A medical biodegradable dressing and preparation method thereof
By combining traditional Chinese medicine extracts with cellulase and pectinase, combined with polylactic acid and soybean lecithin, and using electrospinning technology to prepare a double-layer dressing, the problems of non-biodegradability and poor breathability of existing dressing materials are solved. It achieves biodegradability and long-lasting effect of drug release, and significantly improves the environmental protection and antibacterial effect of the application.
Patent Information
- Application Number
- CN202310842053.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-07-11
AI Technical Summary
Existing medical dressing materials are not biodegradable, have poor air permeability, cause environmental pollution after use, and the active ingredients of traditional Chinese medicine are easily lost.
The traditional Chinese medicine modified fiber is prepared by treating Chinese medicine extract with cellulase and pectinase, combined with polylactic acid and soybean lecithin, and using electrospinning technology to prepare a double-layer dressing. The outer layer uses a blown film and the inner layer uses electrostatic Spun fiber membrane ensures the breathability and drug release effect of the application.
It achieves the biodegradability, breathability and long-lasting effect of drug release of medical dressings, reduces the use cost of polylactic acid, and significantly improves the environmental protection and antibacterial effect of the dressing.
Smart Images

Figure CN116763974B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the medical field, and in particular to a medical biodegradable dressing and a preparation method thereof. Background Art
[0002] Currently, most medical dressings such as wound patches, indwelling needle fixations, and navel patches are made of PU or PE non-woven fabrics, which are non-biodegradable and have poor air permeability. Long-term use can easily cause skin damage and produce white waste after use, polluting the environment.
[0003] White pollution, such as plastic products, will occupy a large amount of land and destroy the soil structure when buried, which will affect the growth of crops; incineration will produce highly toxic dioxins, polluting the atmosphere and damaging the growth of animals and plants; in the process of garbage dumping or filling pits, a large amount of acidic and alkaline organic pollutants will be produced, which will seep into the ground and pollute groundwater sources.
[0004] Medical supplies, in particular, are mostly non-recyclable and reusable. In order to avoid the spread of disease due to incomplete cleaning during the disposal process, it is urgent to use a degradable material as a substitute.
[0005] We know that after the effective ingredients of traditional Chinese medicine are extracted, the fibrous residues are often discarded, resulting in a great waste of resources. The fibrous residues are plant fibers. Since plant fibers are green natural polymer materials with a multi-level microstructure, if they can be added to medical dressings, it will be environmentally friendly and reduce the cost of using polylactic acid PLA. Therefore, the applicant of the present invention further conducted research and development. Summary of the invention
[0006] The first technical problem to be solved by the present invention is to provide a method for preparing a medical biodegradable patch. The method is simple to operate and the raw materials used are degradable, which solves the problem that the materials used in previous preparation methods are non-degradable and pollute the environment. In addition, the patch prepared by this method solves the problems of poor air permeability, non-degradability, and easy loss of effective ingredients of traditional Chinese medicine in previous medical patches.
[0007] To solve the above-mentioned first technical problem, the technical solution of the present invention is: a method for preparing a medical biodegradable dressing, comprising the following steps:
[0008] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, hot-extracting with anhydrous ethanol at 60° C. for 1.5 to 3 h to obtain an extract and a residue, and performing reduced pressure rotary evaporation on the extract at 60° C. to remove the solvent to obtain an extract of effective components of traditional Chinese medicine;
[0009] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 35-42°C for 2-3h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 2-5h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding to crush into Chinese medicine fiber with a particle size of 50-80μm, finally mixing the Chinese medicine fiber with a silane coupling agent, and heat treating at 100°C in a high-speed mixer for 20min to obtain the modified Chinese medicine fiber;
[0010] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heat-treated at 90°C for 18 minutes to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0011] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and compatibilizer are mixed in a mass ratio of (35-50): (30-40): (5-10): (5-10): (1-5), and then granulated, blown film, and rolled to obtain an outer layer blown film; (b) Preparation of inner layer electrospun film: polylactic acid and soybean lecithin are placed in an electrostatic spinning film. In the electrospinning machine, a solvent is added, heated and stirred to dissolve, and then the extract of the Chinese medicine functional component is dripped in, the mass ratio of polylactic acid, soybean lecithin, and the extract of the Chinese medicine functional component is 100: (5-15): (3-10), and the solution is stirred while dripping to obtain an electrospinning solution, and electrospinning is performed on the outer layer blown film, combined with a pressure-sensitive adhesive and a release paper to obtain a double-layer medical biodegradable patch, the surface density of which is 50-100 g / m 2 .
