A composite negative electrode material and preparation method thereof, negative electrode sheet and battery

By adopting a composite negative electrode material with a double-layer clad structure in lithium-ion batteries, the core of silicon nanoparticles and titanium monoxide particles and the cladding of silicon oxide and porous carbon fibers, the volume expansion and conductivity of silicon anode material are solved. The high energy density and good cycle stability and rate performance are achieved.

CN116779769BActive Publication Date: 2024-11-15BYD CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210235984.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-10
Publication Date
2024-11-15
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

The large volume expansion effect and low conductivity of silicon negative electrode materials in lithium-ion batteries lead to poor circulation and rate performance, which cannot meet the needs of high energy density.

Method used

Using composite negative electrode material, the core includes silicon nanoparticles and titanium monoxide particles, the cladding layer includes silicon oxide and porous carbon fibers, is prepared by electrospinning and plasma sintering processes to form a double-layer cladding structure to alleviate volume expansion and improve Conductivity.

Benefits of technology

It achieves low volume expansion effect, excellent cycle stability and high rate performance, and improves the energy density and kinetic performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116779769B_ABST
    Figure CN116779769B_ABST
Patent Text Reader

Abstract

The present application provides a composite negative electrode material including a core, a first coating layer coated on the surface of the core, and a second coating layer coated on the surface of the first coating layer, wherein the core includes silicon nanoparticles and titanium monoxide particles, the first coating layer includes silicon monoxide, and the second coating layer includes carbon fibers with a porous structure. The composite negative electrode material has a small volume expansion effect and good electrical conductivity, and can enable the battery to have good cycle performance, rate performance and high discharge capacity. The present application also provides a preparation method of the composite negative electrode material, a negative electrode sheet and a battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a composite negative electrode material and a preparation method thereof, a negative electrode sheet and a battery. Background Art

[0002] Lithium secondary batteries have been widely used in portable electronic products such as mobile phones and laptops, as well as new energy vehicles. The energy density of lithium-ion batteries based on traditional graphite negative electrodes has approached the ceiling and can no longer meet people's growing demand for standby and endurance. Silicon negative electrode materials with higher theoretical specific capacity are considered to be an effective way to break through the high energy density of lithium secondary batteries. However, silicon negative electrode materials have a large volume effect (volume expansion rate greater than 300%) during the process of lithium insertion and extraction. After multiple cycles, they will become powdered and fall off, which will cause the battery's cycle performance to drop sharply. In addition, silicon is a semiconductor material with low electrical conductivity, which will also lead to poor rate performance of the battery. Therefore, it is necessary to provide a technical solution that can effectively solve the volume expansion problem and conductivity problem of silicon at the same time. Summary of the invention

[0003] In view of this, the present application aims to provide a composite negative electrode material for lithium-ion batteries with a new structure, which has extremely low volume expansion effect and good conductivity, and can make the battery have better cycle performance and rate performance.

[0004] Specifically, the first aspect of the present application provides a composite negative electrode material, which includes a core, a first coating layer coated on the surface of the core, and a second coating layer coated on the surface of the first coating layer, wherein the core includes silicon nanoparticles and titanium monoxide particles; the first coating layer includes silicon monoxide; and the second coating layer includes carbon fibers with a porous structure.

[0005] In the composite negative electrode material provided in the first aspect of the present application, the inner core contains both silicon nanoparticles and titanium monoxide particles. The electrical conductivity of titanium monoxide is close to that of graphite, and its electrical conductivity is good, which can improve the electrical contact between adjacent silicon nanoparticles. The surface of the silicon-containing inner core has two coating layers, and their synergistic effect can effectively alleviate the volume expansion of the inner core silicon. In addition, the porous carbon fibers in the outermost coating layer have good electrical conductivity, which can further improve the electrical conductivity of the silicon nanoparticles and improve the rate performance of the overall composite negative electrode material. The porous structure can provide channels for lithium ion embedding / ejection and increase the contact area between the material and the electrolyte, which is beneficial to the actual utilization of the capacity of the inner core silicon material with high theoretical capacity.

[0006] In a second aspect, the present application provides a method for preparing a composite negative electrode material, comprising the following steps:

[0007] (1) dispersing silicon nanoparticles in an alcohol-containing solvent, adding titanate and dispersing them uniformly, and then adding silicate and a spinnable carbon source and dispersing them uniformly to obtain a mixed solution; electrospinning the mixed solution to obtain a composite fiber membrane;

[0008] (2) The composite fiber membrane is first pre-fired at 200-500°C in an air atmosphere, and then the pre-fired composite fiber membrane is sintered in a plasma device under an inert atmosphere to obtain the composite negative electrode material; wherein the power of the plasma device is 50-200W, and the sintering temperature is 800-1200°C.

[0009] The preparation method is simple in process and convenient in operation, and can prepare a composite negative electrode material for lithium-ion batteries with a novel structure, and has extremely low volume expansion effect, large capacity and excellent cycle stability, etc., which is convenient for its industrial application.

[0010] In a third aspect, the present application provides a negative electrode sheet containing the above-mentioned composite negative electrode material.

