Modified titanium dioxide photocatalyst and preparation method thereof
By modifying titanium dioxide polyglycidyl and photosensitizer, the electron/hole recombination rate is reduced, the problem of low efficiency of TiO2 in visible light is solved, and the efficient application of modified titanium dioxide photocatalysts in water pollution treatment is achieved.
Patent Information
- Application Number
- CN202310891085.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-07-19
AI Technical Summary
TiO2 photocatalysts have low efficiency under visible light sources and high electron/hole recombination rate, which limits their application in water pollution treatment.
Use polyglycidyl and photosensitizers (such as heme chloride, eosin Y) to modify titanium dioxide, and form a modified titanium dioxide photocatalyst through grafting or blending to reduce electron/hole recombination and improve photocatalytic performance. .
The photocatalytic performance of modified titanium dioxide is significantly improved, and the degradation ability of pollutants is enhanced, especially in ultraviolet light and visible light.
Smart Images

Figure CN116786172B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalysts, and in particular to a modified titanium dioxide photocatalyst and a preparation method thereof. Background Art
[0002] TiO2 has become a focus of attention in the field of photocatalysis because of its non-toxic, reasonable cost, environmental friendliness, easy synthesis at low temperature and good chemical stability, and has attracted more and more attention in the field of water treatment and environmental remediation. However, TiO2 can only absorb ultraviolet light and higher energy electromagnetic waves, which limits its application in actual water pollution treatment. Various modifications to TiO2 to improve its photocatalytic performance under visible light sources are a relatively direct and effective means. For example, Zhang Yanan used a hydrothermal method to compound two non-metallic elements, namely N and F, with graphene / TiO2, and successfully prepared N, F modified graphene / titanium dioxide (NF-RGO / TiO2) composite materials, in which N and F elements were doped with urea and NH4F as raw materials. Li Cuixia and other researchers used tetrabutyl titanate as a titanium source to in-situ hydrolyze and prepare lanthanum-doped graphene / TiO2 to form a composite material. Citric acid (CA) was added as a chelating agent during the preparation process, and GO was reduced with sodium borohydride. La 3+ The size of the TiO2 nanoparticles is about 6-8 nm, and they are evenly dispersed on the wrinkles and flat areas of the graphene surface. However, in the current field of photocatalysis, few studies have been able to effectively reduce the electron / hole (e / hole) in TiO2 photocatalysis. - -h + ) recombination rate to improve the photocatalytic performance.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a modified titanium dioxide photocatalyst and a preparation method thereof. The modified titanium dioxide photocatalyst provided in the embodiment of the present invention can effectively reduce the electron / hole (e - -h + ) recombination rate and has excellent photocatalytic performance.
[0005] The present invention is achieved in that:
[0006] In a first aspect, the present invention provides a modified titanium dioxide photocatalyst, which comprises titanium dioxide, polyglycidol for modifying the titanium dioxide, and a photosensitizer.
[0007] In an optional embodiment, the modified titanium dioxide photocatalyst includes the following (1) or (2) photocatalyst: (1) a photocatalyst formed by grafting the polyglycidol and the photosensitizer to form a grafted product and then doping the titanium dioxide; (2) a photocatalyst formed by co-mixing the polyglycidol and the photosensitizer and doping the titanium dioxide.
[0008] In an alternative embodiment, the photosensitizer comprises hemin and eosin Y.
[0009] In an optional embodiment, when the polyglycidol and the photosensitizer are co-doped with the titanium dioxide, the doping amount of the polyglycidol is 0.1-3%, and the doping amount of the photosensitizer is 3-4%;
[0010] When the polyglycidol and the photosensitizer are grafted and then doped with the titanium dioxide, the content of the grafted product is 2-4% or 0.5-1%.
[0011] In an optional embodiment, the modified titanium dioxide photocatalyst is selected from any one of the following photocatalysts;
[0012] (1) The photocatalyst formed by grafting the polyglycidol and the hemin and doping the titanium dioxide; wherein the doping amount of the grafted product is 0.5-1% or 2-4%;
[0013] (2) a photocatalyst formed by doping the titanium dioxide after the polyglycidol and the eosin Y are grafted; wherein the doping amount of the grafted product is 2-4% or 0.5-1%;
[0014] (3) When the hemin or the eosin Y and the polyglycidol are mixed and doped with the titanium dioxide, the doping amount of the polyglycidol is 0.1-3%, and the doping amount of the hemin or the eosin Y is 3-4%.
[0015] In an optional embodiment, the degree of polymerization of the polyglycidol is 123-178, and the degree of branching is 0.15-2.16;
[0016] The mass fraction of the photosensitizer in the grafted product is 3-37%.
[0017] In a second aspect, the present invention provides a method for preparing the modified titanium dioxide photocatalyst described in the aforementioned embodiment, comprising: modifying titanium dioxide using polyglycidol and a photosensitizer.
[0018] In an optional embodiment, the method comprises: subjecting the polyglycidol and the photosensitizer to a grafting reaction to form a grafted product, and then mixing the grafted product with a titanate compound and a hydrolysis agent to react to form titanium dioxide and doping the grafted product with the titanium dioxide.
[0019] In an optional embodiment, the method comprises: mixing the polyglycidol, the photosensitizer titanate compound and a hydrolysis agent to react to form titanium dioxide and allowing the polyglycidol and the photosensitizer to be doped with the titanium dioxide.
[0020] In an optional embodiment, the titanate compound includes butyl titanate, and the hydrolysis agent includes glacial acetic acid.
[0021] The present invention has the following beneficial effects: In the embodiment of the present invention, polyglycidol and a photosensitizer are specifically used to modify titanium dioxide, so that the formed modified titanium dioxide can effectively reduce the electron / hole (e) of photocatalysis. - -h + ) recombination rate and has excellent photocatalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 The test result diagram provided for Characterization 1 of the present invention;
[0024] Figure 2 The test result diagram provided for Characterization 2 of the present invention;
[0025] Figure 3 The test result diagram provided for Characterization 3 of the present invention;
[0026] Figure 4 The test result diagram provided for Characterization 4 of the present invention;
[0027] Figure 5 The test result diagram provided for Experimental Example 1 of the present invention;
[0028] Figure 6 The test result diagram provided for Experimental Example 2 of the present invention;
[0029] Figure 7 The test result diagram provided for Experimental Example 3 of the present invention;
[0030] Figure 8 The test result diagram provided for Experimental Example 4 of the present invention;
[0031] Fig. 9 The test result diagram provided for Experimental Example 5 of the present invention;
[0032] Fig.10 The test result diagram provided for Experimental Example 6 of the present invention;
[0033] Fig.11 The test result diagram provided for Experimental Example 7 of the present invention;
[0034] Fig.12 The test result diagram provided for Experimental Example 8 of the present invention;
[0035] Fig.13 The test result diagram provided for Experimental Example 9 of the present invention;
[0036] Fig.14 The test result diagram provided for Experimental Example 10 of the present invention;
[0037] Fig.15 The test result diagram provided for Experimental Example 11 of the present invention;
[0038] Fig.16 The test result diagram provided for Experimental Example 12 of the present invention;
[0039] Fig.17 The test result diagram provided for Experimental Example 13 of the present invention;
[0040] Fig.18 The test result diagram provided for Experimental Example 14 of the present invention;
[0041] Fig.19 The test result diagram provided for Experimental Example 15 of the present invention;
[0042] Fig. 20 The test result diagram provided for Experimental Example 16 of the present invention;
[0043] Figure 21-22 This is a test result diagram provided for Experimental Example 17 of the present invention. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0045] The embodiment of the present invention provides a modified titanium dioxide photocatalyst, which comprises titanium dioxide, polyglycidol for modifying the titanium dioxide, and a photosensitizer.