[0012] Preferably, the traditional Chinese medicine in step 1) is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1.
[0013] Preferably, the mass ratio of the traditional Chinese medicine fiber to the silane coupling agent in step 2) is 100:(1-5).
[0014] Preferably, the granulation temperature for preparing the outer layer blown film in step 4) is 170-190°C, and the film blowing temperature is 165-185°C.
[0015] Preferably, the solvent in step 4) is one or more of N,N-dimethylformamide, dichloromethane, chloroform, and acetone.
[0016] Preferably, in the step 4), the heating temperature after adding the solvent to prepare the inner electrospinning membrane is 40-50° C., stirring is 2-4 hours, and the stirring speed is 600-1000 r / min.
[0017] Preferably, the electrospinning conditions in step 4) are as follows: voltage 10-20 kV, spinning flow rate 0.4-1.0 mL / h, spinning distance 12-20 cm, spinning solution concentration 8-20%, spinning membrane 40-50°C, heat treatment 4-6 h, spinning diameter 80-150 nm.
[0018] Preferably, the compatibilizer in step 4) comprises one or more of epoxidized soybean oil, stearic acid monoglyceride, maleic anhydride, and citric acid ester.
[0019] After adopting the above-mentioned first technical scheme, the effect of the present invention is: a preparation method of a medical biodegradable patch, the preparation method requires fewer types of raw materials and they are all natural degradable components, will not cause pollution to the environment, and has good environmental protection. The outer layer blown film is made of materials such as Chinese medicine fiber and starch, and is prepared by blow molding, which is both environmentally friendly and can reduce costs. The inner layer electrospinning film is prepared by electrospinning technology, which has both antibacterial effect and is very fit, and has strong air permeability. The soybean lecithin component added to the inner layer electrospinning membrane can effectively distribute hydrophilic and lipophilic components, and can well wrap the extract of Chinese medicine efficacy components. The Chinese medicine efficacy components can be slowly released in the inner layer, which can avoid the problem of damaging the Chinese medicine efficacy components due to the high temperature of the outer layer blown film.
[0020] Since the traditional Chinese medicine in step 1) is a combination of honeysuckle, trichosanthes and isatis root, the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1, and the extracts of the three materials contain flavonoids, chlorogenic acid, sterols, anthraquinones and other substances, all of which have antibacterial effects, and it was found during the research process that this ratio has a good antibacterial effect.
[0021] The following is a description of the performance of the components of the present invention:
[0022] Polylactic acid, as a biopolymer material derived from corn starch, has good biocompatibility and degradability. It can be completely degraded into water and carbon dioxide in the soil and is an environmentally friendly raw material.
[0023] Polybutylene adipate-terephthalate is a thermoplastic biodegradable plastic with good ductility, film-forming properties and elongation at break. It also has good heat resistance and impact resistance. It can reduce the amount of polylactic acid used and make the product have good performance. It is an ideal green and environmentally friendly film packaging material.
[0024] Compatibilizers can improve the incompatibility of different raw materials by blocking or grafting, increase the bonding force between various polymers and small molecules, form a stable structure, and improve the performance of plastics.
[0025] Soybean lecithin has a phospholipid bilayer structure with good hydrophilic and lipophilic properties. It can well wrap the extract of Chinese medicine active ingredients, making it more effectively distributed and combined with the active ingredients, so that the effective ingredients of Chinese medicine can be released lastingly and effectively, thereby achieving the therapeutic effect;
[0026] Both Chinese medicine fiber and Chinese medicine modified fiber are green natural polymer materials with multi-layer microstructure. When added to the outer layer of blown film, waste resources can be recycled, which is both environmentally friendly and can reduce the cost of polylactic acid.
[0027] The second technical problem to be solved by the present invention is: a medical biodegradable dressing, which solves the problems of poor air permeability and non-degradability existing in previous dressings.
[0028] To solve the above-mentioned second technical problem, the technical solution of the present invention is: a medical biodegradable patch, comprising an outer layer blown film and an inner layer electrospun film, the components of the outer layer blown film comprising polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and a compatibilizer; the components of the inner layer electrospun film comprising polylactic acid, soybean lecithin, and an extract of a Chinese medicine active ingredient.
[0029] After adopting the above second technical solution, the effect of the present invention is: a medical biodegradable dressing, which is degradable, has strong air permeability, is not easy to sweat, and has a long-lasting drug release and good effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is the cumulative release rate curve of the drug. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below through specific examples.
