A hard carbon negative electrode material, negative electrode sheet and secondary battery

By using starch, aluminum salt, carbonate/phosphate and other materials in hard carbon negative electrode materials, a hierarchical porous structure is solved, and the structural instability and low sodium ion transport efficiency of hard carbon negative electrode materials in sodium ion batteries is solved. , achieving high energy density and good cycling performance.

CN116789105BActive Publication Date: 2024-11-22JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310848774.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-12
Publication Date
2024-11-22
Estimated Expiration
2043-07-12

AI Technical Summary

Technical Problem

The existing hard carbon anode materials are difficult to achieve high energy density and cyclic stability in sodium ion batteries, mainly due to their unstable structural structure and low sodium ion transmission efficiency.

Method used

By using starch as a carbon precursor, adding aluminum salt for protection, and introducing carbonate/phosphate before pre-carbonization, forming a nano-scale microporous structure, combining polymer organics to build an external porous layer, and preparing a complete structure with a Graded porous hard carbon anode material.

Benefits of technology

The initial reversible capacity and cycling performance of sodium ion batteries are significantly improved. The charge and discharge ratio of the first round is as high as 87%, and the capacity retention rate of 600 cycles can reach 85%, which improves the electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116789105B_ABST
    Figure CN116789105B_ABST
Patent Text Reader

Abstract

The present invention discloses a hard carbon negative electrode material, a negative electrode plate and a secondary battery. The preparation of the hard carbon negative electrode material comprises the following steps: (1) starch, aluminum salt and water are mixed evenly, dried to obtain a powdery mixture, and then ground and mixed evenly with carbonate and / or phosphate to obtain a carbonaceous precursor; (2) the carbonaceous precursor prepared in step (1) is pre-carbonized under an inert atmosphere to obtain a pre-carbonized product; (3) the pre-carbonized product prepared in step (2) is stirred and mixed with a polymer organic matter and a solvent, and then the mixture obtained by stirring and mixing is carbonized under an inert gas to obtain the hard carbon negative electrode material. The hard carbon negative electrode material prepared by the above preparation method has a stable structure and a hierarchical porous structure, which is beneficial to the structural stability of the material during the cycle and the transmission of sodium ions, so that the sodium ion battery containing the hard carbon negative electrode material exhibits a high initial reversible capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a hard carbon negative electrode material, a negative electrode sheet and a secondary battery. Background Art

[0002] Electrochemical power storage devices play an important role in commercial electronics and electric vehicles. Among them, lithium-ion batteries (LIBs) are the most popular devices. Nevertheless, due to the low abundance and uneven distribution of lithium resources, LIBs cannot meet the growing demand for grid-scale electrochemical energy storage. This has prompted more research to turn to more abundant and cheaper potential directions. Sodium-ion batteries have advantages over traditional lithium-ion batteries, including cost and safety.

[0003] The negative electrode material of sodium-ion batteries generally has a low reduction potential and plays an important role in loading and releasing sodium ions. Reduction reactions occur during charging and oxidation reactions occur during discharging. The efficiency of the negative electrode material directly affects the overall kinetic performance of the battery, such as rate performance, power density, etc. At present, there are usually five types of negative electrode materials: carbon-based materials, titanium-based materials, alloy materials, organic compounds and other systems. Among them, carbon-based materials have the highest technical maturity and abundant resources, and are expected to be the first to achieve industrialization. Among carbon-based negative electrode materials, hard carbon (HC) is a feasible sodium ion embedded negative electrode material. It has a disordered, stacked microcrystalline structure, presents rich sodium storage sites and a loose and suitable ion storage and transportation environment, which is not only conducive to the absorption of more Na + , and is beneficial to Na + However, the development of negative electrode materials with high energy density and cycle stability is still a difficult problem for current hard carbon negative electrode active materials. Summary of the invention

[0004] The present invention provides a hard carbon negative electrode material, a negative electrode plate and a secondary battery. Starch is used as a carbon precursor. Aluminum salt is added to protect starch particles so that the starch particles can maintain the integrity of the starch particle structure during pre-carbonization and carbonization. At the same time, carbonate / phosphate is introduced before starch pre-carbonization. A large number of nano-scale micropores can be constructed on the surface of the carbonaceous precursor after pre-carbonization treatment, thereby forming an internal porous hard carbon layer. In addition, an external porous carbon layer with relatively large pores is further formed on the outer surface by carbonization of high molecular organic matter, thereby preparing a hard carbon negative electrode material with good structural integrity and hierarchical porosity, which is beneficial to the structural stability of the material during the sodium ion insertion / extraction process and the transmission of sodium ions between negative electrode materials, so that a sodium ion battery containing the hard carbon negative electrode material exhibits high initial reversible capacity and cycle performance.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A first aspect of the present invention provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0007] (1) mixing starch, aluminum salt and water uniformly, drying to obtain a powdery mixture, and then grinding and mixing the powdery mixture prepared above with a porogen uniformly to obtain a carbonaceous precursor; the porogen is a carbonate and / or a phosphate;

[0008] (2) subjecting the carbonaceous precursor prepared in step (1) to a pre-carbonization treatment under an inert atmosphere to obtain a pre-carbonized product;

[0009] (3) The pre-carbonized product prepared in step (2) is stirred and mixed with a high molecular organic matter and a dispersant, and then the mixture obtained by stirring and mixing is carbonized under an inert gas to obtain the hard carbon negative electrode material.

[0010] Furthermore, in step (1), the starch is selected from one or more of wheat starch, corn starch, soybean starch, mung bean starch, sweet potato starch, rice starch, millet starch and potato starch.

[0011] Furthermore, in step (1), the aluminum salt is selected from one or more of potassium aluminum phosphate, sodium aluminum phosphate, potassium aluminum sulfate, sodium aluminum sulfate, a mixture of aluminum nitrate and potassium nitrate, a mixture of aluminum nitrate and sodium nitrate, sodium aluminum carbonate, and potassium aluminum carbonate.

[0012] Furthermore, in step (1), the mass ratio of the starch, the aluminum salt and the water is preferably 1-50:2-200:1000.

[0013] Furthermore, in step (1), the stirring and mixing temperature is 30-55°C.

[0014] Furthermore, in step (1), the carbonate is selected from one or more of sodium carbonate, potassium carbonate, ammonium carbonate, and ammonium bicarbonate; and the phosphate is selected from one or more of ammonium hypophosphite, ammonium hydrogen phosphate, and ammonium phosphate.