[0046] The modified titanium dioxide photocatalyst includes the following (1) or (2) photocatalysts: (1) a photocatalyst formed by doping the titanium dioxide with a grafted product formed by grafting the polyglycidol and the photosensitizer; (2) a photocatalyst formed by doping the titanium dioxide with the polyglycidol and the photosensitizer. That is, the method of modifying titanium dioxide with polyglycidol and the photosensitizer can be to dope the titanium dioxide with a grafted product formed by grafting the polyglycidol and the photosensitizer, or to dope the titanium dioxide with the two by directly physically blending.
[0047] Further, the photosensitizer may be selected from hemin and eosin Y.
[0048] More specifically, the modified titanium dioxide provided in the embodiment of the present invention can be: a photocatalyst formed by doping the titanium dioxide after grafting polyglycidol and the hemin; it can be a photocatalyst formed by doping the titanium dioxide after grafting polyglycidol and the eosin Y; it can be a photocatalyst formed by doping the titanium dioxide after grafting polyglycidol and eosin Y; it can be a photocatalyst formed by mixing and doping the titanium dioxide with red Y and the polyglycidol; it can also be a photocatalyst formed by mixing and doping the titanium dioxide with hemin and the polyglycidol.
[0049] Wherein, during blending, the doping amount of polyglycidol is 0.1-3%, and the doping amount of the hemin or eosin Y is 3-4%. During grafting and doping, the doping amount of the grafted product is 2-4% or 0.5-1%, and the mass fraction of the photosensitizer in the grafted product is 3-37%. The degree of polymerization of polyglycidol is 123-178, and the degree of branching is 0.15-2.16;
[0050] In a second aspect, the present invention provides a method for preparing the modified titanium dioxide photocatalyst described in the aforementioned embodiment, comprising:
[0051] S1, synthesis of polyglycidol (abbreviated as HPG);
[0052] HPG was synthesized according to the following synthetic route;
[0053] Wherein, m, n and o represent the degree of polymerization of three different ring-opening structural units of glycidol monomer in polyglycidol.
[0054] The specific synthesis method is an existing method and will not be described in detail in the embodiments of the present invention.
[0055] S2, grafting;
[0056] Take hemin and eosin Y as examples for illustration. Specifically, the grafting reaction is carried out according to the following synthetic route:
[0057] or
[0058] Specifically, a photosensitizer, such as hemin or eosin Y, is dissolved, and then DCC and DMAP are added and stirred under a protective gas atmosphere;
[0059] HPG was dissolved and then dripped into the above solution, stirred and reacted in a protective gas atmosphere away from light, and then precipitated with acetone, and the solid precipitate was dissolved with methanol, and then precipitation-dissolution was repeated several times to remove impurities, and then the precipitate was collected and dried.
[0060] S3, doping;
[0061] The steps of doping with the grafted product are as follows:
[0062] The grafted product is mixed with water to form a dispersion, and mixed with an organic solvent and a hydrolysis agent such as glacial acetic acid to form a mixed solution;
[0063] The titanate compound is dissolved in an organic solvent to form a mixed solution, and then the mixed solution is added into a mixed solution to undergo a hydrolysis reaction, and after the reaction is completed, the mixture is dried, ground and heat-treated.
[0064] The steps of direct doping of photosensitizer and HPG are as follows:
[0065] The HPG and photosensitizer are mixed and dispersed with water to form a dispersion, and mixed with an organic solvent and a hydrolysis agent such as glacial acetic acid to form a mixed solution;
[0066] The titanate compound is dissolved in an organic solvent to form a mixed solution, and then the mixed solution is added into a mixed solution to undergo a hydrolysis reaction, and after the reaction is completed, the mixture is dried, ground and heat-treated.
[0067] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0068] Example 1
[0069] This embodiment provides a method for synthesizing polyglycidol, comprising:
[0070] The following steps are merely examples of the embodiments of the present invention:
[0071] ① Use a 25 mL round-bottom flask. During the polymerization process, keep the round-bottom flask in a digital constant-temperature magnetic stirrer containing a mixed solution of acetone and dry ice to ensure a constant reaction temperature of -20°C.
[0072] ② Install septa on two 1-dram (1dr=1.77185 g) vials. First, dry the vials with a flame for a few seconds and then introduce nitrogen.
[0073] ③ The first vial was prepared with 1.7 mol / L isoamyl alcohol solution (THF as solvent), while the second 1-dram bottle was prepared with 3.7x10 -2 mol / L tin trifluoromethanesulfonate solution (THF as solvent).
[0074] ④ Add 0.20 mL of isoamyl alcohol solution and 0.26 mL of tin trifluoromethanesulfonate into a round-bottom flask with a magnetic stirring bar and react at a constant reaction temperature, and continue stirring for 30 minutes to allow the alcohol and the catalyst to combine.
[0075] ⑤ After the activation step, 2.00 g of glycidol monomer was added dropwise.
[0076] ⑥ After the synthesis of polyglycidol, stop stirring, dissolve the crude viscous polymer product in a small amount of methanol (control is required here, add methanol drop by drop to make the product not too viscous), and then pour it into vigorously stirred n-hexane for precipitation to obtain a pure glycidol homopolymer product.
[0077] ⑦ Based on step ⑥, polyglycidol is collected by liquid separation operation and dried in an oven at 90° C. for 24 hours to remove residual n-hexane and methanol. The obtained polyglycidol is recorded as HPG1.
[0078] Example 2
[0079] This embodiment provides a method for synthesizing polyglycidol, which refers to the method of Example 1, except that the amount of isoamyl alcohol in step ④ is changed to 0.16 mL, and the obtained polyglycidol is recorded as HPG2.
[0080] Example 3
[0081] This embodiment provides a method for synthesizing polyglycidol, which refers to the method of Example 1, except that the acetone and dry ice solution in step ① is replaced with a 40° C. constant temperature oil bath, and the obtained polyglycidol is recorded as HPG3.