[0032] A medical biodegradable dressing and a preparation method thereof, comprising the following steps:
[0033] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, hot-extracting with anhydrous ethanol at 60° C. for 1.5 to 3 h to obtain an extract and a residue, and performing reduced pressure rotary evaporation on the extract at 60° C. to remove the solvent to obtain an extract of effective components of traditional Chinese medicine;
[0034] The above-mentioned Chinese medicine can be selected as a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1. Of course, other Chinese medicine combinations can also be selected according to actual needs to achieve different effects;
[0035] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 35-42°C for 2-3h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 2-5h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding to crush into Chinese medicine fiber with a particle size of 50-80μ0, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, to obtain modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:(1-5);
[0036] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0037] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and compatibilizer are mixed in a mass ratio of (35-50): (30-40): (5-10): (5-10): (1-5), and then granulated, blown film, and rolled to obtain an outer layer blown film, wherein the granulation temperature is 170-190°C, and the blowing temperature is 165-185°C; (b) Preparation of inner layer electrospun film: polylactic acid and soybean lecithin are placed in an electrospinning machine, a solvent is added, heated and stirred to dissolve, and then the extract of the Chinese medicine active ingredient is added. The mass ratio of polylactic acid, soybean lecithin and extract of Chinese medicinal active ingredient is 100:(5-15):(3-10), and stirring is performed while dropping to obtain an electrospinning solution. The electrospinning conditions are as follows: voltage 10-20 kV, spinning flow rate 0.4-1.0 mL / h, spinning distance 12-20 cm, spinning solution concentration 8-20%, spinning membrane 40-50 ° C, heat treatment 4-6 h, spinning diameter 80-150 nm, electrospinning is performed on the outer layer blown film, combined with pressure-sensitive adhesive and release paper, etc., to obtain a double-layer medical biodegradable dressing, and the surface density of the dressing is 50-100 g / m 2 .
[0038] The heating temperature for preparing the inner electrospinning membrane in step 4) is 40-50° C., stirring is 2-4 hours, the stirring speed is 600-1000 r / min, the solvent is one or more of N,N-dimethylformamide, dichloromethane, chloroform, and acetone, and the compatibilizer in step 4) includes one or more of epoxidized soybean oil, stearic acid monoglyceride, maleic anhydride, and citric acid ester.
[0039] Example 1
[0040] A method for preparing a medical biodegradable dressing comprises the following steps:
[0041] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, extracting it with anhydrous ethanol at 60° C. for 3 h to obtain an extract and a residue, and performing reduced pressure rotary evaporation on the extract at 60° C. to remove the solvent, thereby obtaining an extract of effective components of traditional Chinese medicine;
[0042] The above-mentioned traditional Chinese medicine is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1;
[0043] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the addition amount of 1.5% cellulase solution and 0.6% pectinase solution are both 4 times the mass of the drug residue, soaking at 42°C for 2h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 5h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding, crushing into Chinese medicine fiber with a particle size of 50μ0, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, to obtain modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:5;
[0044] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0045] 4) Preparation of medical biodegradable dressing: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and epoxy soybean oil were mixed in a mass ratio of 50:30:5:10:5, and then granulated, blown film, and rolled to obtain an outer layer blown film, wherein the granulation temperature was 190°C, the film blowing temperature was 185°C, and the surface density of the outer layer blown film was 60g / m 2; (b) Preparation of inner electrospinning membrane: Put polylactic acid and soybean lecithin into an electrospinning machine, add solvent dichloromethane, heat and stir to dissolve, the heating temperature is 50°C, stirring for 3 hours, and the stirring speed is 1000r / min, then drip the extract of Chinese medicinal efficacy ingredients, the mass ratio of polylactic acid, soybean lecithin, and Chinese medicinal efficacy ingredients extract is 100:15:10, and stir while dripping to obtain an electrospinning solution. The electrospinning conditions are as follows: voltage 20kv, spinning flow rate 1.0mL / h, spinning distance 20cm, spinning solution concentration 20%, spinning membrane 50°C, heat treatment 6h, spinning diameter 100nm, electrospinning is performed on the outer layer blown film, combined with pressure-sensitive adhesive and release paper, etc., to obtain a double-layer medical biodegradable dressing, the surface density of the dressing is 100g / m 2 .
