A kind of sulfonated modified polyacrylamide and preparation method thereof
By mixing acrylamide, solvent-promoting agent and molecular weight extension agent in water and initiating a polymerization reaction, a high molecular weight polyacrylamide colloid is prepared, and then sulfonated with hexamethylenetetramine and sulfonation reagent is solved in the prior art. The problem of difficulty in obtaining high molecular weight and high sulfonation degree has achieved simplification of the process and reduced cost, and is suitable for industrial production.
Patent Information
- Application Number
- CN202310874990.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-07-17
AI Technical Summary
The existing sulfonated modified polyacrylamide preparation process is difficult to obtain high molecular weight and high sulfonation products, and the process cost is high and it is not suitable for industrial production.
A high molecular weight polyacrylamide colloid is prepared by uniformly mixing acrylamide, solvent-enhancing agent and molecular weight extension agent in water, and then sulfonating with hexamethylenetetramine and sulfonation reagent is carried out in water. The reaction was obtained to obtain a sulfonated modified polyacrylamide having ultra-high molecular weight and high sulfonation degree.
The preparation of sulfonated modified polyacrylamide with a molecular weight of no less than 2000w and a sulfonation degree of up to 50% has been achieved, which simplifies the process flow, reduces energy consumption, and is suitable for industrial production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer polymerization, and in particular to a sulfonated modified polyacrylamide and a preparation method thereof. Background Art
[0002] Polyacrylamide is known as the "auxiliary agent for all industries" and is widely used in various industries such as oil and gas fields, water treatment, papermaking, mining, textiles, building materials, agriculture, etc. Since the amide group itself has active chemical properties and is prone to various reactions, its high temperature resistance, salt resistance, and aging resistance are insufficient. Therefore, sulfonated modified polyacrylamide has become an important member of the polyacrylamide family by virtue of the heat resistance, salt resistance, and biological aging resistance of the sulfonic acid group.
[0003] With the demand for higher molecular weight polyacrylamide in current production practice, the existing preparation process of sulfonated modified polyacrylamide is difficult to further improve the molecular weight of sulfonated modified polyacrylamide. First, for the method of directly adding a functional monomer containing a sulfonic acid group to copolymerize with acrylamide and other monomers to obtain sulfonated modified polyacrylamide, the reaction activity of the functional monomer containing a sulfonic acid group is quite different from that of the main monomers acrylamide, acrylic acid, etc. When the amount of the functional monomer added is large, a product with a high molecular weight cannot be obtained by free radical copolymerization. Secondly, for the method of preparing sulfonated modified polyacrylamide by sulfonation reaction of polyacrylamide solution, formaldehyde, and sulfonating agent under alkaline conditions, since high molecular weight polyacrylamide is difficult to dissolve or is in a gel state, it leads to high energy consumption and high cost. It is generally carried out in the laboratory and is not suitable for industrial production; and under alkaline conditions, polyacrylamide will hydrolyze to produce ammonia, and ammonia will consume formaldehyde and sulfonating agent, so it is difficult to obtain sulfonated modified polyacrylamide with both high molecular weight and high sulfonation degree. Summary of the invention
[0004] The embodiment of the present invention provides a sulfonated modified polyacrylamide and a preparation method thereof. The sulfonated modified polyacrylamide has both ultra-high molecular weight and high sulfonation degree.
[0005] In a first aspect, the present invention provides a method for preparing sulfonated modified polyacrylamide, the preparation method comprising:
[0006] (1) adding acrylamide, a dissolving agent, and a molecular weight extending agent to water and mixing them uniformly to obtain a mixed solution; adding a composite initiator to the mixed solution to initiate a polymerization reaction to obtain the polyacrylamide colloid;
[0007] (2) adding hexamethylenetetramine and a sulfonating agent into water to obtain a modified solution;
[0008] (3) adding the polyacrylamide colloid into the modified liquid to carry out a sulfonation reaction to obtain the sulfonated modified polyacrylamide.
[0009] Preferably, the solubilizing agent is a non-ionic surfactant with an HLB value of 12 to 18.