[0082] Example 4
[0083] This embodiment provides a method for synthesizing a polyglycidol-photosensitizer graft product, comprising:
[0084] ①Put 2.5 mL of DMF in a three-necked flask
[0085] ② Dissolve 1 mg of hemin in DMF, then add DCC and DMAP, mix and stir at 0℃ under nitrogen atmosphere for 30 minutes.
[0086] ③ 0.5 g of HPG1 prepared in Example 1 was dissolved in 2.5 mL of DMF and added dropwise into the above mixed solution while the mixed solution was kept in a stirring state.
[0087] ④Stir the reaction at room temperature under nitrogen atmosphere for two days in the dark.
[0088] ⑤ The mixture was precipitated in 500 mL of acetone, the product was dissolved in methanol, and then precipitated with acetone again, and the impurities were removed by repeating five times, after which the modified polymer was collected and vacuum dried at 40°C for 48 hours. The obtained grafted product was recorded as HPG1-hemin.
[0089] Example 5
[0090] This embodiment provides a method for synthesizing a polyglycidol-photosensitizer graft product, which is the same as that of embodiment 4, except that HPG1 in step ③ is replaced by HPG2 in embodiment 2, and the obtained graft product is recorded as HPG2-hemin.
[0091] Example 6
[0092] This embodiment provides a method for synthesizing a polyglycidol-photosensitizer graft product, which is the same as that of embodiment 4, except that one more drop of phosphoric acid is added in step ②, and the obtained graft product is recorded as HPG1-EY.
[0093] Example 7
[0094] This embodiment provides a method for synthesizing a polyglycidol-photosensitizer graft product, which is the same as that of Embodiment 6, except that HPG1 in step ③ is replaced by HPG3 prepared in Embodiment 3, and the obtained graft product is recorded as HPG3-EY.
[0095] Example 8
[0096] This embodiment provides a method for preparing modified titanium dioxide, comprising:
[0097] ① Take 10 mL of distilled water for later use, add 0.1% HPG1-hemin and dissolve it in 10 mL of distilled water, and disperse the HPG1-hemin using an ultrasonic cleaner at room temperature for 30 minutes.
[0098] ② At room temperature, take 35 mL of anhydrous ethanol as the solvent, add 10 mL of butyl titanate, seal it and stir evenly for 10 minutes to form a colorless and transparent uniform solution, and store it for later use.
[0099] ③ Take another 35 mL of anhydrous ethanol as the solvent, add 10 mL of distilled water in step ① into the anhydrous ethanol, and then add 4 mL of glacial acetic acid, and then keep stirring evenly to obtain a new mixed solution.
[0100] ④ Keep the mixed solution obtained in step ③ under uniform stirring, and slowly add the solution prepared in step ② into the mixed solution at a rate of 3 mL / min to allow the hydrolysis reaction to proceed at a uniform rate.
[0101] ⑤ After the above experimental operation is completed, the system is stirred at a constant speed for 30 minutes, and then placed in a constant temperature water bath at 45°C for 30 minutes to obtain a light green gel.
[0102] ⑥ The prepared gel is placed in an oven at 105°C for drying, and then ground. The ground powder is placed in a ceramic crucible and heat treated at 260°C for 2.5 hours to obtain polyglycidol grafted hemin doped titanium dioxide powder recorded as 0.1% HPG1-hemin / TiO2.
[0103] Examples 9-12
[0104] Examples 9-12 prepare modified titanium dioxide by referring to the preparation method of modified titanium dioxide provided in Example 8, with the only difference being the doping of HPG1-hemin, which is 0.5%, 1%, 2% and 3%, respectively, and then recorded as 0.5% HPG1-hemin / TiO2, 1% HPG1-hemin / TiO2, 2% HPG1-hemin / TiO2 and 3% HPG1-hemin / TiO2, respectively.
[0105] Example 13-Example 17
[0106] In Example 13 to Example 17, modified titanium dioxide was prepared in accordance with Examples 8 to 12, respectively, with the only difference being that HPG1-hemin was replaced by HPG2-hemin. Therefore, the modified titanium dioxide prepared in Example 13 to Example 17 were recorded as 1% HPG2-hemin / TiO2, 2% HPG2-hemin / TiO2, 3% HPG2-hemin / TiO2, 4% HPG2-hemin / TiO2 and 5% HPG2-hemin / TiO2, respectively.
[0107] Example 18-Example 22
[0108] In Example 18 to Example 22, modified titanium dioxide was prepared in accordance with Examples 8 to 12, respectively, with the only difference being that HPG1-hemin was replaced by HPG1-EY. Therefore, the modified titanium dioxide prepared in Example 18 to Example 22 were recorded as 1% HPG1-EY / TiO2, 2% HPG1-EY / TiO2, 3% HPG1-EY / TiO2, 4% HPG1-EY / TiO2 and 5% HPG1-EY / TiO2, respectively.
[0109] Example 23-Example 27
[0110] Example 23-Example 27 were used to prepare modified titanium dioxide in accordance with Examples 18-22, with the only difference being that HPG1-EY was replaced by HPG3-EY. Therefore, the modified titanium dioxide prepared in Example 23-Example 27 were recorded as 0.1% HPG3-EY / TiO2, 0.5% HPG3-EY / TiO2, 1% HPG3-EY / TiO2, 2% HPG3-EY / TiO2 and 3% HPG3-EY / TiO2, respectively.
[0111] Embodiment 28
[0112] This embodiment provides a method for preparing modified titanium dioxide, comprising:
[0113] ① Take 10 mL of distilled water for use, add 3% by mass of hemin and 0.1% by mass of HPG1 and dissolve them in 10 mL of distilled water, and use an ultrasonic cleaner to disperse the hemin and HPG1 at room temperature for 30 minutes.
[0114] ② At room temperature, take 35 mL of anhydrous ethanol as the solvent, add 10 mL of butyl titanate, seal it and stir evenly for 10 minutes to form a colorless and transparent uniform solution, and store it for later use.
[0115] ③ Take another 35 mL of anhydrous ethanol as the solvent, add 10 mL of distilled water in step ① into the anhydrous ethanol, and then add 4 mL of glacial acetic acid, and then keep stirring evenly to obtain a new mixed solution.
[0116] ④ Keep the mixed solution obtained in step ③ under uniform stirring, and slowly add the solution prepared in step ② into the mixed solution at a rate of 3 mL / min to allow the hydrolysis reaction to proceed at a uniform rate.
[0117] ⑤ After the above experimental operation is completed, the system is stirred at a constant speed for 30 minutes, and then placed in a constant temperature water bath at 45°C for 30 minutes to obtain a light green gel.