[0046] Example 2
[0047] A method for preparing a medical biodegradable dressing comprises the following steps:
[0048] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, hot-extracting with anhydrous ethanol at 60° C. for 1.5 h to obtain an extract and a drug residue, and performing reduced-pressure rotary evaporation on the extract at a temperature of 60° C. to remove the solvent to obtain an extract of effective components of traditional Chinese medicine, wherein the traditional Chinese medicine is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1;
[0049] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 42°C for 2h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 4h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding, crushing into Chinese medicine fiber with a particle size of 80μm, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, and obtaining modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:3;
[0050] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0051] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate terephthalate, modified starch, modified Chinese medicine fiber, and stearic acid monoglyceride were mixed in a mass ratio of 35:40:10:5:5, and then granulated, blown film, and rolled to obtain an outer layer blown film, wherein the granulation temperature was 170°C, the film blowing temperature was 165°C, and the surface density of the outer layer blown film was 50 g / m 2 (b) Preparation of inner electrospinning membrane: Put polylactic acid and soybean lecithin into an electrospinning machine, add solvent N,N-dimethylformamide, heat and stir to dissolve, the heating temperature is 40°C, stirring for 2h, and the stirring speed is 800r / min, then drip the extract of Chinese herbal effective ingredients, the mass ratio of polylactic acid, soybean lecithin, and Chinese herbal effective ingredients extract is 100:10:3, and stir while dripping to obtain an electrospinning solution. The electrospinning conditions are as follows: voltage 10kv, spinning flow rate 0.4mL / h, spinning distance 15cm, spinning solution concentration 8%, spinning membrane 45°C, heat treatment 4h, spinning diameter 120nm, electrospinning is performed on the outer layer blown film, combined with pressure-sensitive adhesive and release paper, etc., to obtain a double-layer medical biodegradable dressing, the surface density of the dressing is 100g / m 2 .
[0052] Example 3
[0053] A method for preparing a medical biodegradable dressing comprises the following steps:
[0054] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, extracting it with anhydrous ethanol at 60° C. for 2 h, obtaining an extract and a medicine residue, and subjecting the extract to reduced pressure rotary evaporation at 60° C. to remove the solvent, thereby obtaining an extract of effective components of traditional Chinese medicine;
[0055] The above-mentioned traditional Chinese medicine is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1;
[0056] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 35°C for 3h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 2h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding, crushing into Chinese medicine fiber with a particle size of 50μm, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, to obtain modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:1;
[0057] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0058] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate terephthalate, modified starch, modified Chinese medicine fiber, and maleic anhydride were mixed in a mass ratio of 35:35:8:6:1, and then granulated, blown film, and rolled to obtain an outer layer blown film, wherein the granulation temperature was 180°C, the film blowing temperature was 175°C, and the surface density of the outer layer blown film was 30 g / m 2 ; (b) Preparation of inner electrospinning membrane: Put polylactic acid and soybean lecithin into an electrospinning machine, add solvent N,N-dimethylformamide, heat and stir to dissolve, the heating temperature is 40°C, stirring for 4 hours, and the stirring speed is 1000r / min, then drip the extract of Chinese medicine efficacy ingredients, the mass ratio of polylactic acid, soybean lecithin, and Chinese medicine efficacy ingredient extract is 100:5:3, and stir while dripping to obtain an electrospinning solution. The electrospinning conditions are as follows: voltage 15kv, spinning flow rate 0.8mL / h, spinning distance 17cm, spinning solution concentration 13%, spinning membrane 40°C, heat treatment 5h, spinning diameter 150nm, electrospinning is performed on the outer layer blown film, combined with pressure-sensitive adhesive and release paper, etc., to obtain a double-layer medical biodegradable dressing, the surface density of the dressing is 50g / m 2 .