[0010] Preferably, the molecular weight extender is at least one of dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and polyether polyol.
[0011] Preferably, the composite initiator comprises a high temperature initiator, an oxidizing agent, a reducing agent and a molecular weight regulator;
[0012] The high temperature initiator is at least one of azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, and azobisisopropylimidazoline;
[0013] The oxidant is at least one of persulfate, peroxydiphosphate, peroxydicarbonate, hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene peroxide, di-tert-butyl peroxide and tert-butyl perbenzoate;
[0014] The reducing agent is at least one of sulfite, pyrosulfite, hydroxylamine, ferrous salt, thiourea and ascorbic acid.
[0015] More preferably, the molecular weight regulator is at least one of isopropanol, isobutyl alcohol, tert-butyl alcohol, thioglycolic acid, mercaptan, sodium formate, and sodium hypophosphite.
[0016] Preferably, in step (1):
[0017] The weight proportions of the components for preparing the polyacrylamide colloid are as follows: 15-30 parts of acrylamide, 0.1-2 parts of the dissolution promoter, 0.01-2 parts of the molecular weight extender and 66-84 parts of water; wherein the mass ratio of the composite initiator to acrylamide is (0.013-3.5):100.
[0018] More preferably, the mass ratio of the high temperature initiator, the oxidant, the reducing agent, the molecular weight regulator and acrylamide is (0.01-2):(0.001-0.5):(0.001-0.5):(0.001-0.5):100.
[0019] Preferably, in step (1), the method further comprises:
[0020] The pH of the mixed solution is adjusted to 6-8.
[0021] Preferably, in step (1), the method further comprises: introducing nitrogen into the mixed solution, and adding the composite initiator into the mixed solution at -5 to 20°C to initiate the polymerization reaction.
[0022] Preferably, in step (2):
[0023] The molar ratio of hexamethylenetetramine to the sulfonating agent is 1:(2-8).
[0024] Preferably, in step (2), the sulfonation reagent is at least one of sulfite, pyrosulfite and bisulfite.
[0025] Preferably, in step (2), the pH of the modified solution is 2-6.
[0026] Preferably, a pH adjuster is used to adjust the pH of the modified liquid.
[0027] More preferably, the pH adjuster is at least one of phosphoric acid, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium hydroxide.
[0028] Preferably, in step (3), the particle size of the polyacrylamide colloid is 10 to 40 meshes.
[0029] Preferably, in step (3), the temperature of the sulfonation reaction is 70-100° C., and the reaction time is 2-8 hours.
[0030] In a second aspect, the present invention provides a sulfonated modified polyacrylamide prepared by any of the preparation methods described in the first aspect.
[0031] Compared with the prior art, the present invention has at least the following beneficial effects:
[0032] The present invention firstly adopts polymerization reaction to prepare polyacrylamide colloid with high molecular weight, and then directly carries out sulfonation reaction on the polyacrylamide colloid with sulfonation reagent and hexamethylenetetramine to obtain sulfonated modified polyacrylamide. In this way, the molecular weight of sulfonated modified polyacrylamide is not affected by the functional monomer containing sulfonic acid group, and there is no need to dissolve polyacrylamide in advance in the sulfonation reaction, but directly carries out sulfonation reaction with polyacrylamide in colloidal state, the preparation process is simple and easy, and the prepared sulfonated modified polyacrylamide has a molecular weight of not less than 2000w, and the sulfonation degree can be as high as more than 50%. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0034] The present invention provides a method for preparing sulfonated modified polyacrylamide, which comprises:
[0035] (1) adding acrylamide, a dissolving agent, and a molecular weight extending agent to water and mixing them uniformly to obtain a mixed solution; adding a composite initiator to the mixed solution to initiate a polymerization reaction to obtain a polyacrylamide colloid;
[0036] (2) adding hexamethylenetetramine and a sulfonating agent into water to obtain a modified solution;
[0037] (3) Adding polyacrylamide colloid into the modified liquid to carry out sulfonation reaction to obtain sulfonated modified polyacrylamide.