[0011] In a fourth aspect, the present application provides a battery containing a negative electrode plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 Schematic diagram of the structure of the composite negative electrode material in the embodiment of the present application.

[0013] Figure 2 This is a cross-sectional scanning electron microscope (SEM) photograph of the negative electrode sheet of the soft-pack full battery in Example 1 of the present application.

[0014] Figure 3 The cycle curves of button batteries of Example 1 and some comparative examples are shown.

[0015] Figure 4 It is a cycle curve diagram of the soft-pack full battery of Example 1 and some comparative examples. DETAILED DESCRIPTION

[0016] Described below are exemplary implementations of the embodiments of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the embodiments of the present application. These improvements and modifications are also considered to be within the scope of protection of the embodiments of the present application.

[0017] See also Figure 1 , Figure 1A schematic diagram of the structure of a composite negative electrode material provided in an embodiment of the present application. The composite negative electrode material 100 includes a core 10, a first coating layer 20 coated on the surface of the core 10, and a second coating layer 30 coated on the surface of the first coating layer 20, wherein the core 10 includes silicon nanoparticles 101 and titanium monoxide particles 102, the first coating layer 20 includes silicon monoxide, and the second coating layer 30 includes carbon fibers having a porous structure.

[0018] In the present application, the core 10 contains both nano-silicon material and titanium monoxide. The electrical conductivity of titanium monoxide is close to that of graphite, and it has good electrical conductivity, which can improve the electrical contact between adjacent nano-silicon materials, thereby improving the cycle and rate performance. In addition, titanium monoxide is a zero-strain material, and its thermal expansion during the lithium insertion / extraction process is very low, and its presence can also inhibit the volume expansion of silicon.

[0019] The surface of the silicon-containing core 10 has two coating layers, among which the first coating layer 20 formed by silicon monoxide has good stability. Specifically, the internal structure of silicon monoxide changes little during long-term use, and the volume expansion effect is small during the process of inserting and removing lithium ions, which is much lower than that of single silicon materials. Therefore, the first coating layer 20 can also inhibit the expansion of the core nano silicon material. The second coating layer 30 formed by porous carbon fiber has a certain limiting effect, which can work together with the above-mentioned first coating layer 20 to alleviate the volume expansion of the core silicon, and the presence of the porous structure on the carbon fiber can also provide a release channel for the volume expansion of silicon, further alleviating the volume effect of silicon. More importantly, the good electrical conductivity of carbon fiber can further improve the conductivity of nano silicon materials, give the overall composite negative electrode material good electrical conductivity, and improve the rate performance; the porous structure also increases the contact area between the material and the electrolyte, and provides channels for lithium ion insertion / extraction, improves the kinetic performance of the material, and is conducive to the capacity of the core silicon material with high theoretical capacity to be effectively exerted.

[0020] Therefore, the composite negative electrode material 100 provided in the embodiment of the present application has a small volume expansion effect during the lithium extraction / insertion process and good cycle stability; it has good conductivity and rate performance, and the high specific capacity characteristics of the core silicon material can be fully utilized, so that the discharge capacity of the composite negative electrode material is relatively high, which is beneficial to improve the battery energy density.

[0021] Optionally, the diameter distribution range of the silicon nanoparticles is 80-150 nm. In some embodiments of the present application, the mass proportion of the silicon nanoparticles in the composite negative electrode material 100 can be 60%-82%. The silicon nanoparticles in the above range can ensure that the specific capacity of the composite negative electrode material 100 is not too low.

[0022] In some embodiments of the present application, the average diameter of the titanium monoxide particles is 40-60 nm. At this time, the conductivity of titanium monoxide is very high, close to that of graphite, which can significantly improve the conductivity of the negative electrode material and improve the rate performance.

[0023] In some embodiments of the present application, the mass proportion of the titanium monoxide particles in the composite negative electrode material 100 can be 2.5%-20%. By setting the above content of titanium monoxide particles, it is more conducive to improving the conductivity of the composite negative electrode material 100, especially to establish electrical connection between silicon nanoparticles through titanium monoxide in the core 10, and the proportion of silicon nanoparticles with high specific capacity will not be too low. Exemplarily, the mass proportion is, for example, 2.5%-10%, or 3%-8%, etc. Optionally, titanium monoxide particles are distributed on the surface / surroundings of the silicon nanoparticles.

[0024] In some embodiments of the present application, the thickness of the first coating layer 20 (i.e., silicon dioxide layer) can be in the range of 3-25 nm. Controlling the thickness of the first coating layer 20 in this range can better slow down the volume expansion of the core silicon material, and does not affect the insertion / extraction of lithium ions in the core silicon, giving full play to the high specific capacity of the silicon material.

[0025] In the embodiments of the present application, the chemical formula of the silicon oxide is SiOx, 1≤x<2. In some embodiments of the present application, the silicon oxide is amorphous silicon oxide. Among them, the mass of silicon oxide accounts for 1-10% of the mass of the composite negative electrode material 100. This mass ratio can ensure that the thickness of the first coating layer 20 is appropriate, and the volume expansion of the core silicon material will not be effectively reduced due to the low mass of the first coating layer 20, and the first coating layer 20 will not be too thick, which is not conducive to the shuttle of electrons / ions between the core 10 and the second coating layer 30.