[0059] Example 4
[0060] A method for preparing a medical biodegradable dressing comprises the following steps:
[0061] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, extracting it with anhydrous ethanol at 60° C. for 2.5 h to obtain an extract and a residue, and performing reduced pressure rotary evaporation on the extract at 60° C. to remove the solvent, thereby obtaining an extract of effective components of traditional Chinese medicine;
[0062] The above-mentioned traditional Chinese medicine is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1;
[0063] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the addition amount of 1.5% cellulase solution and 0.6% pectinase solution are both 4 times the mass of the drug residue, soaking at 35°C for 2.5h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 3h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding, crushing into Chinese medicine fiber with a particle size of 60μm, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, to obtain modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:4;
[0064] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0065] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and citrate were mixed in a mass ratio of 45:35:8:5:5, and then granulated, blown film, and rolled to obtain an outer layer blown film, wherein the granulation temperature was 190°C, the film blowing temperature was 180°C, and the surface density of the outer layer blown film was 40 g / m 2 ; (b) Preparation of inner electrospinning membrane: Put polylactic acid and soybean lecithin into an electrospinning machine, add solvent acetone, heat and stir to dissolve, the heating temperature is 50°C, stirring for 3 hours, and the stirring speed is 800r / min, then drip the extract of Chinese herbal effective ingredients, the mass ratio of polylactic acid, soybean lecithin, and Chinese herbal effective ingredients extract is 100:12:6, and stir while dripping to obtain an electrospinning solution. The electrospinning conditions are as follows: voltage 18kv, spinning flow rate 0.8mL / h, spinning distance 12cm, spinning solution concentration 16%, spinning membrane 50°C, heat treatment 5.5h, spinning diameter 80nm, electrospinning is performed on the outer layer blown film, combined with pressure-sensitive adhesive and release paper, etc., to obtain a double-layer medical biodegradable patch, the surface density of the patch is 70g / m 2 .
[0066] Example 5
[0067] A method for preparing a medical biodegradable dressing comprises the following steps:
[0068] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, extracting it with anhydrous ethanol at 60° C. for 3 h to obtain an extract and a residue, and performing reduced pressure rotary evaporation on the extract at 60° C. to remove the solvent, thereby obtaining an extract of effective components of traditional Chinese medicine;
[0069] The above-mentioned traditional Chinese medicine is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1;
[0070] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 40°C for 3h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 2h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding, crushing into Chinese medicine fiber with a particle size of 70μm, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, and obtaining modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:3;
[0071] 3) Preparation of modified starch: corn starch and glycerol are placed in a high-speed mixer and heated at 90°C for 18 minutes to obtain modified starch, wherein the mass ratio of corn starch to glycerol is 100:30; cassava starch and potato starch can also be used instead of corn, but their film-forming properties and mechanical properties are not as good as corn starch;
[0072] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and epoxy soybean oil were mixed in a mass ratio of 40:30:10:6:5, and then granulated, blown film, and rolled to obtain an outer layer blown film, wherein the granulation temperature was 170°C, the film blowing temperature was 175°C, and the surface density of the outer layer blown film was 40 g / m 2 ; (b) Preparation of inner electrospinning membrane: Put polylactic acid and soybean lecithin into an electrospinning machine, add chloroform solvent, heat and stir to dissolve, the heating temperature is 45°C, stirring for 2h, and the stirring speed is 600r / min, then drip the extract of Chinese herbal efficacy ingredients, the mass ratio of polylactic acid, soybean lecithin, and Chinese herbal efficacy ingredients extract is 100:9:4, and stir while dripping to obtain an electrospinning solution. The electrospinning conditions are as follows: voltage 12kv, spinning flow rate 0.5mL / h, spinning distance 15cm, spinning solution concentration 8%, spinning membrane 50°C, heat treatment 4h, spinning diameter 100nm, electrospinning is performed on the outer layer blown film, combined with pressure-sensitive adhesive and release paper, etc., to obtain a double-layer medical biodegradable dressing, the surface density of the dressing is 80g / m 2 .
[0073] Comparative Example 1
[0074] A method for preparing a medical biodegradable dressing comprises the following steps:
[0075] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, extracting it with anhydrous ethanol at 60°C for 3h to obtain an extract and a medicine residue, and performing reduced pressure rotary evaporation on the extract at 60°C to remove the solvent to obtain an extract of effective components of traditional Chinese medicine, wherein the traditional Chinese medicine is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1;
[0076] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 42°C for 3h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 5h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding, crushing into Chinese medicine fiber with a particle size of 50μm, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, to obtain modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:5;
[0077] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0078] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate terephthalate, modified starch, modified Chinese medicine fiber, and epoxy soybean oil were mixed in a mass ratio of 50:30:5:10:5, and then granulated, blown film, and rolled to obtain an outer layer blown film, wherein the granulation temperature was 190°C, the film blowing temperature was 185°C, and the surface density of the outer layer blown film was 60g / m 2 ; (b) preparing the inner electrospinning membrane: putting polylactic acid into an electrospinning machine, adding solvent dichloromethane, heating and stirring to dissolve, and then dripping the extract of the Chinese medicine efficacy component, the mass ratio of polylactic acid to the extract of the Chinese medicine efficacy component is 100:10, stirring while dripping to obtain an electrospinning solution, the electrospinning conditions are as follows: voltage 20kv, spinning flow rate 1.0mL / h, spinning distance 20cm, spinning solution concentration 20%, spinning membrane 50℃, heat treatment 6h, spinning diameter 100nm, electrospinning is carried out on the outer layer blown film, combined with pressure-sensitive adhesive and release paper, etc., to obtain a double-layer medical biodegradable dressing, the surface density of the dressing is 100g / m 2 .