[0015] Furthermore, in step (1), the mass ratio of the powdery mixture to the porogen is 100:2-50.

[0016] Furthermore, in step (2), the temperature of the pre-carbonization treatment is preferably 200-450° C., and the time is preferably 2-8 hours; and the heating rate during the pre-carbonization treatment is preferably 1-20° C. / min.

[0017] Furthermore, the preparation method also includes a process of pickling the pre-carbonized product; the pickling can be carried out using an acid solution containing one or more of hydrogen chloride, sulfuric acid, nitric acid, carbonic acid, and formic acid, and the concentration of the acid solution is preferably 0.5-25wt%.

[0018] Furthermore, in step (3), the high molecular organic matter is selected from one or more of polybutadiene, polystyrene, polyethylene, polyethersulfone, polyetherimide, polyimide, phenolic resin, epoxy resin, polyethylene resin, and polystyrene resin.

[0019] Furthermore, in step (3), the mass ratio of the pre-carbonized product to the high molecular organic matter is preferably 1-50:2-500.

[0020] Furthermore, in step (3), the dispersant is one or more of methanol, ethanol, n-propanol, isopropanol, formic acid, and acetic acid.

[0021] Furthermore, in step (3), the mass ratio of the pre-carbonized product to the dispersant is preferably 100:0.1-50.

[0022] Furthermore, in step (3), the stirring and mixing temperature is preferably 80-300°C.

[0023] Furthermore, in step (3), the temperature of the carbonization treatment is preferably 1100-1700° C., and the time is preferably 2-20 h.

[0024] Furthermore, in step (2) and step (3), the inert gas is one or more of nitrogen, helium, neon, and argon.

[0025] A second aspect of the present invention provides a hard carbon negative electrode material, which is prepared by the above-mentioned preparation method.

[0026] Furthermore, the hard carbon negative electrode material is a core-shell structure, which consists of a hard carbon core, an internal porous hard carbon layer and an external porous carbon layer from the inside to the outside; the particle size of the hard carbon core is preferably 0.5-25μm, the thickness of the internal porous hard carbon layer is preferably 2-500nm, and the thickness of the external porous carbon layer is preferably 0.1-5μm.

[0027] A third aspect of the present invention provides a negative electrode plate, comprising the hard carbon negative electrode material described in the first aspect.

[0028] Furthermore, the negative electrode plate includes a current collector and a negative electrode active material layer coated on the surface of the current collector.

[0029] Furthermore, the negative electrode active material layer of the negative electrode plate contains the following components by mass percentage: 85-99.6% of hard carbon negative electrode material, 0.2-7% of conductive material, and 0.2-8.0% of binding material.

[0030] Furthermore, the method for preparing the negative electrode sheet comprises the following steps:

[0031] (1) weighing the hard carbon negative electrode material, the conductive material and the binding material according to the mass ratio of each component in the negative electrode active material layer of the negative electrode plate, and stirring and mixing the hard carbon negative electrode material with part of the conductive material, part of the binding material and water for the first time to obtain a primary mixture;

[0032] (2) mixing the primary mixture prepared in step (1) with the remaining conductive material, the remaining adhesive material, and water for a second time to obtain a secondary mixture, wherein the solid content of the secondary mixture is 40-60% and the viscosity is 1-9 Pa.s;

[0033] (3) The secondary mixed material prepared in step (2) is coated on the negative electrode fluid, and the negative electrode sheet is obtained by drying, cold pressing and cutting.

[0034] Furthermore, the rotation speed of the first stirring is preferably 100-3000 r / min, and the time is preferably 20-200 min; the rotation speed of the second stirring is preferably 100-3000 r / min, and the time is preferably 5 min-10 h.

[0035] Furthermore, the solid matter content in the secondary mixture is more preferably 45-55%, and the viscosity is more preferably 2-4 Pa.s.

[0036] Furthermore, the conductive material is selected from one or more of conductive carbon black, acetylene black, graphite, graphene, carbon microwires, carbon nanowires, carbon microtubes, and carbon nanotubes.

[0037] Furthermore, the bonding material is selected from one or more of polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, methacryloyl, polyacrylic acid, lithium polyacrylate, polyacrylamide, polyamide, polyimide, polyacrylate, styrene-butadiene rubber, sodium alginate, polyethylene glycol, and guar gum.

[0038] Furthermore, the negative electrode current collector is selected from one or more of aluminum foil, porous aluminum foil, foam nickel / aluminum foil, galvanized aluminum foil, nickel-plated aluminum foil, carbon-coated aluminum foil, nickel foil, and titanium foil.

[0039] A fourth aspect of the present invention provides a secondary battery comprising the hard carbon negative electrode material described in the second aspect or the negative electrode plate described in the third aspect.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1. The present invention provides a method for preparing a hard carbon negative electrode material. The hard carbon negative electrode material uses starch as a carbon precursor. When the starch is pre-carbonized at a temperature of 200 to 450° C., hydrogen bonds between molecules inside the starch granules are broken, water molecules evaporate violently, the disorder of the internal system of the starch granules increases, and the internal ordered structure gradually changes to a disordered structure. The starch granules are completely destroyed and broken. Therefore, the present invention coats and protects the starch granules by adding aluminum salts. On the one hand, aluminum combines with the generated water molecules to form an aluminum hydroxide protective layer. On the other hand, aluminum combines with the decomposed water molecules to form sodium hydrogen phosphate / potassium, sodium hydrogen sulfate / potassium, sodium hydrogen carbonate / potassium and other substances, which can form a water-absorbing layer to prevent the water molecules from evaporating violently and decomposing violently. The formed aluminum hydroxide protective layer and water-absorbing layer can encapsulate the starch granules and provide structural support, so that the starch granules can be pre-carbonized. The carbonization process can maintain the integrity of the starch granule structure; in addition, the present invention introduces carbonate / phosphate before starch pre-carbonization, and the carbonate / phosphate gradually releases the internal gaseous molecules during the pre-carbonization process and is evenly dispersed on the surface of the carbonaceous precursor, constructing a large number of nano-scale micropores, and performing internal porous carbon layer differentiation. The carbonized pre-carbonization product can maintain sufficient stability during the subsequent high-temperature carbonization process; in addition, by further introducing high-molecular organic matter, an external porous carbon layer with relatively large pores is formed on the outer surface of the negative electrode material after carbonization, thereby preparing a hard carbon negative electrode material with good structural integrity and hierarchical porosity, which is beneficial to the structural stability of the material during the sodium ion insertion / extraction process and the transmission of sodium ions between the negative electrode materials, so that the sodium ion battery containing the hard carbon negative electrode material exhibits high initial reversible capacity and cycle performance.