[0026] In some embodiments of the present application, the thickness of the second coating layer 30 formed by the porous carbon fiber is 40-130 nm. The second coating layer 30 of suitable thickness can not only further inhibit the volume expansion of the silicon material in the core 10, but also ensure the good conductivity of the overall composite negative electrode material 100 and ensure good electrical contact between two adjacent composite negative electrode material particles.

[0027] Optionally, the mass of the carbon fiber accounts for 10-20% of the mass of the composite negative electrode material 100. This mass ratio can ensure that the coating thickness of the second coating layer 30 is appropriate while not reducing the specific capacity of the composite negative electrode material 100 too much.

[0028] Furthermore, the thickness ratio of the second coating layer 30 to the first coating layer 20 is (2-40): 1. Through the above configuration, the volume expansion of the nano silicon particles can be better suppressed under the synergistic effect of the two, and the rate performance and fast charging performance of the composite negative electrode material 100 can be improved.

[0029] In some embodiments of the present application, the diameter distribution range of the carbon fibers is 0.1-1 μm.

[0030] In the embodiment of the present application, the pore size distribution range of the porous structure on the carbon fiber is 5-30nm; the porosity of the second coating layer is 60%-96%, for example, 60%, 70%, 80%, 90%, etc.

[0031] The present application also provides a method for preparing the composite negative electrode material, comprising the following steps:

[0032] (1) dispersing silicon nanoparticles in an alcohol-containing solvent, adding titanate and dispersing them uniformly, and then adding silicate and a spinnable carbon source and dispersing them uniformly to obtain a mixed solution; electrospinning the mixed solution to obtain a composite fiber membrane;

[0033] (2) The composite fiber membrane is first pre-fired at 200-500°C in an air atmosphere, and then the pre-fired composite fiber membrane is sintered in a plasma device under an inert atmosphere to obtain the composite negative electrode material; wherein the power of the plasma device is 50-200W, and the sintering temperature is 800-1200°C.

[0034] In the above preparation method, when preparing the mixed solution for electrospinning, titanate and silicate will be hydrolyzed in an alcohol-containing solvent and converted into TiO2 and SiO2 respectively. In step (1), when preparing the mixed solution, silicon nanoparticles are first dispersed in an alcohol-containing solvent to obtain a dispersion of silicon nanoparticles, and then titanate is added, and then silicate and a spinnable carbon source are added. Such a raw material addition sequence can ensure that the silicon nanoparticles and titanium oxide obtained by hydrolysis of titanate will be coated by the silicon oxide obtained by hydrolysis of silicate, and after subsequent treatment, a composite negative electrode material with the above structure can be better obtained. Among them, the composite fiber membrane obtained by electrospinning includes a spinning membrane matrix formed by fibers of the carbon source, and silicon nanoparticles, SiO2, and TiO2 coated therein. The composite fiber membrane is pre-sintered in an air atmosphere, which helps the carbon fiber to be initially formed at a low temperature and prepare a carbon fiber material with uniform morphology. The pre-sintered composite fiber membrane has more stable properties and helps to improve the electrochemical performance of the prepared composite negative electrode material. If high-temperature calcination is directly used, the carbon fiber is easy to burn off, and the generated carbon fiber is easy to agglomerate. After that, the pre-sintered composite fiber membrane is sintered in a plasma device. In addition to carbonizing it and converting the organic carbon material fibers therein into conductive carbon fibers, it can also make pores in the carbon fibers to form a porous structure on the surface of the carbon fibers, and convert TiO2 into TiO and SiO2 into silicon oxide. Among them, the selection of plasma equipment for high-temperature sintering can form a uniform porous structure on the carbon fibers.

[0035] Wherein, the silicate includes one or more of methyl orthosilicate, ethyl orthosilicate, orthopropyl orthosilicate, isopropyl orthosilicate, orthobutyl orthosilicate, amyl orthosilicate, etc. The titanate includes one or more of tetrabutyl titanate, isopropyl titanate, tetraisopropyl titanate, tetraethyl titanate, isopropyl tris(dioctyl pyrophosphate acyloxy) titanate, etc. The spinnable carbon source includes one or more of polyacrylonitrile, polyacrylic acid, polymethyl methacrylate, polytetrafluoroethylene, polyvinyl pyrrolidone, polyvinyl alcohol, etc., but is not limited thereto. The alcohol-containing solvent may be an alcohol solvent, or a mixture of an alcohol solvent and other solvents (such as water, an organic solvent). Wherein, the alcohol solvent may be one or more of methanol, ethanol, ethylene glycol, n-propanol, polyethylene glycol, etc.

[0036] In some embodiments of the present application, in step (1), the preparation method of the mixed solution includes: first dispersing silicon nanoparticles in an alcohol-containing solvent, then adding titanate and dispersing uniformly, then adding silicate and dispersing uniformly, and finally adding a spinnable carbon source and dispersing uniformly to obtain a mixed solution for electrospinning. This is more conducive to obtaining more composite negative electrode materials with the above structure.