[0079] Compared with Example 1, in Comparative Example 1, soybean lecithin is no longer added when preparing the inner electrospinning membrane, and other technical features remain unchanged. The role of soybean lecithin can be clearly found through subsequent comparison.
[0080] Comparative Example 2
[0081] A method for preparing a medical biodegradable dressing comprises the following steps:
[0082] 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, hot-extracting with anhydrous ethanol at 60° C. for 1.5 h to obtain an extract and a drug residue, and performing reduced-pressure rotary evaporation on the extract at a temperature of 60° C. to remove the solvent to obtain an extract of effective components of traditional Chinese medicine, wherein the traditional Chinese medicine is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:1;
[0083] 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 42°C for 2h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 4h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding, crushing into Chinese medicine fiber with a particle size of 80μm, finally mixing the Chinese medicine fiber with a silane coupling agent, heating at 100°C in a high-speed mixer for 20min, and obtaining modified Chinese medicine fiber, the mass ratio of Chinese medicine fiber to silane coupling agent is 100:3;
[0084] 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30;
[0085] 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film particles: polylactic acid, polybutylene adipate terephthalate, modified starch, modified Chinese medicine fiber, and epoxidized soybean oil were mixed in a mass ratio of 35:40:10:5:5, and then granulated at a granulation temperature of 170°C to obtain outer layer blown film particles; (b) The composition of the inner layer blown film: polylactic acid: soybean lecithin: Chinese medicine active ingredient extract is 100:10:3, and the film is blown and rolled in a double-layer co-extrusion manner at a blowing temperature of 165°C. Combined with pressure-sensitive adhesive and release paper, a double-layer medical biodegradable patch is obtained, and the surface density of the patch is 100g / m 2 .
[0086] Compared with Example 2, the inner layer blown film and the inner layer electrospun film of this comparative example 2 are different, and other technical features are the same as those of Example 2. The advantages of using electrospun film for the inner layer can be seen through comparison.
[0087] Effect verification test:
[0088] 1. Water vapor permeability
[0089] According to the YY / T 0148 standard, a plate containing 1kg of anhydrous calcium chloride was placed in an electric drying oven at a temperature of 36-38°C. Five boxes of 95mm×25mm×20mm were taken, each containing about 2g of absorbent cotton, and about 20ml of water was poured into each box, and the top of the opening was completely sealed with the test material strip. The sealed boxes were weighed to the milligram, and they were placed in the cabinet for about 18 hours (the time was recorded to the accuracy of 15 minutes).
[0090] Take the box out of the cabinet, cool it under standard atmospheric pressure for 1 hour, and weigh it again to the nearest milligram.
[0091] The water vapor permeability per 24 hours was calculated using the top opening area and mass loss of each box in grams per square meter (g·m -2 )express.
[0092] The results are shown in Table 1 below.
[0093] Table 1 Comparison of water vapor permeability test results
[0094] Group <![CDATA[Air permeability / g·m -2 ·24h]]> Example 1 990 Example 2 1002 Example 3 963 Example 4 900 Example 5 935 Comparative Example 1 908 Comparative Example 2 819 Commercially available PU patch 712
[0095] As can be seen from Table 1, the medical biodegradable dressing prepared in Examples 1 to 5 and Comparative Examples 1 to 2 of the present invention and the commercially available PU dressing have significantly higher water vapor permeability than the commercially available PP dressing, and Example 2 has a permeability about 22% higher than that of Comparative Example 2, and about 40% higher than that of the commercially available PP dressing, indicating that both Examples 1 to 5 and Comparative Examples 1 to 2 can better maintain the permeability. The inner layer film of Comparative Example 2 is prepared by the film blowing process, and has a lower permeability than Examples 1 to 5 and Comparative Example 1. It can be seen that the inner layer electrospinning film can well maintain the permeability of the dressing, and long-term application is not easy to cause sweating.