[0118] ⑥ The prepared gel is placed in an oven at 105°C for drying, and then ground. The ground powder is placed in a ceramic crucible and heat treated at 260°C for 2.5 hours to obtain polyglycidol composite hemin chloride doped titanium dioxide powder recorded as 0.1% HPG1 / 3% hemin / TiO2.
[0119] Examples 29-32
[0120] Examples 29-32 prepare modified titanium dioxide by referring to the preparation method of modified titanium dioxide provided in Example 28, with the only difference being the doping of HPG1, which is 0.5%, 1%, 2% and 3% respectively, and then recorded as 0.5% HPG1 / 3% hemin / TiO2, 1% HPG1 / 3% hemin / TiO2, 2% HPG1 / 3% hemin / TiO2 and 3% HPG1 / 3% hemin / TiO2 respectively.
[0121] Examples 33-37
[0122] Examples 33-37 respectively refer to the preparation method of the modified titanium dioxide provided in Examples 28-32 for preparing modified titanium dioxide, with the only difference being that 3% of hemin is replaced by 4% of eosin Y. The prepared modified titanium dioxide are respectively recorded as 0.1% HPG1 / 4%EY / TiO2, 0.5% HPG1 / 4%EY / TiO2, 1% HPG1 / 4%EY / TiO2, 2% HPG1 / 4%EY / TiO2 and 3% HPG1 / 4%EY / TiO2.
[0123] Representation 1
[0124] The polyglycidol prepared in Example 1 to Example 3 was subjected to nuclear magnetic resonance detection to obtain its hydrogen spectrum. Figure 1 , Figure 1 a in the middle represents the H NMR spectrum of HPG1; Figure 1 b in the middle represents the H NMR spectrum of HPG2; Figure 1 Figure c in the figure shows the H NMR spectrum of HPG3.
[0125] according to Figure 1 From a, we can see that the hydrogen atom at the chemical shift of 0.94 is the methyl hydrogen of the initiator isopentanol. The chemical shift is marked as 6. Then, we can integrate and get a total of 690 hydrogen atoms in a polyglycidol molecular chain except for the hydroxyl group and the initiator. The degree of polymerization of polyglycidol can be calculated by formula 1:
[0126]
[0127] In the formula, n(H) is the number of H atoms obtained by integration, and 5 is the number of hydrogen atoms in the glycidol monomer structure in HPG.
[0128] According to formula 1, the degree of polymerization of HPG1 is 138, the degree of polymerization of HPG2 is 178, and the ratio of the degree of polymerization of HPG1 and HPG2 is close to 8:10, indicating that HPGs with different degrees of polymerization have been successfully synthesized, and the degree of polymerization of HPG can be effectively controlled by changing the amount of initiator. The degree of polymerization of HPG3 is 123, and the ratio of the degree of polymerization of HPG1 and HPG3 is about 1:1, indicating that changing the polymerization temperature will not affect the degree of polymerization of HPG.
[0129] Representation 2
[0130] The polyglycidol prepared in Example 1 and Example 3 was subjected to nuclear magnetic resonance detection to obtain its carbon spectrum. Figure 2 , Figure 2 a in the middle represents the NMR carbon spectrum of HPG1; Figure 1 Figure b shows the NMR carbon spectrum of HPG3.
[0131] from Figure 2 It can be observed that glycidol mainly undergoes catalytic ring-opening polymerization during the polymerization process, and nuclear magnetic resonance carbon spectrum analysis shows that it has four structural units: linear (L 1,3 ), linear (L 1,4 ), dendritic (D) and terminal (T), and the degree of branching of the hyperbranched polyglycidol can be calculated using the following formula:
[0132]
[0133] In the formula, DB is the degree of branching of the desired polymer, and 2D, L1,3, and L1,4 are the numbers of carbon atoms obtained by the corresponding integration of the NMR carbon spectrum.
[0134] Calculated by formula 2, the branching degree of HPG1 is 0.15, and the branching degree of HPG3 is 2.16, which shows that the branching degree of HPG can be effectively controlled by temperature change, and the higher the reaction temperature, the higher the branching degree of the synthesized HPG. This HPG with a higher branching degree can provide more hydroxyl groups for the photocatalytic reaction.
[0135] Representation 3
[0136] HPG1, hemin, EY, HPG1-hemin and HPG1-EY were detected by infrared. The results are shown in Figure 3 , Figure 3 a in the figure shows the infrared spectra of HPG1, hemin and HPG1-hemin; Figure 3 Panel b shows the infrared spectra of HPG1, EY and HPG1-EY.
[0137] according to Figure 3 As shown in Figure a, the infrared spectra of HPG1-hemin are roughly similar to those of HPG1, and the peak intensity is slightly stronger than that of HPG1, which indicates that there is a certain interaction between HPG1 and hemin. The infrared spectrum of HPG1-hemin is 3417cm -1 The absorption peak at 1660cm -1 The carbonyl peak appears at 1104 cm -1The original COC vibration peak is enhanced to a certain extent. This is because some hydroxyl groups of HPG1 undergo esterification reaction with the carboxyl groups of hemin, which weakens the stretching vibration peak of -OH in HPG1-hemin to a certain extent. The formation of ester bond causes carbonyl peak to appear in the infrared spectrum, and the COC vibration peak is enhanced to a certain extent, indicating that HPG1 and hemin are successfully grafted.
[0138] according to Figure 3 As shown in Figure b, the infrared spectrum of HPG1-EY is similar to that of EY. -1 The hydroxyl absorption peak at the position of HPG1-EY did not change significantly. This is because, on the one hand, the hydroxyl group of HPG1 reacted with the carboxyl group of EY for esterification, and on the other hand, the grafted EY molecules also contained new hydroxyl groups. Compared with HPG1, HPG1-EY has a higher absorption peak at 1075 cm -1 The COC vibration peak at 1645cm -1 There is also an obvious carbonyl peak at 1563 cm -1 The position is the keto carbonyl peak of the EY molecule, indicating that HPG1 and EY were successfully grafted.
[0139] Representation 4
[0140] Thermogravimetric analysis of HPG1-hemin, HPG2-hemin, HPG1-EY and HPG3-EY was performed. The results are shown in Figure 4 (TG and DTG curves), where Figure 4 a in the middle shows the thermogravimetric analysis diagram of HPG1-hemin; Figure 4 b shows the thermogravimetric analysis diagram of HPG2-hemin; Figure 4 c represents the thermogravimetric analysis diagram of HPG1-EY; and Figure 4 (d) shows the thermogravimetric analysis diagram of HPG3-EY.