[0038] The present invention firstly adopts acrylamide and other monomers to obtain polyacrylamide colloid with high molecular weight through polymerization reaction, then prepares a modification liquid including a sulfonation reagent and hexamethylenetetramine, and then directly places the polyacrylamide colloid in the modification liquid for sulfonation reaction to obtain sulfonated modified polyacrylamide. In this way, the molecular weight of the sulfonated modified polyacrylamide is not affected by the functional monomer containing sulfonic acid group, and the polyacrylamide does not need to be dissolved in advance in the sulfonation reaction, but the sulfonation reaction is directly carried out with the polyacrylamide in colloidal state, the preparation process is simple and easy, and the prepared sulfonated modified polyacrylamide has a molecular weight of not less than 2000w, and the sulfonation degree can be as high as 50% or more.
[0039] According to some preferred embodiments, the solubilizing agent is a non-ionic surfactant with an HLB value of 12-18.
[0040] It should be noted that the HLB value is the hydrophilic-lipophilic balance value, that is, the comprehensive affinity of the hydrophilic and lipophilic groups in the surfactant molecule to oil or water. Specifically, the solubilizing agent includes but is not limited to alkylphenol polyoxyethylene ether (OP-10), Tween-20, Tween-40, and Tween-60.
[0041] According to some preferred embodiments, the molecular weight extender is at least one of dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and polyether polyol.
[0042] It should be noted that at least one is any one or a mixture of any several in any proportion. The molecular weight of the polyether polyol is determined according to actual preparation requirements and is not specifically limited here.
[0043] According to some preferred embodiments, in step (1):
[0044] The weight parts of the components for preparing the polyacrylamide colloid are as follows: 15 to 30 parts of acrylamide (for example, 15 parts, 16 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts or 30 parts), 0.1 to 2 parts of a dissolution promoter (for example, 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.6 parts or 2 parts), 0.01 to 2 parts of a molecular weight extender (for example, 0.01 parts, 0.02 parts, 0.05 parts, 0.06 parts, 0.08 parts, 0.1 parts, 0.2 parts, 0.5 parts, 1.6 parts or 2 parts), 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.6 parts or 2 parts) and 66 to 84 parts of water (for example, it can be 66 parts, 68 parts, 70 parts, 72 parts, 75 parts, 76 parts, 78 parts, 80 parts, 82 parts or 84 parts); wherein the mass ratio of the composite initiator to acrylamide is (0.013 to 3.5):100 (for example, it can be 0.013:100, 0.01:100, 0.05:100, 1:100, 1.5:100, 2:100, 2.5:100, 3:100 or 3.5:100).
[0045] In the present invention, experiments have confirmed that by limiting the amount of acrylamide, solubilizer, and molecular weight extender, it can further ensure that the prepared polyacrylamide has an ultra-high molecular weight, so as to provide ultra-high molecular weight polyacrylamide for the sulfonation reaction, and meet the industry's demand for high molecular weight sulfonated modified polyacrylamide.
[0046] According to some preferred embodiments, the composite initiator includes a high temperature initiator, an oxidizing agent, a reducing agent and a molecular weight regulator;
[0047] The high temperature initiator is at least one of azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, and azobisisopropylimidazoline;
[0048] The oxidant is at least one of persulfate, peroxydiphosphate, peroxydicarbonate, hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene peroxide, di-tert-butyl peroxide and tert-butyl perbenzoate;
[0049] The reducing agent is at least one of sulfite, pyrosulfite, hydroxylamine, ferrous salt, thiourea and ascorbic acid.
[0050] In the present invention, the composite initiator can utilize the heat released by the redox initiator when initiating the polymerization reaction at low temperature to increase the temperature of the reaction system, thereby causing the high-temperature initiator to decompose and generate free radicals to continuously initiate the polymerization reaction, thereby reducing energy consumption and increasing the copolymerization reaction conversion rate and the molecular weight of the polymer.
[0051] According to some preferred embodiments, the molecular weight regulator is at least one of isopropanol, isobutanol, tert-butanol, thioglycolic acid, mercaptan, sodium formate, and sodium hypophosphite.