[0096] 2. Mechanical properties and degradation experiments
[0097] The tensile strength was measured according to GB / T 1040.3; the extensibility, peel strength and holding power were measured according to YY / T 0148 standard. The results are shown in Table 2.
[0098] Table 2 Comparison of mechanical properties and relative biodegradation rates
[0099]
[0100] As shown in Table 2, the tensile strength of the medical biodegradable dressing prepared in Examples 1 to 5 and Comparative Examples 1 to 2 of the present invention is higher than that of the commercially available PU dressing, and the tensile strength of Comparative Example 2 is similar to that of the commercially available PU dressing. Comparative Example 2 has a higher extensibility and is prone to deformation, resulting in enhanced longitudinal stretching; Comparative Example 2 has a lower stickiness and is prone to falling off after long-term use, indicating that the blown film reduces the performance of the dressing. The commercially available PU dressing has a lower peel strength and may easily fall off after a long time.
[0101] It can also be seen that the inner layer electrospun membrane of Examples 1 to 5 has better performance than the inner layer blown film, has greater tensile strength, moderate extensibility, is not easy to deform, has greater stickiness, is not easy to fall off, and the relative biodegradation rate is almost 100% degraded in 4 months, which is greater than 90%, that is, it is considered to be fully biodegradable.
[0102] 3. Antibacterial effect
[0103] Using Staphylococcus aureus and Escherichia coli as test bacteria, the antibacterial effects of a medical biodegradable dressing prepared in Examples 1 to 5 and Comparative Examples 1 to 2 and a commercially available PU dressing on the test bacteria were tested.
[0104] 1 ml of a concentration of 10 6 CFU / ml of Staphylococcus aureus and Escherichia coli were evenly coated on the agar medium with a sterile glass rod. When the bacterial solution was completely spread, a film with a diameter of 0.5 cm was cut with a sterilized puncher and placed in the center of the medium. The culture dish was inverted and cultured at 37℃ for 24 hours, and the diameter of the inhibition zone was measured. The test was repeated 3 times.
[0105] The results are shown in Table 3.
[0106] Table 3 Antibacterial effect test
[0107]
[0108] From the diameter of the antibacterial zone in Table 3, it can be seen that the diameter of the antibacterial zone in Examples 1 to 5 and Comparative Example 1 is significantly larger than that in Comparative Example 2, indicating that the antibacterial effect is significantly reduced after the electrospinning process is changed to the blow molding process. After the inner layer film of Comparative Example 2 is blow molded at high temperature, the effective ingredients are destroyed by high temperature, resulting in a low antibacterial effect. Examples 1 to 5 have a higher antibacterial effect than Comparative Example 1, indicating that not adding soybean lecithin affects the drug loading of the dressing, thereby affecting the antibacterial effect. The antibacterial effect of the commercially available PU dressing is almost 0, indicating that a medical biodegradable dressing prepared in Examples 1 to 5 has a good antibacterial effect.
[0109] 4. In vitro release performance test
[0110] Weigh samples, each of which is about 10 mg of theoretical Chinese medicine extract, and place them in 10 ml of phosphate buffer solution (PBS, pH = 7.4), and shake at 37 ° C for 2h, 4h, 6h, 8h, 12h, 16h, 20h, 24h, 30h, 36h. Use an ultraviolet spectrophotometer to test the drug release of Examples 1 to 5 and Comparative Examples 1 to 2. The results are shown in the drug cumulative release rate curve attached to the specification. Figure 1 .
[0111] from Figure 1 It can be seen that the in vitro cumulative release rates of Examples 1 to 5 are similar, and are close to 100% in 36h, with sustained release of the drug effect. The cumulative release rate of Comparative Example 1 is faster than that of Example 1, which may be caused by the fact that no soybean lecithin is added to Comparative Example 1. The cumulative release rate of Comparative Example 2 is faster than that of Example 2, and the cumulative release rate tends to be stable when it reaches about 62%, which should be close to 100% in theory, but it may be because the inner layer electrospinning membrane of Comparative Example 2 is a blown film, and the high temperature causes the activity of the effective ingredients of traditional Chinese medicine to decrease, which is inconsistent with the theoretical value, and the release rate is faster.
[0112] The above-described embodiments are merely descriptions of preferred implementations of the present invention and are not intended to limit the scope of the present invention. Various modifications and alterations to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the scope of protection defined by the claims of the present invention.