[0042] 2. The present invention uses the above-mentioned hard carbon negative electrode material with a hierarchical porous structure to construct different sodium ion batteries, and the prepared secondary batteries show a high first-cycle charge and discharge ratio and good cycle performance, and the high first-cycle charge and discharge ratio can be as high as 87% or more; the button battery prepared with the above-mentioned hard carbon negative electrode material as the negative electrode active material has an initial reversible capacity of not less than 322mAh / g, and the capacity retention rate after 600 cycles can be as high as 85%, also showing excellent cycle performance; and from the performance of the sodium ion battery containing the hard carbon negative electrode material prepared by different preparation methods, it can be seen that the aluminum salt protective layer and the hierarchical porous structure are beneficial to the improvement of the battery capacity, initial coulomb efficiency and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 Schematic diagram of the structure of hard carbon negative electrode material, where ① is the hard carbon core, ② is the internal porous hard carbon layer, and ③ is the external porous carbon layer. DETAILED DESCRIPTION

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. The term "includes" or "comprising" described in the present invention means that it may include or contain other components in addition to the components described. The term "includes" or "comprising" described in the present invention may also be replaced by the closed form "for" or "consisting of..."

[0045] As described in the background technology, sodium ion negative electrode materials are an important component of sodium ion batteries. Hard carbon is a feasible sodium ion embedded negative electrode material. Currently, the development of negative electrode materials with high energy density and cycle stability is still a difficulty in current hard carbon negative electrode active materials.

[0046] In order to solve the above technical problems, the embodiment of the present invention provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0047] (1) Mixing starch, aluminum salt and water, drying to obtain a powdery mixture, and then grinding and mixing the powdery mixture prepared above with a porogen to obtain a carbonaceous precursor; the porogen is a carbonate and / or a phosphate;

[0048] (2) subjecting the carbonaceous precursor prepared in step (1) to a pre-carbonization treatment under an inert atmosphere to obtain a pre-carbonized product;

[0049] (3) The pre-carbonized product prepared in step (2) is stirred and mixed with a high molecular organic matter and a dispersant, and then the mixture obtained by stirring and mixing is carbonized under an inert gas to obtain the hard carbon negative electrode material.

[0050] In some preferred embodiments of the present invention, the starch can be selected from one or more of wheat starch, corn starch, soybean starch, mung bean starch, sweet potato starch, rice starch, millet starch and potato starch; the aluminum salt can be selected from one or more of potassium aluminum phosphate, sodium aluminum phosphate, potassium aluminum sulfate, sodium aluminum sulfate, a mixture of aluminum nitrate and potassium nitrate, a mixture of aluminum nitrate and sodium nitrate, sodium aluminum carbonate and potassium aluminum carbonate; wherein the mass ratio of starch, aluminum salt and water is preferably 1-50:2-200:1000, for example 25:50:1000, 50:125:1000, etc.; more specifically, the present invention stirs and mixes the starch, aluminum salt and water at 30-55°C.

[0051] The present invention introduces aluminum salt before pre-carbonizing starch. When the starch is pre-carbonized at a temperature of 200-450° C., hydrogen bonds between molecules in starch granules are broken, water molecules evaporate violently, the disorder of the internal system of starch granules increases, and the internal ordered structure gradually changes into a disordered structure. The starch granules are completely destroyed and broken. Therefore, the present invention coats and protects the starch granules by adding aluminum salt. On the one hand, aluminum combines with the generated water molecules to form an aluminum hydroxide protective layer. On the other hand, aluminum combines with the decomposed water molecules to form sodium hydrogen phosphate / potassium, sodium hydrogen sulfate / potassium, sodium hydrogen carbonate / potassium and other substances, which can form a water absorption layer to prevent the water molecules from evaporating violently and decomposing violently. The formed aluminum hydroxide protective layer and water absorption layer can encapsulate the starch granules and provide structural support, so that the starch granules can maintain the integrity of the starch granule structure during the pre-carbonization and carbonization processes.

[0052] In some preferred embodiments of the present invention, the carbonate may be selected from one or more of sodium carbonate, potassium carbonate, ammonium carbonate, and ammonium bicarbonate; the phosphate may be selected from one or more of ammonium hypophosphite, ammonium hydrogen phosphate, and ammonium phosphate; wherein the mass ratio of the powdery mixture to the porogen is 100:2-50, for example, 100:2, 100:3, 100:5, 100:8, 100:10, 100:15, 100:20, 100:25, 100:30, 100:35, 100:40, 100:45, 100:50, etc., including but not limited to the mass ratios listed above.

[0053] The present invention introduces carbonate / phosphate as a pore regulator to regulate the pore structure of the carbonaceous precursor. During the pre-carbonization process, the carbonate / phosphate gradually releases the gaseous molecules inside and disperses evenly on the surface of the carbonaceous precursor, constructing a large number of nano-scale micropores and performing porous carbon layer differentiation. The carbonized pores can maintain sufficient stability during the subsequent high-temperature carbonization process.

[0054] In some preferred embodiments of the present invention, the temperature of the pre-carbonization treatment is preferably 200-450°C, for example 200°C, 230°C, 250°C, 280°C, 300°C, 320°C, 350°C, 380°C, 400°C, 420°C, 450°C, etc., including but not limited to the pre-carbonization treatment temperatures listed above, and the time is preferably 2-8h, for example 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc., including but not limited to the pre-carbonization treatment time listed above; in addition, the heating rate during the pre-carbonization treatment is preferably 1-20°C / min, which can be 2°C / min, 4°C / min, 6°C / min, 8°C / min, 10°C / min, 12°C / min, 14°C / min, 16°C / min, 18°C / min, 20°C / min, etc.

[0055] In some preferred embodiments of the present invention, the above-mentioned preparation method also includes a process of pickling the pre-carbonized product to remove aluminum-containing impurities; wherein the pickling can use an acid solution containing one or more of hydrogen chloride, sulfuric acid, nitric acid, carbonic acid, and formic acid, and the concentration of the acid solution is preferably 0.5-25wt%.