[0037] In some embodiments of the present application, the mass ratio of the silicon nanoparticles to the volume ratio of the silicate is (0.5-3): (1-5) g / mL. The mass ratio of the silicon nanoparticles to the volume ratio of the titanate is (0.5-3): (0.1-1) g / mL. The amount ratio of the silicon nanoparticles to the spinnable carbon source is (0.5-3): (1-10).

[0038] In some embodiments of the present application, the electrospinning parameters include: a spinning voltage of 10-30 kV, a feeding speed of the mixed solution of 30-110 μL / min, and a receiving device of the electrospinning device of 200-800 rpm. The receiving device may be a receiving roller with a controllable speed, which can carry the composite fiber membrane obtained by spinning the mixed solution.

[0039] In the embodiment of the present application, the pre-burning temperature is 200-500° C., specifically 250, 300, 320, 350, 400, 450° C., etc. In some embodiments, the pre-burning temperature is 320-500° C. The pre-burning time can be 1-3 hours, such as 1.5 hours, 2 hours, etc.

[0040] In the present application, plasma equipment is selected for high temperature sintering, so that the organic carbon material fiber can be transformed into a conductive carbon fiber, and the carbon fiber is pore-formed, and the porous structure of the carbon fiber can be made more uniform. The power of the plasma equipment (specifically the power of the plasma source) can be adjusted to adjust the size and distribution of the porous structure. Plasma is an ionized gas-like substance produced after the atoms are ionized. As the power of the plasma equipment increases, the energy carried by the plasma beam generated by the electric field will become stronger and stronger. The material is affected by these plasmas. On the one hand, because of the huge energy impact, a porous structure will appear on the surface to achieve the purpose of etching. On the other hand, the chemical bonds on the surface are ionized, and redox reactions are more likely to occur.

[0041] In the embodiment of the present application, the sintering temperature in the plasma equipment is 800-1200°C, specifically 850, 900, 1000, 1050, 1100, 1150, 1200°C, etc. In some embodiments, the sintering temperature is 800-1000°C. The sintering time may be 1-3h, such as 1.5h, 2h, etc. The inert atmosphere includes at least one of argon (Ar), helium (He) and nitrogen (N2) atmospheres.

[0042] The method for preparing the composite negative electrode material provided in the embodiment of the present application has a simple process and is convenient to operate. A composite negative electrode material for lithium-ion batteries with a novel and stable structure is prepared, and has excellent properties such as extremely low volume expansion effect, large capacity and cycle performance, which is convenient for its industrial application.

[0043] The embodiment of the present application also provides a negative electrode plate, which contains the composite negative electrode material described above in the embodiment of the present application.

[0044] Specifically, the negative electrode sheet includes a negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector, and the negative electrode active material layer contains the above-mentioned composite negative electrode material. In some embodiments, the negative electrode active material layer also contains a binder to improve the adhesion of the composite negative electrode material to the negative electrode current collector. As described above in the present application, since the outer layer of the composite negative electrode material has a conductive carbon fiber coating layer, the negative electrode active material layer may not need to add a conductive agent. Of course, in some other embodiments, in order to further improve the conductivity of the negative electrode active material layer, a conductive agent may also be contained. At this time, the negative electrode active material layer contains the above-mentioned composite negative electrode material, a binder and a conductive agent. Exemplary conductive agents may be graphite, carbon black, graphene, etc. Among them, in the negative electrode active material layer, the mass content of the composite negative electrode material may be 50-90wt%, the content of the binder may be 1-10wt%, and the content of the conductive agent may be 0.1-10wt. The compaction density of the negative electrode sheet may be 1.1-2g / cm 3 .

[0045] The present application also provides a battery, which includes the negative electrode sheet described above in the present application. In addition to the negative electrode sheet, the battery also includes a positive electrode sheet, and a separator and an electrolyte between the positive electrode sheet and the negative electrode sheet. The structure of the battery can refer to the conventional description in the battery field, and will not be repeated here.

[0046] Since the battery adopts the above-mentioned composite negative electrode material with excellent performance as the negative electrode active material, the battery can take into account high energy density, good cycle performance and rate performance, etc., which is conducive to its wide application.

[0047] The technical solution of the present application is further described below through several specific embodiments.

[0048] Example 1

[0049] A method for preparing a composite negative electrode material comprises the following steps:

[0050] 0.5g of silicon nanoparticles (purchased from Aladdin, with an average diameter of about 120nm and a diameter distribution range of 80-150nm) were dispersed in a mixture of 5mL of ethanol and ethylene glycol (ethanol: ethylene glycol volume ratio of 1:1), stirred at 1000 rpm for 1h, 1mL of isopropyl titanate was added, stirred at 1000 rpm for 2h, then 1mL of butyl orthosilicate and 1g of polyacrylonitrile were added, stirred at 200 rpm for more than 12h, and a silicon-containing electrospinning mixed solution was obtained. The mixed solution was then electrospun according to the following process parameters to obtain a composite fiber membrane: the speed of the receiving device of the electrospinning equipment was 800 rpm, the spinning voltage was 10kV, and the feeding rate of the spinning solution was 30μL / min.