[0141] according to Figure 4 It can be seen that HPG1-hemin reaches the maximum decomposition rate at 369°C, HPG2-hemin reaches the maximum decomposition rate at 302°C, HPG1-EY reaches the maximum decomposition rate at 312°C, and HPG5-EY reaches the maximum decomposition rate at 283°C. Figure 4 The residual mass fraction observed at 700°C is the mass fraction of the successfully grafted photosensitizer. The mass fraction of hemin in HPG1-hemin is 3.42%, the mass fraction of hemin in HPG2-hemin is 13.13%, the mass fraction of EY in HPG1-EY is 33.33%, and the mass fraction of EY in HPG5-EY is 37.51%. Figure 4From (a) and (b), it can be concluded that the increase in the degree of polymerization can effectively increase the grafting rate of the photosensitizer, because the increase in the degree of polymerization allows the polymer to have more hydroxyl groups to react with the photosensitizer. Figure 4 From (c) and (d), it can be seen that the increase in the degree of branching can increase the grafting rate of the photosensitizer. This is because the higher the degree of branching of the polymer, the more hydroxyl groups are exposed on the surface, and the contact with the photosensitizer is more complete during the grafting reaction, so the grafting rate can be increased to a certain extent.
[0142] In summary, the molecular weight distribution of the synthesized HPG is relatively uniform. By comparing the number average molecular weight Mn of the polymer and its corresponding grafted product, it can be obtained that: the mass fraction of EY in HPG1-EY is about 25.86%; the mass fraction of EY in HPG5-EY is about 32.45%; the mass fraction of hemin in HPG1-hemin is about 9.58%; the mass fraction of hemin in HPG2-hemin is about 14.22%. Compared with the ungrafted polymer, the number average molecular weight Mn of the grafted products of the same polymer shows a certain amount of increase, indicating that the photosensitizer and the polymer are successfully grafted, which is consistent with the results of infrared analysis, and the growth ratio is relatively consistent with the results of TGA analysis, thereby determining the grafting rate of photosensitizer and HPG.
[0143] Experimental Example 1
[0144] Powder diffraction analysis was performed on TiO2, 1% HPG1-hemin / TiO2, 3% HPG2-hemin / TiO2, 3% HPG1-EY / TiO2, 1% HPG3-EY / TiO2, 1% HPG1 / 3% hemin / TiO2 and 1% HPG1 / 4% EY / TiO2. The results are shown in Figure 5 .
[0145] according to Figure 5It can be seen that the XRD curve of TiO2 shows 9 main diffraction peaks. By comparing with the PDF standard card JCPDS No. 21-1272, it is concluded that the above 9 diffraction peaks are the main diffraction peaks of anatase TiO2, and the corresponding comparison relationships are: 25.48° corresponds to the (101) crystal plane, 38.17° corresponds to the (004) crystal plane, 48.23° corresponds to the (200) crystal plane, 54.07° corresponds to the (105) crystal plane, 55.41° corresponds to the (211) crystal plane, 62.72° corresponds to the (204) crystal plane, 69.10° corresponds to the (116) crystal plane, 70.46° corresponds to the (117) crystal plane, and 71.30° corresponds to the (123) crystal plane. ° corresponds to the (220) crystal plane, 75.31° corresponds to the (215) crystal plane; except for the above 9 diffraction peaks, no other diffraction peaks appear, indicating that the prepared 1% HPG1-hemin / TiO2, 3% HPG2-hemin / TiO2, 3% HPG1-EY / TiO2, 1% HPG3-EY / TiO2, 1% HPG1 / 3% hemin / TiO2 and 1% HPG1 / 4% EY / TiO2 samples did not change the crystal form of rutile TiO2, that is, the modified TiO2 prepared by composite is still rutile crystal form TiO2 with good photocatalytic performance.
[0146] Experimental Example 2
[0147] The adsorption rates of HPG1 / 3% hemin / TiO2 and HPG1 / 4% EY / TiO2 with different mass fractions were detected. The specific method was as follows: 0.1 g of sample powder was weighed on a balance and placed in a 50 mL beaker, 30 mL of 20 mg / L MB solution was added, and then the beaker was placed in a dark box and kept stirring evenly for 1 hour to allow the entire system to reach adsorption equilibrium. Subsequently, 3 mL of the solution was aspirated using a disposable plastic pipette while the system was kept stirring and transferred to a centrifuge tube for centrifugation for 10 minutes, and then the upper layer of powder-free solution was aspirated for absorbance test.
[0148] Results Figure 6 ,in, Figure 6 a represents the adsorption rate results of HPG1 / 3%hemin / TiO2 with different mass fractions. Figure 6 b in the figure shows the adsorption rate of HPG1 / 4%EY / TiO2 with different mass fractions. Figure 6It can be seen that when other conditions remain unchanged, the content of HPG mass fraction has a great influence on the adsorption rate of the composite photocatalyst, and the adsorption rate curve presents a parabolic shape. Specifically, the HPG1 / 3% hemin / TiO2 composite photocatalyst reaches a maximum adsorption rate of 60.4% when the HPG1 mass fraction is 2%, and the HPG1 / 4% EY / TiO2 composite photocatalyst reaches a maximum adsorption rate of 30.62% when the HPG mass fraction is 3%. When the HPG1 content is 0%, that is, the adsorption rate of pure TiO2 to MB dye is low, with the increase of HPG content, the adsorption rate of HPG1 / 3% hemin / TiO2 composite photocatalyst to MB dye increases accordingly. This is because the agglomeration phenomenon caused by HPG molecules increases the specific surface area of the composite photocatalyst, so it greatly improves the adsorption performance of the composite photocatalyst, but with the further increase of HPG content, the content of TiO2 is too low, so after the adsorption performance of the composite photosensitizer reaches the highest point, with the increase of HPG mass fraction, the adsorption performance gradually decreases.
[0149] Experimental Example 3
[0150] The adsorption rates of HPG1-hemin / TiO2, HPG2-hemin / TiO2, HPG1-EY / TiO2, and HPG3-EY / TiO2 with different mass fractions were detected. For the detection method, see Experimental Example 2.
[0151] Results Figure 7 ,in, Figure 7 a in the figure represents the adsorption rate results of HPG1-hemin / TiO2 with different mass fractions; Figure 7 b in the figure shows the adsorption rate results of HPG2-hemin / TiO2 with different mass fractions; Figure 7 c in the middle represents the adsorption rate results of HPG1-EY / TiO2 with different mass fractions; Figure 7 d in the figure shows the adsorption rate of HPG3-EY / TiO2 with different mass fractions. Figure 7It can be seen that when other conditions remain unchanged, the mass fraction of HPG has a great influence on the adsorption rate of the composite photocatalyst, and the adsorption rate curves are all parabolic. The adsorption rates of MB dye by HPG1-hemin / TiO2, HPG2-hemin / TiO2 and HPG1-EY / TiO2 are the highest when the mass fraction is 3%, and the adsorption rates are 60.3%, 55.45% and 50.72% respectively. The HPG3-EY / TiO2 composite photocatalyst reaches the highest adsorption rate of 93.12% when the mass fraction of HPG3-EY is 1%. When the polymer mass fraction is 0%, that is, the adsorption rate of pure TiO2 to MB dye is low. As the polymer content increases, the adsorption rate of the composite photocatalyst to MB dye increases accordingly. Through SEM, it can be seen that this is because the agglomeration phenomenon caused by the polymer molecules increases the specific surface area of the composite photocatalyst, so the adsorption performance of the composite photocatalyst is greatly improved. However, as the polymer content further increases, the TiO2 content is too low, and the HPG molecules have almost no adsorption capacity. Therefore, after the adsorption performance of the composite photosensitizer reaches the highest point, the adsorption performance gradually decreases with the increase of the HPG mass fraction.