[0052] According to some more preferred embodiments, the mass ratio of the high temperature initiator, the oxidant, the reducing agent, the molecular weight regulator and the acrylamide is (0.01-2):(0.001-0.5):(0.001-0.5):(0.001-0.5):100 (for example, it can be 0.01:0.001:0.001:0.001:100, 0.02:0.001:0.002:0.001:100, 0.1:0.005:0.005:0.01:100, 1:0.2:0.2:0.2:100, 1.5:0.3:0.3:0.5:100 or 2:0.5:0.5:0.5:100).
[0053] According to some preferred embodiments, in step (1), the step further includes: adjusting the pH of the mixed solution to 6-8 (for example, 6, 6.5, 7, 7.5 or 8).
[0054] According to some more preferred embodiments, step (1) further includes: adjusting the pH of the mixed solution to 7.0-7.5 (for example, 7.0, 7.1, 7.2, 7.3, 7.4 or 7.5).
[0055] In the present invention, it has been experimentally confirmed that the pH of the mixed solution is adjusted to 6-8, so that the acidity and alkalinity of the reaction medium can be prevented from affecting the decomposition rate of the initiator and the polymerization degree of the polyacrylamide colloid can be guaranteed.
[0056] According to some preferred embodiments, step (1) further includes: introducing nitrogen into the mixed solution, and adding a composite initiator to the mixed solution at -5 to 20°C (for example, -5°C, -2°C, 0°C, 1°C, 2°C, 3°C, 5°C, 8°C, 10°C, 12°C, 15°C, 18°C or 20°C) to initiate the polymerization reaction.
[0057] According to some preferred embodiments, the time for introducing nitrogen is 30 to 50 min (for example, 30 min, 35 min, 40 min, 45 min or 50 min).
[0058] In the present invention, since oxygen, as an inhibitor, will affect the polymerization reaction of polyacrylamide, nitrogen needs to be introduced to remove oxygen to ensure that the polymerization reaction proceeds normally.
[0059] Specifically, the preparation method of polyacrylamide colloid includes: adding acrylamide, a dissolving agent, and a molecular weight extending agent into water and mixing them evenly to obtain a mixed solution; adjusting the pH of the mixed solution to 6-8, passing nitrogen for 30-50 minutes, and then adding a composite initiator to initiate a polymerization reaction at -5-20°C to obtain polyacrylamide colloid.
[0060] According to some preferred embodiments, in step (2), the molar ratio of hexamethylenetetramine to the sulfonating agent is 1:(2-8) (for example, it can be 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5 or 1:8).
[0061] According to some preferred embodiments, in step (2), the sulfonation reagent is at least one of sulfite, pyrosulfite, and bisulfite.
[0062] According to some preferred embodiments, in step (2), the pH of the modified solution is 2 to 6 (for example, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5 or 6).
[0063] According to some preferred embodiments, a pH adjuster is used to adjust the pH of the modified liquid.
[0064] According to some more preferred embodiments, the pH adjuster is at least one of phosphoric acid, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium hydroxide.
[0065] In the present invention, the amount of polyacrylamide colloid and the modified liquid is not specifically limited, and is determined according to the sulfonation degree requirement. Hexamethylenetetramine and sulfonating agent play a role in the modified liquid, and water is only used as a solvent to dissolve hexamethylenetetramine and sulfonating agent. Therefore, hexamethylenetetramine and sulfonating agent are used as calculation standards, and the amount of hexamethylenetetramine and sulfonating agent is determined according to the required sulfonation degree and the amide groups contained in the polyacrylamide colloid. Among them, the more hexamethylenetetramine and sulfonating agent are used, the higher the sulfonation degree of the sulfonated modified polyacrylamide.
[0066] According to some more preferred embodiments, in step (3), the particle size of the polyacrylamide colloid is 10 to 40 mesh (for example, it can be 10 mesh, 12 mesh, 15 mesh, 18 mesh, 20 mesh, 25 mesh, 30 mesh, 35 mesh or 40 mesh).
[0067] It should be noted that, in order to facilitate the full reaction of the polyacrylamide colloid and the modified liquid, the polyacrylamide colloid prepared in step (1) is crushed and granulated to obtain a polyacrylamide colloid with a particle size of 10 to 40 meshes.