[0051] The above-mentioned composite fiber membrane was placed in a muffle furnace and pre-fired for 2 hours in an air atmosphere at a temperature of 500°C, and then placed in a plasma equipment (Zhengzhou Kejia Electric Furnace Co., Ltd., model KJ-OTF-1700-F5), sintered for 2 hours in an argon atmosphere, the sintering temperature was 900°C, and the power of the plasma equipment was 200W to obtain a composite negative electrode material.

[0052] The composite negative electrode material of Example 1 has a double-layer coating structure, the core includes silicon nanoparticles and titanium monoxide particles, the first coating layer coated on the surface of the core contains amorphous silicon oxide, and the second coating layer coated on the surface of the first coating layer is formed by carbon fibers with a porous structure. Among them, in the composite negative electrode material, the mass proportion of silicon nanoparticles is 76%; the mass proportion of titanium monoxide particles is 6%, and the average diameter is 50nm; the mass proportion of silicon oxide is 6%, and the thickness of the first coating layer (i.e., silicon oxide layer) is 10nm; the mass proportion of carbon fiber is 12%, and the thickness of the second coating layer (i.e., carbon fiber coating layer) is 53nm, the diameter of carbon fiber is distributed in the range of 0.1-1μm, the pore size distribution range of the porous structure on carbon fiber is 5-30nm, and the porosity of the second coating layer is 95%.

[0053] Preparation of a soft-pack lithium battery:

[0054] The composite negative electrode material of Example 1 was mixed with commercial graphite in a mass ratio of 10:90 as the negative electrode active material, and dispersed in deionized water with a conductive agent Super P and a binder CMC in a mass ratio of 9:0.5:0.5 to obtain a negative electrode slurry; the negative electrode slurry was evenly coated on a copper foil current collector, vacuum dried, punched, and cut into 80×60 mm sheets to obtain a negative electrode sheet (the cross-sectional SEM photo of which is shown in FIG. 1 ). Figure 2 As shown, Figure 2The white circle in the middle represents the composite negative electrode material). The lithium iron phosphate electrode is used as the positive electrode, the above negative electrode electrode is used as the negative electrode, the PE / PP film is used as the separator, LiPF6 is used as the electrolyte, and the aluminum-plastic film is used as the shell to assemble a soft-pack lithium battery.

[0055] Preparation of a lithium button battery:

[0056] The composite negative electrode material of Example 1 was used as the active material, and was dispersed in deionized water with the conductive agent Super P and the binder sodium carboxymethyl cellulose (CMC) at a mass ratio of 7:1.5:1.5 to obtain a slurry; the slurry was then evenly coated on the negative electrode current collector copper foil, vacuum dried, punched, and cut into small discs with a diameter of 1.5 cm to obtain a pole piece. A metal lithium sheet was used as the counter electrode, a PP (polypropylene) / PE (polyethylene) laminated film was used as a separator, and LiPF6 was used as an electrolyte, and assembled with the above-mentioned pole piece into a button battery.

[0057] Example 2

[0058] The method for preparing the composite negative electrode material of Example 2 is different from that of Example 1 in that the power of the plasma equipment is 100W.

[0059] The composite negative electrode material provided in Example 2 is different from that in Example 1 in that: in the composite negative electrode material of Example 2, the mass proportion of silicon nanoparticles is 78.5%; the mass proportion of titanium monoxide particles is 5.5%, and the average diameter of titanium monoxide particles is 52nm; the mass proportion of silicon monoxide is 5%, and the thickness of the first coating layer is 9.5nm; the mass proportion of carbon fiber is 11%, and the diameter of carbon fiber is distributed in the range of 0.1-1μm, the thickness of the second coating layer is 50nm, and the porosity of the second coating layer is 75%.

[0060] Example 3

[0061] The method for preparing the composite negative electrode material of Example 3 is different from that of Example 1 in that the power of the plasma equipment is 50W.

[0062] The composite negative electrode material provided in Example 3 is different from that in Example 1 in that: in the composite negative electrode material of Example 3, the mass proportion of silicon nanoparticles is 80%; the mass proportion of titanium monoxide particles is 5%, and the average diameter of titanium monoxide particles is 56nm; the mass proportion of silicon monoxide is 4%, and the thickness of the first coating layer is 9nm; the mass proportion of carbon fiber is 11%, the thickness of the second coating layer is 48nm, and the porosity of the second coating layer is 60%.

[0063] Example 4

[0064] A method for preparing a composite negative electrode material, which is different from Example 1 in that the amount of isopropyl titanate added is 0.5 mL.

[0065] The structure of the composite negative electrode material obtained in Example 4 is basically the same as that in Example 1, and the main difference between the two is that in the composite negative electrode material of Example 4, the mass proportion of titanium monoxide particles is 3%, and other parameters fluctuate slightly or remain unchanged. Among them, the average diameter of titanium monoxide particles is 47nm; the mass proportion of silicon nanoparticles is 79%; the thickness of the first coating layer is 10nm, and the mass proportion of silicon monoxide is 6%; the thickness of the second coating layer is 53nm, the mass proportion of carbon fiber is 12%, and the porosity of the second coating layer is 93%.