[0056] In some preferred embodiments of the present invention, the above-mentioned high molecular organic matter is selected from one or more of polybutadiene, polystyrene, polyethylene, polyethersulfone, polyetherimide, polyimide, phenolic resin, epoxy resin, polyethylene resin, and polystyrene resin; wherein the mass ratio of the pre-carbonized product to the high molecular organic matter is preferably 1-50:2-500, more preferably 1:5-20, for example 1:2, 1:5, 1:8, 1:10, 1:12, 1:15, 1:20, etc.

[0057] The present invention further introduces high molecular weight organic matter to form an external porous carbon layer with relatively large pores on the outer surface of the negative electrode material after carbonization, which is beneficial to the sodium ion transmission between the hard carbon negative electrode materials and improves the cycle performance of the material.

[0058] In some preferred embodiments of the present invention, the above-mentioned dispersant is one or more of methanol, ethanol, n-propanol, isopropanol, formic acid, and acetic acid, wherein the mass ratio of the pre-carbonized product to the dispersant is preferably 100:0.1-50, such as 100:5, 100:10, 100:15, 100:20, 100:25, 100:30, 100:35, 100:40, 100:45, 100:50, etc., including but not limited to the mass ratios listed above. More specifically, the temperature for stirring and mixing the above-mentioned pre-carbonized product with the high molecular organic matter and the dispersant is preferably 80-300°C, such as 80°C, 90°C, 100°C, 120°C, 150°C, 180°C, 200°C, 230°C, 250°C, 280°C, 300°C, etc., including but not limited to the temperatures listed above.

[0059] In some preferred embodiments of the present invention, the temperature of the carbonization treatment is preferably 1100-1700°C, for example, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, etc., and the time is preferably 2-20h, for example, 3h, 4h, 5h, 6h, 7h, 8h, 10h, 12h, 13h, 15h, 17h, 18h, etc., including but not limited to the carbonization treatment time listed above.

[0060] In some preferred embodiments of the present invention, the inert gas introduced during the pre-carbonization and carbonization processes is one or more of nitrogen, helium, neon, and argon.

[0061] In addition, the embodiments of the present invention also provide a hard carbon negative electrode material, which is prepared by the above preparation method.

[0062] In some preferred embodiments of the present invention, the above-mentioned hard carbon negative electrode material is a core-shell structure, which consists of a hard carbon core, an internal porous hard carbon layer and an external porous carbon layer from the inside to the outside; wherein, the particle size of the hard carbon core is preferably 0.5-25μm, the thickness of the internal porous hard carbon layer is preferably 2-500nm, and the thickness of the external porous carbon layer is preferably 0.1-5μm.

[0063] The embodiments of the present invention also provide a negative electrode plate, comprising the hard carbon negative electrode material described in the second aspect.

[0064] In some preferred embodiments of the present invention, the above-mentioned negative electrode plate includes a current collector and a negative electrode active material layer coated on the surface of the current collector, wherein the negative electrode active material layer of the negative electrode plate contains the following components in mass percentage: 85-99.6% of hard carbon negative electrode material, 0.2-7% of conductive material, and 0.2-8.0% of binding material.

[0065] In some preferred embodiments of the present invention, the above-mentioned negative electrode current collector is selected from one or more of aluminum foil, porous aluminum foil, foam nickel / aluminum foil, galvanized aluminum foil, nickel-plated aluminum foil, carbon-coated aluminum foil, nickel foil, and titanium foil; the conductive material is selected from one or more of conductive carbon black, acetylene black, graphite, graphene, carbon microwires, carbon nanowires, carbon microtubes, and carbon nanotubes; the binding material is selected from one or more of polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, methacryloyl, polyacrylic acid, lithium polyacrylate, polyacrylamide, polyamide, polyimide, polyacrylate, styrene-butadiene rubber, sodium alginate, polyethylene glycol, and guar gum.

[0066] In some preferred embodiments of the present invention, the method for preparing the negative electrode sheet comprises the following steps:

[0067] (1) weighing the hard carbon negative electrode material, the conductive material and the binding material according to the mass ratio of each component in the negative electrode active material layer of the negative electrode plate, and stirring and mixing the hard carbon negative electrode material with part of the conductive material, part of the binding material and water for the first time to obtain a primary mixture;

[0068] (2) mixing the primary mixture prepared in step (1) with the remaining conductive material, the remaining adhesive material, and water for a second time to obtain a secondary mixture, wherein the solid content of the secondary mixture is 40-60% and the viscosity is 1-9 Pa.s;

[0069] (3) The secondary mixed material prepared in step (2) is coated on the negative electrode fluid, and the negative electrode sheet is obtained by drying, cold pressing and cutting.

[0070] In some preferred embodiments of the present invention, the rotation speed of the first stirring is preferably 100-3000 r / min, and the time is preferably 20-200 min; the rotation speed of the second stirring is preferably 100-3000 r / min, and the time is preferably 5 min-10 h.

[0071] In some preferred embodiments of the present invention, the solid matter content in the secondary mixture is more preferably 45-55%, and the viscosity is more preferably 2-4 Pa.s.

[0072] The embodiments of the present invention provide a secondary battery comprising the hard carbon negative electrode material or negative electrode sheet.

[0073] In some preferred embodiments of the present invention, the above-mentioned secondary battery comprises a positive electrode plate, a negative electrode plate, a separator and an electrolyte; wherein the positive electrode active material in the positive electrode plate may be one or more of sodium nickel manganate, sodium nickel cobalt manganate, sodium nickel cobalt aluminum, sodium vanadium fluorophosphate, sodium ferromanganese fluorophosphate, sodium nickel ferromanganate, sodium nickel copper manganate, sodium nickel copper manganese ferrate, sodium hexacyanoferrate, sodium hexacyanomanganate, sodium hexacyanonicnickelate, sodium hexacyanoferrate nickelate, sodium hexacyanoferrate manganate, sodium hexacyanoferrate manganate, sodium titanium phosphate, and sodium titanium manganese phosphate; the isolation membrane may be a polymer organic membrane of at least one of polyethylene, polypropylene, polysulfonyl, polyacrylonitrile, polyvinyl alcohol, polyarylethersulfone, polyvinylidene fluoride, and polymalonic acid.