[0068] According to some preferred embodiments, in step (3), the temperature of the sulfonation reaction is 70-100°C (for example, it can be 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C), and the reaction time is 2-8h (for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h).
[0069] In the present invention, water is used as the reaction medium for polymerization reaction and sulfonation reaction, which not only has low cost, but also can eliminate the influence of organic solvent on environmental pollution, has a simple preparation process, and does not require heating due to the exothermic reaction. Moreover, the environment of the reaction medium is neutral, the preparation process is environmentally friendly, pollution-free, low in energy consumption, the product is non-toxic and non-corrosive, and does not generate secondary pollution, which is in line with the development direction of green environmental protection chemical additives.
[0070] The present invention also provides a sulfonated modified polyacrylamide, which is prepared by the preparation method provided by the present invention.
[0071] In order to more clearly illustrate the technical solution and advantages of the present invention, a sulfonated modified polyacrylamide and a preparation method thereof are described in detail through several embodiments below.
[0072] Preparation of polyacrylamide colloid A:
[0073] 200 g of acrylamide, 2 g of a solvent promoter (op-10), and 1 g of a molecular weight extender (dimethylaminoethyl methacrylate) were added to 797 g of deionized water and mixed and dissolved to obtain a mixed solution; the pH of the mixed solution was adjusted to 7.0-7.2, and nitrogen was introduced for 30 minutes, and then a composite initiator was added to initiate a polymerization reaction at 0-2° C. After the reaction was completed, the mixture was kept warm at the highest reaction temperature at that time for 2 hours to obtain polyacrylamide colloid A;
[0074] Among them, the composite initiator includes 0.03g of high-temperature initiator (azobisisobutylamidine hydrochloride), 0.002g of oxidant (tert-butyl hydroperoxide), 0.002g of reducing agent (sodium metabisulfite), 0.002g of reducing agent (ferrous sulfate), and 0.003g of molecular weight regulator (sodium formate).
[0075] Preparation of polyacrylamide colloid B:
[0076] 200 g of acrylamide, 3 g of a solvent promoter (op-10), and 2 g of a molecular weight extender (dimethylaminoethyl methacrylate) were added to 795 g of deionized water and mixed and dissolved to obtain a mixed solution; the pH of the mixed solution was adjusted to 7.0-7.2, and nitrogen was introduced for 30 minutes, and then a composite initiator was added to initiate a polymerization reaction at 0-2° C. After the reaction was completed, the mixture was kept warm for 2 hours to obtain polyacrylamide colloid B;
[0077] Among them, the composite initiator includes 0.02g of high-temperature initiator (azobisisobutylamidine hydrochloride), 0.002g of oxidant (tert-butyl hydroperoxide), 0.002g of reducing agent (sodium metabisulfite), 0.002g of reducing agent (ferrous sulfate), and 0.003g of molecular weight regulator (sodium formate).
[0078] Preparation of polyacrylamide colloid C:
[0079] 200 g of acrylamide, 3 g of a solvent promoter (op-10), and 2 g of a molecular weight extender (polyether polyol) were added to 795 g of deionized water and mixed and dissolved to obtain a mixed solution; the pH of the mixed solution was adjusted to 7.0-7.2, and nitrogen was introduced for 30 minutes, and then a composite initiator was added to initiate a polymerization reaction at 0-2° C. After the reaction was completed, the mixture was kept warm for 2 hours to obtain polyacrylamide colloid C;
[0080] The composite initiator includes 0.02 g of high-temperature initiator (azobisisopropylimidazoline), 0.002 g of oxidant (hydrogen peroxide), 0.004 g of reducing agent (sodium sulfite), and 0.003 g of molecular weight regulator (tert-butyl alcohol).
[0081] Preparation of the modified solution: 4.5 g of hexamethylenetetramine, 20 g of sodium bisulfite, 20 g of a buffer solution having a pH value of about 4, and 55.5 g of deionized water are fully mixed and dissolved to obtain a modified solution.