[0066] Example 5

[0067] A method for preparing a composite negative electrode material, which is different from Example 1 in that the amounts of silicon nanoparticles, isopropyl titanate, butyl orthosilicate and polyacrylonitrile are 0.35 g, 2 mL, 2 mL and 2 g, respectively.

[0068] The difference between the composite negative electrode material of Example 5 and Example 1 is that in the composite negative electrode material of Example 5, the mass proportion of silicon nanoparticles is 60%; the mass proportion of titanium monoxide particles is 10%, and the average diameter of titanium monoxide particles is 51nm; the mass proportion of silicon monoxide is 10%, and the thickness of the first coating layer is 25nm; the mass proportion of carbon fiber is 20%, the thickness of the second coating layer is 130nm, and the porosity of the second coating layer is 92%.

[0069] Example 6

[0070] The method for preparing the composite negative electrode material of Example 6 is different from that of Example 1 in that the amounts of silicon nanoparticles, isopropyl titanate, butyl orthosilicate and polyacrylonitrile used are 0.4 g, 4 mL, 0.2 mL and 1.5 g, respectively.

[0071] The difference between the composite negative electrode material of Example 6 and Example 1 is that the mass proportion of silicon nanoparticles is 65%; the mass proportion of titanium monoxide particles is 20%, and the average diameter of titanium monoxide particles is 56nm; the thickness of the first coating layer is 3nm, and the mass proportion of silicon monoxide is 1%; the thickness of the second coating layer is 85nm, the mass proportion of carbon fiber is 14%, and the porosity of the second coating layer is 91%.

[0072] Example 7

[0073] A method for preparing a composite negative electrode material, which is different from Example 1 in that the sintering temperature in the plasma equipment is 800°C.

[0074] The structure of the composite negative electrode material prepared in Example 7 is basically the same as that in Example 1, except that: in the composite negative electrode material of Example 7, the mass proportion of silicon nanoparticles is 81%; the mass proportion of titanium monoxide particles is 4%, and the average diameter of titanium monoxide particles is 47nm; the thickness of the first coating layer is 8nm, the mass proportion of silicon monoxide is 4%, the thickness of the second coating layer is 53nm, the mass proportion of carbon fiber is 11%, and the porosity of the second coating layer is 90%.

[0075] Example 8

[0076] A method for preparing a composite negative electrode material, which is different from Example 1 in that the sintering temperature in the plasma equipment is 1200°C.

[0077] The difference between the composite negative electrode material of Example 8 and Example 1 is that the mass proportion of silicon nanoparticles is 74.5%; the mass proportion of titanium monoxide particles is 6.5%, and the average diameter of titanium monoxide particles is 51nm; the thickness of the first coating layer is 9.5nm, and the mass proportion of silicon monoxide is 6%; the thickness of the second coating layer is 55nm, the mass proportion of carbon fiber is 13%, and the porosity of the second coating layer is 96%.

[0078] Example 9

[0079] A method for preparing a composite negative electrode material, which is different from Example 1 in that the pre-firing temperature in an air atmosphere is 400°C.

[0080] The difference between the composite negative electrode material of Example 9 and Example 1 is that: in the composite negative electrode material, the mass proportion of silicon nanoparticles is 76.9%; the mass proportion of titanium monoxide particles is 5.7%, and the average diameter of titanium monoxide particles is 48nm; the thickness of the first coating layer is 10nm, and the mass proportion of silicon monoxide is 5.8%; the thickness of the second coating layer is 52nm, the mass proportion of carbon fiber is 11.6%, and the porosity of the second coating layer is 93%.

[0081] The composite negative electrode material provided in the above Examples 1-9 has characteristic peaks in its X-ray diffraction (XRD) spectrum at 2θ=28.4°, 47.3°, 56.1°, 69.1°, and 76.4°, which correspond to the characteristic diffraction peaks of the (111), (220), (311), (400), and (331) crystal planes of elemental silicon, respectively. The X-ray diffraction spectrum has characteristic peaks at 2θ of 37.3°, 43.4°, 63.0°, 75.4°, and 79.5°, which correspond to the characteristic diffraction peaks of the (111), (200), (220), (311), and (222) crystal planes of TiO, respectively. Among them, the half-peak width of the characteristic peak at 2θ of 28.4° is 0.2-4°, the half-peak width of the characteristic peak at 2θ of 47.3° is 0.5-5°, the half-peak width of the characteristic peak at 2θ of 56.1° is 0.1-3°, and the half-peak width of the characteristic peak at 2θ of 69.1° is 0.2-5°; the half-peak width of the characteristic peak at 2θ of 76.4° is 0.2-5°; the half-peak width of the characteristic peak at 2θ of 37.3° is 0.1-3°, the half-peak width of the characteristic peak at 2θ of 43.4° is 0.2-4°, the half-peak width of the characteristic peak at 2θ of 63.0° is 0.2-4°, the half-peak width of the characteristic peak at 2θ of 75.4° is 0.3-3°, and the half-peak width of the characteristic peak at 2θ of 79.5° is 0.2-4°. The half-width of these characteristic diffraction peaks is relatively narrow, which can reflect that the crystallization performance of the composite negative electrode material is good.