[0074] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0075] Example 1

[0076] This embodiment relates to the preparation of a hard carbon negative electrode material and a negative electrode sheet, wherein:

[0077] The specific operations for preparing hard carbon negative electrode materials are as follows:

[0078] (1) corn starch, sodium aluminum phosphate, and water are mixed in a mass ratio of 25:50:1000, and then the mixture is stirred at 45° C. Subsequently, the obtained mixture is filtered, washed with ethanol several times, and dried at 55° C. to obtain a powdery mixture. The powdery mixture and sodium carbonate are ground and mixed in a mass ratio of 100:3 to form a uniform carbonaceous precursor;

[0079] (2) placing the carbonaceous precursor in a heating furnace and pre-carbonizing it under nitrogen gas at 230°C for 4 hours at a heating rate of 4°C / min. Washing it with a low-concentration acid solution (16.3 wt% hydrogen chloride) and water for multiple times to obtain a pre-carbonized product;

[0080] (3) Phenolic resin and liquid containing pre-carbonized product (obtained by mixing pre-carbonized product and ethanol in a ratio of 100:15) were added to a blender in sequence, the mass ratio of pre-carbonized product to phenolic resin being 1:8, and the mixture was stirred and mixed at 120°C to fully mix the phenolic resin and pre-carbonized product; the mixture was then sent to a heating furnace, nitrogen gas was introduced to expel the air inside, the temperature was raised to 1450°C at a heating rate of 5°C / min, a carbonization treatment was performed for 5 hours, and the carbonized product was then crushed and screened to obtain a graded porous hard carbon negative electrode material.

[0081] The specific operations for preparing the negative electrode sheet are as follows:

[0082] 94.5 parts of hard carbon negative electrode material, 1.0 part of conductive material (conductive carbon black and carbon nanotubes are mixed in a mass ratio of 19:1), 1.75 parts of binding material (sodium carboxymethyl cellulose and polyacrylic acid are mixed in a mass ratio of 1:2), and water are placed in a stirring pot of a mixer, and dry-mixed and stirred at a speed of 1500 r / min for 100 minutes to obtain a primary mixture;

[0083] Add 1.0 part of the above conductive material, 1.75 parts of the above bonding material and water to the primary mixture, stir at a speed of 2500 r / min for 2 hours, then add water until the solid content in the stirring pot is 51%, and adjust the viscosity to 2.6 Pa.s to obtain a secondary mixture;

[0084] The secondary mixed material is coated on the carbon-coated aluminum foil negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet;

[0085] The mass ratio of the hard carbon negative electrode material to the conductive material and the bonding material in the negative electrode sheet prepared in this embodiment is 94.5:2.0:3.5.

[0086] Example 2

[0087] This embodiment relates to the preparation of a hard carbon negative electrode material and a negative electrode sheet, wherein:

[0088] The specific operations for preparing hard carbon negative electrode materials are as follows:

[0089] (1) corn starch, sodium aluminum phosphate, and water were mixed in a mass ratio of 25:50:1000, and then stirred at 45°C. Subsequently, the obtained mixture was filtered, washed with ethanol several times, and dried at 55°C to obtain a powder mixture. The powder mixture and sodium carbonate were ground and mixed in a mass ratio of 100:3 to form a uniform carbonaceous precursor;

[0090] (2) placing the carbonaceous precursor in a heating furnace and pre-carbonizing it under nitrogen gas at 230°C for 4 hours at a heating rate of 4°C / min. Washing it with a low-concentration acid solution (16.3 wt% hydrogen chloride) and water for multiple times to obtain a pre-carbonized product;

[0091] (3) Phenolic resin and liquid containing pre-carbonized product (obtained by mixing pre-carbonized product and ethanol in a ratio of 100:15) were added to a blender in sequence, the mass ratio of pre-carbonized product to phenolic resin being 1:12, and the mixture was stirred and mixed at 230°C to fully mix the phenolic resin and pre-carbonized product; the mixture was then sent to a heating furnace, nitrogen gas was introduced to expel the air inside, the temperature was raised to 1450°C at a heating rate of 5°C / min, a carbonization treatment was performed for 5 hours, and the carbonized product was then crushed and screened to obtain a graded porous hard carbon negative electrode material.

[0092] The specific operations for preparing the negative electrode sheet are as follows:

[0093] 94.5 parts of hard carbon negative electrode material, 1.0 part of conductive material (conductive carbon black and carbon nanotubes are mixed in a mass ratio of 19:1), 1.75 parts of binding material (sodium carboxymethyl cellulose and polyacrylic acid are mixed in a mass ratio of 1:2), and water are placed in a stirring pot of a mixer, and dry-mixed and stirred at a speed of 1500 r / min for 100 minutes to obtain a primary mixture;

[0094] Add 1.0 part of the conductive material, 1.75 parts of the adhesive and water to the primary mixture, stir at 2500 r / min for 2 hours, then add water until the solid content in the stirring pot is 49%, and adjust the viscosity to 3.1 Pa.s to obtain a secondary mixture;

[0095] The secondary mixed material is coated on the carbon-coated aluminum foil negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet;

[0096] The mass ratio of the hard carbon negative electrode material to the conductive material and the bonding material in the negative electrode sheet prepared in this embodiment is 94.5:2.0:3.5.

[0097] Example 3

[0098] This embodiment relates to the preparation of a hard carbon negative electrode material and a negative electrode sheet, wherein:

[0099] The specific operations for preparing hard carbon negative electrode materials are as follows:

[0100] (1) corn starch, sodium aluminum phosphate, and water were mixed in a mass ratio of 25:50:1000, and then stirred at 45°C. Subsequently, the obtained mixture was filtered, washed with ethanol several times, and dried at 55°C to obtain a powder mixture. The powder mixture and sodium carbonate were ground and mixed in a mass ratio of 100:3 to form a uniform carbonaceous precursor;

[0101] (2) placing the carbonaceous precursor in a heating furnace and pre-carbonizing it under nitrogen gas at 230°C for 4 hours at a heating rate of 4°C / min. Washing it with a low-concentration acid solution (16.3 wt% hydrogen chloride) and water for multiple times to obtain a pre-carbonized product;

[0102] (3) Phenolic resin and liquid containing pre-carbonized product (obtained by mixing pre-carbonized product and ethanol at a ratio of 100:15) were added to a blender in sequence, with the mass ratio of pre-carbonized product to phenolic resin being 1:15. The mixture was stirred and mixed at 120°C to fully mix the phenolic resin and pre-carbonized product. The mixture was then sent to a heating furnace, nitrogen gas was introduced to expel the air inside, the temperature was raised to 1450°C at a heating rate of 5°C / min, and carbonization treatment was performed for 5 hours. The carbonized product was then crushed and screened to obtain a graded porous hard carbon negative electrode material.