[0152] Experimental Example 4
[0153] The ultraviolet photocatalytic performance of HPG1 / 3% hemin / TiO2 with different mass fractions was detected. The detection method was as follows: 0.1g sample powder was weighed on a balance and placed in a 50mL beaker, 30mL of MB solution with a concentration of 20mg / L was added, and then the beaker was placed in a dark box and kept stirring evenly for 1h to allow the whole system to reach an adsorption equilibrium state. The beaker was placed 10cm below the ultraviolet lamp tube, and the solution was kept stirring evenly. The ultraviolet lamp was turned on to allow it to undergo a photocatalytic reaction. Every 20 minutes, the dark box door was opened and 3mL of solution was aspirated using a disposable plastic straw and transferred to a 5mL centrifuge tube for centrifugation for 10 minutes. The upper layer of powder-free solution was aspirated and stored away from light. The centrifuge speed was 2000r / min. Gloves and sunglasses were worn each time sampling to avoid damage to the eyes and skin caused by ultraviolet light. When aspirating the sample, the aspiration was ensured to be uniform so that the ratio of solution to powder aspirated by the disposable plastic straw was consistent each time. After 6 samplings, the light was turned off, and the absorbance of the solution stored away from light was measured and the data was recorded.
[0154] Results Figure 8 , Figure 8By comparing the curves in the figure, it can be found that with the increase of the mass fraction of HPG1 in the HPG1 / 3% hemin / TiO2 composite photocatalyst, the photocatalytic degradation performance of the photocatalyst for MB dye shows a trend of first increasing and then decreasing. When the mass fraction of HPG is 1%, the photocatalytic performance of the HPG1 / 3% hemin / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye by the 1% HPG1 / 3% hemin / TiO2 composite photocatalyst reaches 96.37% when irradiated with ultraviolet light for 60 minutes, and the corresponding TiO2 is 32.19%, which is 2.99 times the degradation performance of the pure TiO2 photocatalyst under the same conditions. The composite of HPG and photosensitizer hemin shows a good synergistic effect on the improvement of photocatalytic performance.
[0155] Experimental Example 5
[0156] The ultraviolet light photocatalytic performance of HPG1 / 4%EY / TiO2 with different mass fractions was tested. The testing method is shown in Experimental Example 4.
[0157] Results Fig. 9 ,according to Fig. 9 It can be seen that the MB dye degradation rate of 1% HPG1 / 4% EY / TiO2 composite photocatalyst reached 97.83% when exposed to visible light for 120 minutes, and the corresponding TiO2 was 34.74%, which is 2.82 times the degradation performance of pure TiO2 photocatalyst under the same conditions.
[0158] Experimental Example 6
[0159] The ultraviolet photocatalytic performance of HPG1-EY / TiO2 of different masses was tested. The testing method is shown in Experimental Example 4.
[0160] Results Fig.10 , Fig.10By comparing the curves in the figure, it can be found that as the mass fraction of HPG1-EY in the HPG1-EY / TiO2 composite photocatalyst increases, the photocatalytic degradation performance of the photocatalyst for MB dye shows a trend of first increasing and then decreasing. Specifically, when the mass fraction of HPG1-EY is 3%, the photocatalytic performance of the HPG1-EY / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye by the 3% HPG1-EY / TiO2 composite photocatalyst reaches 56.15% when irradiated with ultraviolet light for 120 minutes, and the corresponding TiO2 is 41.26%, which is 1.36 times the degradation performance of the pure TiO2 photocatalyst under the same conditions. This is because a large number of hydroxyl groups in HPG1-EY participate in the photocatalytic reaction, and the generated hydroxyl radicals can effectively enhance the photocatalytic degradation efficiency; when the mass fraction of HPG reaches 4%, the photocatalytic performance of the HPG / TiO2 composite photocatalyst decreases, because TiO2 is a component that effectively carries out photocatalytic reactions, and its mass fraction is too low, resulting in reduced photocatalytic performance.
[0161] Experimental Example 7
[0162] The ultraviolet photocatalytic performance of HPG3-EY / TiO2 of different masses was tested. The testing method is shown in Experimental Example 4.
[0163] Results Fig.11 ,according to Fig.11 It can be seen that with the increase of the mass fraction of HPG3-EY in the HPG3-EY / TiO2 composite photocatalyst, the photocatalytic degradation performance of the photocatalyst for MB dye shows a trend of first increasing and then decreasing. When the mass fraction of HPG3-EY is 1%, the photocatalytic performance of the HPG3-EY / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye by the 1% HPG3-EY / TiO2 composite photocatalyst reaches 88.96% when irradiated with ultraviolet light for 120 minutes, and the corresponding TiO2 is 41.26%, which is 2.16 times the degradation performance of the pure TiO2 photocatalyst under the same conditions. This is because a large number of hydroxyl groups in HPG3-EY participate in the photocatalytic reaction, and the generated hydroxyl radicals can effectively enhance the photocatalytic degradation efficiency. When the mass fraction of HPG3-EY reaches 2%, the photocatalytic performance of the HPG / EY / TiO2 composite photocatalyst drops sharply. This is because TiO2 is a component that effectively carries out photocatalytic reactions, and its mass fraction is too low, resulting in reduced photocatalytic performance.
[0164] Experimental Example 8
[0165] The ultraviolet photocatalytic performance of HPG1-hemin / TiO2 of different masses was tested. The testing method is shown in Experimental Example 4.
[0166] Results Fig.12 ,according to Fig.12It can be seen that with the increase of the mass fraction of HPG1-hemin in the HPG1-hemin / TiO2 composite photocatalyst, the photocatalytic degradation performance of the photocatalyst for MB dye shows a trend of first increasing and then decreasing. When the mass fraction of HPG1-hemin is 1%, the photocatalytic performance of the HPG1-hemin / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye by the 1% HPG1-hemin / TiO2 composite photocatalyst reaches 64.32% when irradiated with ultraviolet light for 120 minutes, and the corresponding TiO2 is 41.26%, which is 1.56 times the degradation performance of the pure TiO2 photocatalyst under the same conditions. This is because a large number of hydroxyl groups in HPG1-hemin participate in the photocatalytic reaction, and the generated hydroxyl radicals can effectively enhance the photocatalytic degradation efficiency; when the mass fraction of HPG1-hemin reaches 2%, the photocatalytic performance of the HPG1-hemin / TiO2 composite photocatalyst decreases, because TiO2 is a component that effectively carries out photocatalytic reactions, and its mass fraction is too low, resulting in reduced photocatalytic performance.