Claims
1. A method for preparing a medical biodegradable dressing, Features: The following steps are involved: 1) Preparing extracts of effective components of traditional Chinese medicine: crushing the traditional Chinese medicine, hot-extracting with anhydrous ethanol at 60° C. for 1.5 to 3 h to obtain an extract and a residue, and performing reduced pressure rotary evaporation on the extract at 60° C. to remove the solvent to obtain an extract of effective components of traditional Chinese medicine; 2) Preparing modified Chinese medicine fiber: drying the drug residue in step 1) at 60°C, crushing, passing through 80 mesh, adding 1.5% cellulase solution and 0.6% pectinase solution respectively, the amount of 1.5% cellulase solution and 0.6% pectinase solution added is 4 times the weight of the drug residue, soaking at 35-42°C for 2-3h, filtering, washing with water until neutral, drying at 60°C, adding 5% sodium hydroxide solution, soaking for 2-5h, filtering, washing with water until neutral, drying again at 60°C, and then ultrafine grinding to crush into Chinese medicine fiber with a particle size of 50-80μm, finally mixing the Chinese medicine fiber with a silane coupling agent, and heat treating at 100°C in a high-speed mixer for 20min to obtain the modified Chinese medicine fiber; 3) Preparation of modified starch: corn starch and glycerol were placed in a high-speed mixer and heat-treated at 90° C. for 18 min to obtain modified starch, wherein the mass ratio of corn starch to glycerol was 100:30; 4) Preparation of medical biodegradable patch: (a) Preparation of outer layer blown film: polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and compatibilizer are mixed in a mass ratio of (35-50): (30-40): (5-10): (5-10): (1-5), and then granulated, blown film, and rolled to obtain an outer layer blown film; (b) Preparation of inner layer electrospun film: polylactic acid and soybean lecithin are placed in an electrostatic spinning film. In the electrospinning machine, a solvent is added, heated and stirred to dissolve, and then the extract of the Chinese medicine functional component is dripped in, the mass ratio of polylactic acid, soybean lecithin, and the extract of the Chinese medicine functional component is 100: (5-15): (3-10), and the solution is stirred while dripping to obtain an electrospinning solution, and electrospinning is performed on the outer layer blown film, combined with a pressure-sensitive adhesive and a release paper to obtain a double-layer medical biodegradable patch, the surface density of which is 50-100 g / m 2 .
2. A method for preparing a medical biodegradable dressing as claimed in claim 1, Features: The traditional Chinese medicine in step 1) is a combination of honeysuckle, trichosanthes and isatis root, and the mass ratio of honeysuckle, trichosanthes and isatis root is 2:1:
1.
3. A method for preparing a medical biodegradable dressing as claimed in claim 1, Features: The mass ratio of the traditional Chinese medicine fiber to the silane coupling agent in the step 2) is 100:(1-5).
4. A method for preparing a medical biodegradable dressing as claimed in claim 1, Features: In the step 4), the granulation temperature for preparing the outer layer blown film is 170-190°C, and the film blowing temperature is 165-185°C.
5. A method for preparing a medical biodegradable dressing as claimed in claim 1, Features: The solvent in step 4) is one or more of N,N-dimethylformamide, dichloromethane, chloroform and acetone.
6. A method for preparing a medical biodegradable dressing as claimed in claim 1, Features: In the step 4), the heating temperature after adding the solvent to prepare the inner electrospinning membrane is 40-50° C., stirring is 2-4 hours, and the stirring speed is 600-1000 r / min.
7. A method for preparing a medical biodegradable dressing as claimed in claim 1, Features: The electrospinning conditions in step 4) are as follows: voltage 10-20 kV, spinning flow rate 0.4-1.0 mL / h, spinning distance 12-20 cm, spinning solution concentration 8-20%, spinning membrane 40-50° C., heat treatment 4-6 h, spinning diameter 80-150 nm.
8. A method for preparing a medical biodegradable dressing as claimed in claim 1, Features: The compatibilizer in step 4) includes one or more of epoxidized soybean oil, stearic acid monoglyceride, maleic anhydride, and citric acid ester.
9. A medical biodegradable patch prepared by the method for preparing a medical biodegradable patch according to any one of claims 1 to 8, Features: It comprises an outer layer blown film and an inner layer electrostatic spinning film, wherein the components of the outer layer blown film include polylactic acid, polybutylene adipate-terephthalate, modified starch, modified Chinese medicine fiber, and a compatibilizer; the components of the inner layer electrostatic spinning film include polylactic acid, soybean lecithin, and extracts of Chinese medicine functional ingredients.