[0103] The specific operations for preparing the negative electrode sheet are as follows:

[0104] 94.5 parts of hard carbon negative electrode material, 1.0 part of conductive material (conductive carbon black and carbon nanotubes are mixed in a mass ratio of 19:1), 1.75 parts of binding material (sodium carboxymethyl cellulose and polyacrylic acid are mixed in a mass ratio of 1:2), and water are placed in a stirring pot of a mixer, and dry-mixed and stirred at a speed of 1500 r / min for 100 minutes to obtain a primary mixture;

[0105] Add 1.0 part of the conductive material, 1.75 parts of the adhesive and water to the primary mixture, stir at 2500 r / min for 2 hours, then add water until the solid content in the stirring pot is 48%, and adjust the viscosity to 2.3 Pa.s to obtain a secondary mixture;

[0106] The secondary mixed material is coated on the carbon-coated aluminum foil negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet;

[0107] The mass ratio of the hard carbon negative electrode material to the conductive material and the bonding material in the negative electrode sheet prepared in this embodiment is 94.5:2.0:3.5.

[0108] Example 4

[0109] This embodiment relates to the preparation of a hard carbon negative electrode material and a negative electrode sheet, wherein:

[0110] The specific operations for preparing hard carbon negative electrode materials are as follows:

[0111] (1) corn starch, sodium aluminum phosphate, and water were mixed in a mass ratio of 50:125:1000, and then stirred at 50°C. Subsequently, the obtained mixture was filtered, washed with ethanol several times, and dried at 55°C to obtain a powder mixture. The powder mixture and sodium carbonate were ground and mixed in a mass ratio of 100:5 to form a uniform carbonaceous precursor;

[0112] (2) placing the carbonaceous precursor in a heating furnace and pre-carbonizing it under nitrogen gas at 280°C for 4 hours at a heating rate of 4°C / min. Washing it with a low-concentration acid solution (16.3 wt% hydrogen chloride) and water for multiple times to obtain a pre-carbonized product;

[0113] (3) Phenolic resin and liquid containing pre-carbonized product (obtained by mixing pre-carbonized product and ethanol in a ratio of 100:25) were added to a blender in sequence, the mass ratio of pre-carbonized product to phenolic resin being 1:8, and the mixture was stirred at 120°C to fully mix the phenolic resin and pre-carbonized product; the mixture was then sent to a heating furnace, nitrogen gas was introduced to expel the air inside, the temperature was raised to 1300°C at a heating rate of 5°C / min, carbonization treatment was performed for 6 hours, and the carbonized product was then crushed and screened to obtain a graded porous hard carbon negative electrode material.

[0114] The specific operations for preparing the negative electrode sheet are as follows:

[0115] 95.0 parts of hard carbon negative electrode material, 0.875 parts of conductive material (conductive carbon black and carbon nanotubes are mixed in a mass ratio of 19:1), 1.625 parts of binding material (sodium carboxymethyl cellulose and polyacrylic acid are mixed in a mass ratio of 1:2), and water are placed in a stirring pot of a stirrer, and dry-mixed and stirred at a speed of 1500 r / min for 90 minutes to obtain a primary mixture;

[0116] Add 0.875 parts of the conductive material, 1.625 parts of the adhesive and water to the primary mixture, stir at 3000 r / min for 90 min, then add water until the solid content in the stirring pot is 51%, and adjust the viscosity to 3.7 Pa.s to obtain a secondary mixture;

[0117] The secondary mixed material is coated on the carbon-coated aluminum foil negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet;

[0118] The mass ratio of the hard carbon negative electrode material to the conductive material and the bonding material in the negative electrode sheet prepared in this embodiment is 95.0:1.75:3.25.

[0119] Example 5

[0120] This embodiment relates to the preparation of a hard carbon negative electrode material and a negative electrode sheet, wherein:

[0121] The specific operations for preparing hard carbon negative electrode materials are as follows:

[0122] (1) corn starch, sodium aluminum phosphate, and water were mixed in a mass ratio of 50:125:1000, and then stirred at 50°C. Subsequently, the obtained mixture was filtered, washed with ethanol several times, and dried at 55°C to obtain a powder mixture. The powder mixture and sodium carbonate were ground and mixed in a mass ratio of 100:5 to form a uniform carbonaceous precursor;

[0123] (2) placing the carbonaceous precursor in a heating furnace and pre-carbonizing it under nitrogen gas at 280°C for 4 hours at a heating rate of 4°C / min. Washing it with a low-concentration acid solution (16.3 wt% hydrogen chloride) and water for multiple times to obtain a pre-carbonized product;

[0124] (3) Phenolic resin and liquid containing pre-carbonized product (obtained by mixing pre-carbonized product and ethanol at a ratio of 100:30) were added to a blender in sequence, with a mass ratio of pre-carbonized product to phenolic resin of 1:10. The mixture was stirred at 120°C to fully mix the phenolic resin and pre-carbonized product. The mixture was then sent to a heating furnace, nitrogen gas was introduced to expel the air inside, the temperature was raised to 1300°C at a heating rate of 5°C / min, and carbonization treatment was performed for 6 hours. The carbonized product was then crushed and screened to obtain a graded porous hard carbon negative electrode material.

[0125] The specific operations for preparing the negative electrode sheet are as follows:

[0126] 95.0 parts of hard carbon negative electrode material, 0.875 parts of conductive material (conductive carbon black and carbon nanotubes are mixed in a mass ratio of 19:1), 1.625 parts of binding material (sodium carboxymethyl cellulose and polyacrylic acid are mixed in a mass ratio of 1:2), and water are placed in a stirring pot of a stirrer, and dry-mixed and stirred at a speed of 1800 r / min for 100 minutes to obtain a primary mixture;

[0127] Add 0.875 parts of the conductive material, 1.625 parts of the adhesive and water to the primary mixture, stir at 3000 r / min for 100 min, then add water until the solid content in the stirring pot is 52%, and adjust the viscosity to 3.8 Pa.s to obtain a secondary mixture;

[0128] The secondary mixed material is coated on the carbon-coated aluminum foil negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet;

[0129] The mass ratio of the hard carbon negative electrode material to the conductive material and the bonding material in the negative electrode sheet prepared in this embodiment is 95.0:1.75:3.25.