[0167] Experimental Example 9
[0168] The ultraviolet photocatalytic performance of HPG2-hemin / TiO2 of different masses was tested. The testing method is shown in Experimental Example 4.
[0169] Results Fig.13 ,according to Fig.13 It can be seen that with the increase of the mass fraction of HPG2-hemin in the HPG2-hemin / TiO2 composite photocatalyst, the photocatalytic degradation performance of the photocatalyst for MB dye shows a trend of first increasing and then decreasing. When the mass fraction of HPG2-hemin is 3%, the photocatalytic performance of the HPG2-hemin / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye by the 3% HPG2-hemin / TiO2 composite photocatalyst reaches 72.17% when irradiated with ultraviolet light for 120 minutes, and the corresponding TiO2 is 41.26%, which is 1.75 times the degradation performance of the pure TiO2 photocatalyst under the same conditions. This is because a large number of hydroxyl groups in HPG2-hemin participate in the photocatalytic reaction, and the generated hydroxyl radicals can effectively enhance the photocatalytic degradation efficiency; when the mass fraction of HPG2-hemin reaches 4%, the photocatalytic performance of the HPG2-hemin / TiO2 composite photocatalyst decreases, because TiO2 is a component that effectively carries out photocatalytic reactions, and its mass fraction is too low, resulting in reduced photocatalytic performance.
[0170] Experimental Example 10
[0171] Ultraviolet light photocatalytic detection was carried out on 3% HPG1-EY / TiO2, TiO2, 2% HPG1 / 1% EY / TiO2, 3% HPG1 / TiO2, 1% HPG1-hemin / TiO2, 3% HPG2 / TiO2, 0.97% HPG1 / 0.03% hemin / TiO2, 1% HPG3-ET / TiO2, 0.6% HPG3 / 0.4% EY / TiO2, 1% HPG3 / TiO2, 3% HPG2-hemin / TiO2, 2.6% HPG3 / 0.4% hemin / TiO2, etc. For the detection method, see Experimental Example 4.
[0172] Results Fig.14 ,according to Fig.14 It can be seen that the photocatalytic efficiency of the modified titanium dioxide formed by the grafted product is greater than that of the control sample, indicating that the grafting of HPG and photosensitizer can produce a synergistic effect. The electrons and holes generated by TiO2 under ultraviolet light can be more efficiently converted into superoxide radicals and hydroxyl radicals, thereby further reducing the electron-hole (e – -h + )'s recombination rate is beneficial to the progress of the photocatalytic reaction, thereby effectively and significantly improving the photocatalytic degradation efficiency.
[0173] Experimental Example 11
[0174] The visible light photocatalytic performance of HPG1 / 3% hemin / TiO2 of different masses was tested. The testing method was as in Experimental Example 4, except that the ultraviolet light was replaced by visible light.
[0175] Results Fig.15 ,according to Fig.15It can be seen that the photocatalytic data curve of the HPG / 3% hemin / TiO2 composite photocatalyst under visible light irradiation shows a roughly similar trend to its ultraviolet light photocatalytic data curve, that is, the degradation rate of MB dye is low at the beginning of the photocatalytic reaction, and the degradation rate of MB dye gradually increases with the progress of the visible light catalytic reaction, and the increase in the photocatalytic degradation rate is large in the early stage of the photocatalytic reaction, and the increase in the photocatalytic degradation rate gradually decreases with the progress of the photocatalytic reaction. When the mass fraction of HPG1 is 1%, the photocatalytic performance of the HPG1 / 3% hemin / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye of the 1% HPG1 / 3% hemin / TiO2 composite photocatalyst reaches 88.52% when the visible light irradiation is 120 minutes, and the corresponding TiO2 is 34.74%, which is 2.55 times the degradation performance of the pure TiO2 photocatalyst under the same conditions. In summary, the effect of the mass fraction of HPG in the HPG1 / 3% hemin / TiO2 composite photocatalyst on the photocatalytic performance under ultraviolet light or visible light irradiation is basically the same, and a certain mass fraction of HPG can improve the visible light catalytic activity of the composite photocatalyst to a certain extent.
[0176] Experimental Example 12
[0177] The visible light photocatalytic performance of HPG1 / 4%EY / TiO2 of different masses was tested. The testing method is shown in Experimental Example 11.
[0178] Results Fig.16 ,according to Fig.16 It can be seen that the degradation rate of MB dye by 1% HPG1 / 4% hemin / TiO2 composite photocatalyst reached 86.26% when exposed to visible light for 120 minutes, and the corresponding TiO2 was 34.74%, which is 2.48 times the degradation performance of pure TiO2 photocatalyst under the same conditions.
[0179] Experimental Example 13
[0180] The visible light photocatalytic performance of HPG1-EY / TiO2 of different masses was tested. The testing method is shown in Experimental Example 11.
[0181] Results Fig.17 ,according to Fig.17It can be seen that the photocatalytic data curve of the HPG1-EY / TiO2 composite photocatalyst under visible light irradiation shows a roughly similar trend to its ultraviolet light photocatalytic data curve. That is, the degradation rate of MB dye is low at the beginning of the photocatalytic reaction, and as the visible light catalytic reaction proceeds, the degradation rate of MB dye gradually increases, and the increase in the photocatalytic degradation rate is large in the early stage of the photocatalytic reaction, and the increase in the photocatalytic degradation rate gradually decreases as the photocatalytic reaction proceeds; when the mass fraction of HPG1-EY is 3%, the photocatalytic performance of the HPG1-EY / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye of the 3% HPG1-EY / TiO2 composite photocatalyst reaches 41.15% when the visible light irradiation is 120 minutes, and the corresponding TiO2 is 34.74%, which is 1.18 times the degradation performance of the pure TiO2 photocatalyst under the same conditions.
[0182] In summary, the effect of the mass fraction of HPG1-EY in the HPG1-EY / TiO2 composite photocatalyst on the photocatalytic performance under ultraviolet or visible light irradiation is basically the same. A certain mass fraction of HPG1-EY can improve the visible light catalytic activity of the composite photocatalyst to a certain extent.
[0183] Experimental Example 14
[0184] The visible light photocatalytic performance of HPG3-EY / TiO2 of different masses was tested. The testing method is shown in Experimental Example 11.