[0082] In order to highlight the beneficial effects of the present application, the following comparative example is set for Example 1.

[0083] Comparative Example 1

[0084] The difference between Comparative Example 1 and Example 1 is that after pre-sintering in a muffle furnace, the sample is placed in a plasma device and sintered at 900° C., but the power of the plasma device is 0 W (equivalent to not providing a plasma environment, but sintering in an inert atmosphere).

[0085] In the preparation of the composite negative electrode material in Comparative Example 1, since no plasma equipment was used for sintering, there were few porous structures on the outer carbon fibers, and the titanium oxide in the system was mainly titanium dioxide.

[0086] Comparative Example 2

[0087] The difference between Comparative Example 2 and Example 1 is that butyl orthosilicate is not added when preparing the mixed solution for electrospinning.

[0088] Compared with Example 1, the composite negative electrode material obtained in Comparative Example 2 does not have a silicon oxide coating layer between the inner core and the porous carbon fiber coating layer.

[0089] Comparative Example 3

[0090] The difference between Comparative Example 3 and Example 1 is that isopropyl titanate is not added when preparing the mixed solution for electrospinning.

[0091] Compared with Example 1, the composite negative electrode material obtained in Comparative Example 3 has a core containing only silicon nanoparticles but no titanium monoxide.

[0092] Comparative Example 4

[0093] The difference between Comparative Example 4 and Example 1 is that the mixed solution of Example 1 is not subjected to electrospinning, but is centrifuged and vacuum dried at 105°C for 12 hours to obtain a mixed powder. The mixed powder is first calcined in a muffle furnace at a temperature of 500°C for 2 hours, and then placed in a plasma device for calcination for 2 hours at a temperature of 900°C, but the power of the plasma device is 0 W.

[0094] In the composite negative electrode material obtained in Comparative Example 4, the outermost coating layer is an amorphous carbon coating layer. This is mainly because polyacrylonitrile is not electrospun to form spinning fibers, and thus no carbon fibers can be obtained after sintering.

[0095] In order to strongly support the beneficial effects of the present application, the negative electrode composite materials of the above embodiments and comparative examples were respectively assembled into button cells and soft-pack lithium batteries according to the method described in Example 1. In addition, commercial silicon nanomaterials were also assembled into button cells and soft-pack lithium batteries as negative electrode materials to form comparative example 5.

[0096] Each button cell and soft-pack lithium battery is placed in a blue electric test cabinet for charge and discharge cycle testing, with a charge and discharge current of 0.5C. The voltage range of the button cell is 0.005-1.5V, and the voltage range of the soft-pack cell is 2-3.8V. When charging, each battery is first charged at a constant current of 0.5C to the charge cut-off voltage (1.5V for button cells and 3.8V for soft-pack cells), and then charged at a constant voltage to a full charge state, with a cut-off current of 0.05C; when discharging, it is discharged at a constant current of 0.5C to the corresponding discharge cut-off voltage (0.005V for button cells and 2V for soft-pack cells). Test the first charge specific capacity, first discharge specific capacity, first coulomb efficiency, capacity retention rate after a certain number of cycles, cycle life, etc. of each battery.

[0097] Among them, the first charge specific capacity of each soft-pack lithium battery and button battery refers to the ratio of the capacity charged in the first charge of each battery to the mass of the active material serving as the positive electrode of the battery; its first discharge specific capacity refers to the ratio of the capacity discharged in the first discharge of each battery to the mass of the active material serving as the positive electrode of the battery. The first (or "first cycle") coulomb efficiency of each soft-pack lithium battery and button battery refers to the ratio of the first discharge specific capacity of the corresponding battery to its first charge specific capacity. The capacity retention rate of each button battery and soft-pack lithium battery refers to the ratio of the discharge capacity of the corresponding battery after a certain number of cycles (300 cycles for button batteries and 600 cycles for soft-pack lithium batteries) to its first discharge capacity. The cycle life of each button battery and soft-pack lithium battery refers to the number of cycles corresponding to the time when the discharge capacity of the battery decays to 80% of the initial discharge capacity.

[0098] In addition, the soft-pack full battery is also subjected to EIS (alternating current impedance) testing, the testing method includes: discharging each assembled soft-pack full battery to 50% SOC cutoff, and performing EIS testing on a Gammary electrochemical workstation, with a test frequency of 100KHz to 0.05Hz.

[0099] The test results are summarized in Table 1 and Table 2 below.

[0100] Table 1 Summary of test results of button batteries of various embodiments and comparative examples

[0101]

[0102] Table 2 Summary of test results of soft-pack batteries of various embodiments and comparative examples

[0103]

[0104] Note: The cycle performance of the soft-pack batteries in several comparative examples is poor, and the cycle life cannot reach 600 cycles. The cycle capacity retention rate data of the soft-pack batteries in comparative examples 1-5 in Table 2 are the data when they reach the corresponding cycle life number of cycles.