[0130] Example 6

[0131] This embodiment relates to the preparation of a hard carbon negative electrode material and a negative electrode sheet, wherein:

[0132] The specific operations for preparing hard carbon negative electrode materials are as follows:

[0133] (1) corn starch, sodium aluminum phosphate, and water were mixed in a mass ratio of 50:125:1000, and then stirred at 50°C. Subsequently, the obtained mixture was filtered, washed with ethanol several times, and dried at 55°C to obtain a powder mixture. The powder mixture and sodium carbonate were ground and mixed in a mass ratio of 100:5 to form a uniform carbonaceous precursor;

[0134] (2) placing the carbonaceous precursor in a heating furnace and pre-carbonizing it under nitrogen gas at 280°C for 4 hours at a heating rate of 4°C / min. Washing it with a low-concentration acid solution (16.3 wt% hydrogen chloride) and water for multiple times to obtain a pre-carbonized product;

[0135] (3) Phenolic resin and liquid containing pre-carbonized product (obtained by mixing pre-carbonized product and ethanol at a ratio of 100:50) were added to a blender in sequence, with a mass ratio of pre-carbonized product to phenolic resin of 1:15. The mixture was stirred and mixed at 120°C to fully mix the phenolic resin and pre-carbonized product. The mixture was then sent to a heating furnace, nitrogen gas was introduced to remove the air inside, the temperature was raised to 1300°C at a heating rate of 5°C / min, and carbonization treatment was performed for 6 hours. The carbonized product was then crushed and screened to obtain a graded porous hard carbon negative electrode material.

[0136] The specific operations for preparing the negative electrode sheet are as follows:

[0137] 95.0 parts of hard carbon negative electrode material, 0.875 parts of conductive material (conductive carbon black and carbon nanotubes are mixed in a mass ratio of 19:1), 1.625 parts of binding material (sodium carboxymethyl cellulose and polyacrylic acid are mixed in a mass ratio of 1:2), and water are placed in a stirring pot of a stirrer, and dry-mixed and stirred at a speed of 1800 r / min for 100 minutes to obtain a primary mixture;

[0138] Add 0.875 parts of the conductive material, 1.625 parts of the adhesive and water to the primary mixture, stir at 3000 r / min for 100 min, then add water until the solid content in the stirring pot is 53%, and adjust the viscosity to 4.3 Pa.s to obtain a secondary mixture;

[0139] The secondary mixed material is coated on the carbon-coated aluminum foil negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet;

[0140] The mass ratio of the hard carbon negative electrode material to the conductive material and the bonding material in the negative electrode sheet prepared in this embodiment is 95.0:1.75:3.25.

[0141] Comparative Example 1

[0142] This comparative example involves the preparation of a hard carbon negative electrode material and a negative electrode plate, and the only difference from Example 1 is that no sodium aluminum phosphate is added in the preparation of the hard carbon negative electrode material.

[0143] Comparative Example 2

[0144] This comparative example involves the preparation of a hard carbon negative electrode material and a negative electrode plate, and the only difference from Example 1 is that no sodium carbonate is added in the preparation of the hard carbon negative electrode material.

[0145] Comparative Example 3

[0146] This comparative example involves the preparation of a hard carbon negative electrode material and a negative electrode plate, and the only difference from Example 1 is that no phenolic resin is added in the preparation of the hard carbon negative electrode material.

[0147] Application and performance testing

[0148] The negative electrode material prepared in the above embodiment and comparative example is used as the negative electrode active material to prepare the negative electrode plate, and the sodium ion secondary battery and button battery are assembled. The specific preparation process is as follows:

[0149] Assembly of sodium-ion secondary batteries:

[0150] Positive electrode sheet: Sodium nickel copper manganate is mixed with a conductive agent (conductive carbon black and carbon nanotubes are mixed in a mass ratio of 19:1) and a PVDF adhesive material in a mass ratio of 97.5:1.5:1, mixed with NMP as a solvent and then coated on a carbon-coated current collector, and dried, rolled, cut and stripped to obtain a positive electrode sheet;

[0151] Diaphragm: Polyethylene separator;

[0152] Electrolyte: NaClO4 dissolved in solvent EC&DMC (volume ratio 1:1), NaClO4 concentration is 1M;

[0153] The positive electrode sheet, separator and negative electrode sheet are stacked and wound in sequence to obtain a bare cell, and the tabs are ultrasonically welded. The bare cell is placed in a battery shell, dried at 160° C. to remove moisture, and an electrolyte is injected into the battery shell and packaged to obtain a secondary battery.

[0154] Button battery assembly:

[0155] The negative electrode sheets of each embodiment and comparative example were punched into discs with a diameter of 12 mm, a metal sodium sheet was used as a counter electrode, a polypropylene film was used as an isolation membrane, and the electrolyte was prepared by dissolving NaClO4 in a solvent EC&DMC (volume ratio 1:1) with a concentration of 1M; button batteries were assembled in a glove box.

[0156] (1) Performance test of secondary batteries: first perform formation and constant capacity, and record the ratio of the battery's formation and constant capacity first cycle charge and discharge; then charge at 0.2C to 3.9V, charge at 3.9V constant voltage until the current decreases to 0.05C, discharge at 0.33C to 2.0V, then charge at 0.2C to 3.9V, charge at 3.9V constant voltage until the current decreases to 0.05C, and cycle the battery in this way, record the battery's charge and discharge at 100 cycles, 300 cycles, the percentage of the capacity to the first cycle, and the number of cycles corresponding to the capacity percentage decaying to 80%, to evaluate the battery's electrochemical performance.

[0157] (2) Performance test of button cell: The button cell is subjected to a discharge / charge test at 0 to 2.0 V to test the initial charge capacity of the button cell, i.e., the initial reversible capacity.

[0158] The results of the performance test of the above secondary battery are shown in Table 1 below:

[0159] Table 1

[0160]

[0161] It can be seen from the above table that the sodium ion secondary batteries containing the negative electrode materials prepared by Examples 1-5 all have a relatively high first-cycle charge and discharge ratio (not less than 87%) and better cycle stability, and as the number of cycles increases, the advantage of the cycle performance is more obvious, and the number of cycles corresponding to the capacity dropping to 80% of the initial capacity is not less than 440 cycles, and the secondary battery constructed with the negative electrode sheet prepared in Example 1 has a corresponding number of cycles when the capacity drops to 80% of the initial capacity is 545 cycles, which is much higher than Comparative Examples 1-3.