[0185] Results Fig.18 ,according to Fig.18 It can be seen that the degradation rate of MB dye is low at the beginning of the photocatalytic reaction. As the visible light catalytic reaction proceeds, the degradation rate of MB dye gradually increases, and the increase in the photocatalytic degradation rate is large in the early stage of the photocatalytic reaction. The increase in the photocatalytic degradation rate gradually decreases as the photocatalytic reaction proceeds. When the mass fraction of HPG3-EY is 1%, the photocatalytic performance of the HPG3-EY / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye by the 1% HPG3-EY / TiO2 composite photocatalyst reaches 73.22% when the visible light is irradiated for 120 minutes, and the corresponding TiO2 is 34.74%, which is 2.11 times the degradation performance of the pure TiO2 photocatalyst under the same conditions.
[0186] Experimental Example 15
[0187] The visible light photocatalytic performance of HPG1-hemin / TiO2 of different masses was tested. The testing method is shown in Experimental Example 11.
[0188] Results Fig.19 ,according to Fig.19It can be seen that the degradation rate of MB dye is low in the initial stage of the photocatalytic reaction. As the visible light catalytic reaction proceeds, the degradation rate of MB dye gradually increases, and the increase in the photocatalytic degradation rate is large in the early stage of the photocatalytic reaction, and the increase in the photocatalytic degradation rate gradually decreases with the progress of the photocatalytic reaction; when the mass fraction of HPG1-hemin is 1%, the photocatalytic performance of the HPG1-hemin / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye of 1% HPG1-hemin / TiO2 composite photocatalyst reaches 42.32% when irradiated with visible light for 120 minutes, and the corresponding TiO2 is 34.74%, which is 1.22 times the degradation performance of pure TiO2 photocatalyst under the same conditions.
[0189] Experimental Example 16
[0190] The visible light photocatalytic performance of HPG, 2-hemin / TiO2 of different masses was tested. The testing method is shown in Experimental Example 11.
[0191] Results Fig. 20 ,according to Fig. 20 It can be seen that the degradation rate of MB dye is low in the initial stage of the photocatalytic reaction. As the visible light catalytic reaction proceeds, the degradation rate of MB dye gradually increases, and the increase in the photocatalytic degradation rate is large in the early stage of the photocatalytic reaction, and the increase in the photocatalytic degradation rate gradually decreases with the progress of the photocatalytic reaction; when the mass fraction of HPG2-hemin is 3%, the photocatalytic performance of the HPG2-hemin / TiO2 composite photocatalyst is the best, that is, the degradation rate of MB dye by the 3% HPG2-hemin / TiO2 composite photocatalyst reaches 63.17% when irradiated with visible light for 120 minutes, and the corresponding TiO2 is 34.74%, which is 1.82 times the degradation performance of the pure TiO2 photocatalyst under the same conditions.
[0192] Experimental Example 17
[0193] Photocatalytic cycle experiments were carried out on 1% HPG1 / 3% hemin / TiO2, 1% HPG1 / 4% EY / TiO2, 3% HPG1-EY / TiO2, 1% HPG3-EY / TiO2, 1% HPG1-hemin / TiO2 and 3% HPG2-hemin / TiO2, respectively. The method is as follows: the samples after the ultraviolet or visible light catalytic experiment reaction are recovered, washed and filtered repeatedly three times to ensure that the samples are clean, and then the ultraviolet or visible light catalytic experiment steps are repeated again, the absorbance is measured and the data is recorded. A total of four photocatalytic cycle experiments are carried out.
[0194] Results Fig.21 and Fig. 22 .in, Fig.21a in the middle represents the UV cycle experiment result of 1% HPG1 / 3% hemin / TiO2; Fig.21 b in the figure shows the UV cycle experiment result of 1% HPG1 / 4% EY / TiO2; Fig.21 Figure c shows the results of the visible light cycle experiment of 1% HPG1 / 3% hemin / TiO2; Fig.21 (d) shows the visible light cycling experimental results of 1% HPG1 / 4% EY / TiO2. Fig. 22 a in the middle represents the UV cycle experimental results of 3% HPG1-EY / TiO2; Fig. 22 b in the figure shows the UV cycle experimental results of 1% HPG3-EY / TiO2; Fig. 22 c in the middle represents the UV cycling experimental results of 1% HPG1-hemin / TiO2; Fig. 22 D in the middle shows the UV cycling experimental results of 3% HPG2-hemin / TiO2; Fig. 22 e in the middle represents the visible light cycle experimental results of 3% HPG1-EY / TiO2; Fig. 22 f in the middle represents the visible light cycle experimental results of 1% HPG3-EY / TiO2; Fig. 22 g in the middle represents the visible light cycle experimental results of 1% HPG1-hemin / TiO2; Fig. 22 h in the figure represents the visible light cycling experimental results of 3% HPG2-hemin / TiO2.
[0195] according to Fig.21 and 22 It can be seen that after four cycles of experiments, the ultraviolet and visible light catalytic properties of 1% HPG1 / 3% hemin / TiO2, 1% HPG1 / 4% EY / TiO2, 3% HPG1-EY / TiO2, 1% HPG3-EY / TiO2, 1% HPG1-hemin / TiO2 and 3% HPG2-hemin / TiO2 have basically not decreased, indicating that the modified titanium dioxide provided in the embodiments of the present invention has good stability in photocatalytic degradation reactions.
[0196] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A modified titanium dioxide photocatalyst, characterized in that: The modified titanium dioxide photocatalyst includes the photocatalyst of (1) or (2) below: (1) A photocatalyst formed by grafting polyglycidol and a photosensitizer to form a grafted product and then doping it with titanium dioxide; the content of the grafted product is 2-4% or 0.5-1%; (2) A photocatalyst formed by co-doping titanium dioxide with polyglycidol and a photosensitizer; the doping amount of the polyglycidol is 0.1-3%, and the doping amount of the photosensitizer is 3-4%; The photosensitizer is selected from hemin and eosin Y; The degree of polymerization of the polyglycidol is 123-178, and the degree of branching is 0.15-2.16; The mass fraction of the photosensitizer in the grafted product is 3-37%.
2. A method for preparing the modified titanium dioxide photocatalyst according to claim 1, characterized in that: include: Titanium dioxide was modified by polyglycidol and photosensitizer.
3. The preparation method according to claim 2, characterized in that: include: The polyglycidol and the photosensitizer are subjected to a grafting reaction to form a grafted product, and then the grafted product is mixed with a titanate compound and a hydrolysis agent to react to form titanium dioxide and the grafted product is doped with the titanium dioxide.
4. The preparation method according to claim 2, characterized in that: include: The polyglycidol, the photosensitizer titanate compound and a hydrolysis agent are mixed and reacted to form titanium dioxide and the polyglycidol and the photosensitizer are doped with the titanium dioxide.
5. The preparation method according to claim 3 or 4, characterized in that: The titanate compound includes butyl titanate, and the hydrolysis agent includes glacial acetic acid.