[0105] From Table 1 and Figure 3 It can be seen that the button battery of the embodiment of the present application has a longer cycle life, and there is no obvious diving phenomenon after more than 300 cycles, while the comparative example has an obvious diving phenomenon after 200 cycles. It can be seen that the composite negative electrode material of the present application has excellent cycle stability.

[0106] From Table 2 and Figure 4It can be seen that the EIS value of the soft-pack battery in the embodiment of the present application is small, the conductivity is good, and the cycle performance is better. In addition, it can be seen from the data of Examples 1-3 that increasing the power of plasma treatment can increase the porosity of the porous carbon fiber coating layer, which can significantly improve the conductivity of the composite negative electrode material, reduce the impedance of the battery, and improve the cycle performance. The conductivity of the negative electrode material of Comparative Examples 1-5 is worse than that of the embodiment of the present application, and the material porosity is low, the ion diffusion impedance is large, and therefore the cycle life is short.

[0107] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A composite negative electrode material, characterized in that: The composite negative electrode material comprises a core, a first coating layer coated on the surface of the core, and a second coating layer coated on the surface of the first coating layer, wherein the core comprises silicon nanoparticles and titanium monoxide particles; the first coating layer comprises silicon monoxide; and the second coating layer comprises carbon fibers having a porous structure; Wherein, the composite negative electrode material is prepared by the following preparation method: (1) dispersing silicon nanoparticles in an alcohol-containing solvent, adding titanate and dispersing them uniformly, and then adding silicate and a spinnable carbon source and dispersing them uniformly to obtain a mixed solution; electrospinning the mixed solution to obtain a composite fiber membrane; (2) The composite fiber membrane is pre-fired at 200-500°C in an air atmosphere, and then the pre-fired composite fiber membrane is sintered in a plasma device under an inert atmosphere to obtain the composite negative electrode material; wherein the power of the plasma device is 50-200W and the sintering temperature is 800-1200°C.

2. The composite negative electrode material according to claim 1, characterized in that The diameter distribution range of the silicon nanoparticles is 80-150 nm.

3. The composite negative electrode material according to claim 1, characterized in that The silicon nanoparticles account for 60%-82% by mass in the composite negative electrode material.

4. The composite negative electrode material according to claim 1, characterized in that The average diameter of the titanium monoxide particles is 40-60 nm.

5. The composite negative electrode material according to claim 1, characterized in that The mass proportion of the titanium monoxide particles in the composite negative electrode material is 2.5%-20%.

6. The composite negative electrode material according to claim 1, characterized in that The thickness of the first coating layer is 3-25 nm.

7. The composite negative electrode material according to claim 1, characterized in that: The silicon oxide is amorphous silicon oxide; the chemical formula of the silicon oxide is SiOx, 1≤x<2; the mass of the silicon oxide accounts for 1-10% of the mass of the composite negative electrode material.

8. The composite negative electrode material according to claim 1, characterized in that The thickness of the second coating layer is 40-130 nm.

9. The composite negative electrode material according to claim 1, characterized in that: The mass of the carbon fiber accounts for 10-20% of the mass of the composite negative electrode material.

10. The composite negative electrode material according to any one of claims 1 to 9, characterized in that: The porosity of the second coating layer is 60%-96%.

11. The composite negative electrode material according to any one of claims 1 to 9, characterized in that: The pore size distribution range of the porous structure on the carbon fiber is 5-30nm; the diameter distribution range of the carbon fiber is 0.1-1μm.

12. A method for preparing a composite negative electrode material according to any one of claims 1 to 11, characterized in that: The following steps are involved: (1) dispersing silicon nanoparticles in an alcohol-containing solvent, adding titanate and dispersing them uniformly, and then adding silicate and a spinnable carbon source and dispersing them uniformly to obtain a mixed solution; electrospinning the mixed solution to obtain a composite fiber membrane; (2) The composite fiber membrane is pre-fired at 200-500°C in an air atmosphere, and then the pre-fired composite fiber membrane is sintered in a plasma device under an inert atmosphere to obtain the composite negative electrode material; wherein the power of the plasma device is 50-200W and the sintering temperature is 800-1200°C.

13. The preparation method according to claim 12, characterized in that: The preparation method of the mixed solution comprises: first dispersing silicon nanoparticles in an alcohol-containing solvent, then adding titanate and dispersing uniformly, then adding silicate and dispersing uniformly, and finally adding a spinnable carbon source and dispersing uniformly to obtain the mixed solution.

14. The preparation method according to claim 12, characterized in that: The sintering time is 1-3 hours; the pre-burning time is 1-3 hours.

15. A negative electrode plate, characterized in that: Contains the composite negative electrode material as described in any one of claims 1 to 11.

16. A battery, characterized in that: Comprising the negative electrode sheet as described in claim 15.

Citation Information

Cited By

  • Composite negative electrode material, preparation method therefor, negative electrode piece, battery, and electric device

    EP4478459A1