[0162] Compared with Example 1, Comparative Example 1 did not add sodium aluminum phosphate during the preparation of the hard carbon negative electrode material, and the cycle stability was relatively poor. It is speculated that this is due to the structural rupture of starch particles during the pre-carbonization and carbonization processes. As the negative electrode active material, the negative electrode active material particles have poor structural stability during the battery's cyclic charge and discharge process, thereby affecting the battery's cycle performance. In addition, Comparative Example 2 did not add sodium carbonate during the preparation of the hard carbon negative electrode material, and Comparative Example 3 did not add high molecular organic matter during the preparation of the hard carbon negative electrode material. The secondary battery prepared with the hard carbon negative electrode materials prepared in Comparative Examples 2 and 3 as the negative electrode active material has a relatively low first cycle charge and discharge ratio (less than 85%), and the cycle performance is inferior to that of Example 1, which also shows that the formation of a hierarchical porous structure is conducive to improving the electrochemical performance of the battery.

[0163] The results of the performance test of the button cell are shown in Table 2 below:

[0164] Table 2

[0165]

[0166] It can be seen from the above table that, similar to the performance of the above-mentioned secondary batteries, the sodium ion button batteries containing the negative electrode materials prepared by Examples 1-5 all have relatively high initial reversible capacities (the initial reversible capacity of the button battery constructed with the negative electrode sheet prepared in Example 5 can be as high as 326.7 mAh / g).

[0167] It can be seen from Example 1 and Comparative Examples 1-3 that, compared with Example 1, during the preparation of the negative electrode material, the button battery constructed with the negative electrode material prepared without adding sodium aluminum phosphate, sodium carbonate or phenolic resin has a relatively low initial reversible capacity, which further illustrates that the formation of the protective layer and the graded porous structure are beneficial to improving the electrochemical properties of the negative electrode material.

[0168] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a hard carbon negative electrode material, characterized in that: The following steps are involved: (1) Mix starch, aluminum salt and water and dry them to obtain a powder mixture, then grind and mix the powder mixture prepared above with a porogen to obtain a carbonaceous precursor; the porogen is carbonate and / or phosphate; the mass ratio of starch, aluminum salt and water is 1-50:2-200:1000; (2) subjecting the carbonaceous precursor prepared in step (1) to a pre-carbonization treatment under an inert atmosphere to obtain a pre-carbonized product; (3) The pre-carbonized product prepared in step (2) is stirred and mixed with a high molecular weight organic matter and a dispersant, and then the mixture obtained by stirring and mixing is carbonized under an inert gas to obtain the hard carbon negative electrode material.

2. The preparation method according to claim 1, characterized in that: In step (1), the starch is selected from one or more of wheat starch, corn starch, soybean starch, mung bean starch, sweet potato starch, rice starch, millet starch, and potato starch; The aluminum salt is selected from one or more of potassium aluminum phosphate, sodium aluminum phosphate, potassium aluminum sulfate, sodium aluminum sulfate, mixture 1, mixture 2, sodium aluminum carbonate, and potassium aluminum carbonate. The mixture 1 is a mixture of aluminum nitrate and potassium nitrate, and the mixture 2 is a mixture of aluminum nitrate and sodium nitrate.

3. The preparation method according to claim 1, characterized in that: In step (1), the carbonate is selected from one or more of sodium carbonate, potassium carbonate, ammonium carbonate, and ammonium bicarbonate; the phosphate is selected from one or more of ammonium hypophosphite, ammonium hydrogen phosphate, and ammonium phosphate; The mass ratio of the powdery mixture to the porogen is 100:2-50.

4. The preparation method according to claim 1, characterized in that: In step (2), the temperature of the pre-carbonization treatment is 200-450 °C, and the time is 2-8 h; the heating rate during the pre-carbonization treatment is 1-20 °C / min.

5. The preparation method according to claim 1, characterized in that: In step (3), the high molecular organic matter is selected from one or more of polybutadiene, polystyrene, polyethylene, polyethersulfone, polyetherimide, polyimide, phenolic resin, epoxy resin, polyethylene resin, and polystyrene resin; the mass ratio of the pre-carbonized product to the high molecular organic matter is 1-50:2-500; The dispersant is one or more of methanol, ethanol, n-propanol, isopropanol, formic acid, and acetic acid; the mass ratio of the pre-carbonized product to the dispersant is 100:0.1-50; The stirring and mixing temperature is 80-300°C.

6. The preparation method according to claim 1, characterized in that: In step (3), the temperature of the carbonization treatment is 1100-1700°C and the time is 2-20 h.

7. A hard carbon negative electrode material, characterized in that: The hard carbon negative electrode material is prepared by the preparation method according to any one of claims 1 to 6.

8. The hard carbon negative electrode material according to claim 7, characterized in that: The hard carbon negative electrode material is a core-shell structure, which consists of a hard carbon core, an internal porous hard carbon layer and an external porous carbon layer from the inside to the outside; the particle size of the hard carbon core is 0.5-25 μm, the thickness of the internal porous hard carbon layer is 2-500 nm, and the thickness of the external porous carbon layer is 0.1-5 μm.

9. A negative electrode plate, characterized in that: The hard carbon negative electrode material according to claim 7 or 8; the method for preparing the negative electrode sheet comprises the following steps: (1) weighing a hard carbon negative electrode material, a conductive material and a binding material according to the mass ratio of each component in the negative electrode active material layer of the negative electrode plate, and stirring and mixing the hard carbon negative electrode material with a portion of the conductive material, a portion of the binding material and water for the first time to obtain a primary mixture; (2) the primary mixture prepared in step (1) is mixed with the remaining conductive material, the remaining adhesive material and water for a second time to obtain a secondary mixture, wherein the solid content of the secondary mixture is 40-60% and the viscosity is 1-9 Pa.s; (3) The secondary mixed material prepared in step (2) is coated on the negative electrode fluid, and the negative electrode sheet is obtained by drying, cold pressing and cutting.

10. A secondary battery, characterized in that: Contains the hard carbon negative electrode material according to claim 7, or the negative electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Hard carbon composite material, material preparation method, electrode plate and battery

    CN116130659A

  • Negative electrode material as well as preparation method and application thereof

    CN116344812A

  • Hard carbon negative electrode material, and preparation method therefor and use thereof

    WO2023098191A1

  • Hard carbon negative electrode material for sodium-ion battery and preparation method therefor

    WO2023109660A1