent hexamethylenediamine, spray curing to obtain the final coating.

[0055] Under the same conditions, the coating prepared by the chemical grafting method of the present invention and the coating prepared by the conventional physical blending method were tested by ASTM D3359. The test results are shown in Figure 4 .

[0056] like Figure 4 As shown, the coating prepared by the chemical grafting method of the present invention has almost no coating shedding, and the overall peeling rate is less than 5%, which meets the ASTM 5B standard. In contrast, the mechanical properties of the coating prepared by the physical blending method are poor, with more coating shedding and overall lattice shedding, which can only meet the ASTM 1B standard. It can be seen that in terms of coating adhesion, the coating prepared by the chemical grafting method has better mechanical properties.

[0057] The present invention has been described in detail above in conjunction with specific embodiments. However, the present invention is not limited to the above description. Various changes made within the knowledge of those skilled in the art without departing from the concept of the present invention still fall within the protection scope of the present invention.

Claims

1. A heat-insulating flame-retardant coating, characterized in that: The preparation raw materials include the following components: nano metal oxide, silane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, vinyl methacrylate, glycidyl methacrylate, methacrylate ethylated cage-shaped silsesquioxane, azobisisobutyronitrile, nano antimony doped tin oxide, nano lanthanum hexaboride, and organic solvent; the molar ratio of the nano metal oxide, silane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, vinyl methacrylate, glycidyl methacrylate, and methacrylate ethylated cage-shaped silsesquioxane is 2:2:2:2:2:1; and the preparation method includes the following steps: (1) dispersing nano-metal oxide in an anhydrous ethanol solution, adding a silane coupling agent, heating to T1 and stirring at a constant temperature until the ethanol is completely evaporated to obtain nanoparticles, washing the obtained nanoparticles to remove impurities, and then adding them to anhydrous ethanol for dispersion to obtain a suspension A; (2) adding a flame retardant 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to an appropriate amount of an organic solvent, heating and stirring under nitrogen protection until the 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is completely dissolved, adding vinyl methacrylate, reacting for a period of time, cooling to room temperature, removing the solvent by evaporation, and then adding anhydrous ethanol, heating to T2 and stirring at a constant temperature to obtain a solution B; (3) dissolving glycidyl methacrylate and ethyl methacrylate cage-shaped silsesquioxane in anhydrous ethanol, adding suspension A and solution B, stirring thoroughly, adding azobisisobutyronitrile, stirring continuously, and the solution obtained after the polymerization reaction is recorded as solution C; (4) Add nano antimony-doped tin oxide and nano lanthanum hexaboride to solution C, and stir at room temperature until they are completely dispersed to obtain a heat-insulating flame-retardant coating.

2. The heat-insulating flame-retardant coating according to claim 1, characterized in that: The mass fractions of azobisisobutyronitrile, nano antimony-doped tin oxide and nano lanthanum hexaboride are 0.05%, 1.5% and 1.5% respectively.

3. The heat-insulating flame-retardant coating according to claim 1, characterized in that: The nano metal oxide is a mixture of any one or more of nano zinc oxide, nano titanium dioxide, nano aluminum oxide, and nano iron oxide in any proportion.

4. The heat-insulating flame-retardant coating according to claim 1, characterized in that: The silane coupling agent is a mixture of any one or more of KH-570, A172, A151, and KH171 in any proportion.

5. The heat-insulating flame-retardant coating according to claim 1, characterized in that: The particle size of the nano metal oxide is 15-30 nm.

6. The heat-insulating flame-retardant coating according to claim 1, characterized in that: The constant temperature stirring temperature T1 in step (1) is 45°C.

7. The heat-insulating flame-retardant coating according to claim 1, characterized in that: The organic solvent in step (2) is a mixture of equal volumes of xylene and tetrahydrofuran.

8. The heat-insulating flame-retardant coating according to claim 1, characterized in that: The constant temperature stirring temperature T2 in step (2) is 60°C.

Citation Information

Patent Citations

  • Full-shielded infrared and ultraviolet polyurethane nanometer transparent heat insulating coating

    CN102746781A

  • Method for preparing phosphorus-containing flame-retardant acrylic resin

    CN105237674A

  • Ultraviolet isolation type high-transparency temperature control glass coating and preparation method

    CN108504275A

  • Preparation method of heat-insulation coating

    CN108659635A

  • Nanometer thermal insulation paint for glass coating and preparation method

    CN108948881A