[0082] Example 1
[0083] After the polyacrylamide colloid A is crushed and granulated, 100 g of polyacrylamide colloid A particles are weighed and added into a reactor containing 45 g of the modification liquid and stirred sufficiently to allow the polyacrylamide colloid A particles to fully and evenly contact with the modification liquid. Then, the reactor is sealed and heated to 90° C. for reaction for 4 hours to obtain sulfonated modified polyacrylamide.
[0084] Example 2
[0085] After the polyacrylamide colloid A is crushed and granulated, 100 g of polyacrylamide colloid A particles are weighed and added into a reactor containing 75 g of the modification liquid and stirred sufficiently to allow the polyacrylamide colloid A particles to fully and evenly contact with the modification liquid. Then, the reactor is sealed and heated to 90° C. for reaction for 4 hours to obtain sulfonated modified polyacrylamide.
[0086] Example 3
[0087] After the polyacrylamide colloid A is crushed and granulated, 100 g of polyacrylamide colloid A particles are weighed and added into a reactor containing 105 g of the modification liquid and stirred sufficiently to allow the polyacrylamide colloid A particles to fully and evenly contact with the modification liquid. Then, the reactor is sealed and heated to 90° C. for reaction for 4 hours to obtain sulfonated modified polyacrylamide.
[0088] Example 4
[0089] After the polyacrylamide colloid B is crushed and granulated, 100 g of polyacrylamide colloid B particles are weighed and added into a reactor containing 75 g of the modified liquid and stirred sufficiently to allow the polyacrylamide colloid B particles to fully and evenly contact with the modified liquid. Then, the reactor is sealed and heated to 90° C. for reaction for 4 hours to obtain sulfonated modified polyacrylamide.
[0090] Example 5
[0091] After the polyacrylamide colloid B is crushed and granulated, 100 g of polyacrylamide colloid B particles are weighed and added into a reactor containing 105 g of the modified liquid and stirred sufficiently to allow the polyacrylamide colloid B particles to fully and evenly contact with the modified liquid. Then, the reactor is sealed and heated to 90° C. for reaction for 4 hours to obtain sulfonated modified polyacrylamide.
[0092] Example 6
[0093] Example 6 is basically the same as Example 2, except that polyacrylamide colloid A is replaced by polyacrylamide colloid C.
[0094] Example 7
[0095] Example 7 is basically the same as Example 2, except that the reactor is sealed and heated to 100° C. for 2 h.
[0096] Example 8
[0097] Example 8 is basically the same as Example 2, except that the reactor is sealed and heated to 70° C. for 8 h.
[0098] Comparative Example 1
[0099] Sulfonated modified polyacrylamide is obtained by free radical copolymerization of an aqueous solution of acrylamide and 2-acrylamide-2-methylpropane sulfonic acid; wherein the total mass proportion of acrylamide and 2-acrylamide-2-methylpropane sulfonic acid in the solution is 20wt%, that is, the effective content is 20wt%, wherein 2-acrylamide-2-methylpropane sulfonic acid accounts for 30wt% of the effective content.
[0100] Comparative Example 2
[0101] Sulfonated modified polyacrylamide is obtained by free radical copolymerization of an aqueous solution of acrylamide and 2-acrylamide-2-methylpropane sulfonic acid; wherein the total mass proportion of acrylamide and 2-acrylamide-2-methylpropane sulfonic acid in the solution is 25wt%, that is, the effective content is 25wt%, wherein 2-acrylamide-2-methylpropane sulfonic acid accounts for 50wt% of the effective content.
[0102] The sulfonated modified polyacrylamide obtained in Examples 1 to 8 and the colloidal sulfonated modified polyacrylamide obtained in Comparative Examples 1 and 2 were granulated, dried and ground to obtain sulfonated modified polyacrylamide particles. The sulfonated modified polyacrylamide particles were used as samples. The above samples were dissolved in water and methanol was added for precipitation to remove unreacted residual monomers, hexamethylenetetramine and sulfonation reagent, and then dried again to test the molecular weight and sulfonation degree. The test results are shown in Table 1.
[0103] Molecular weight test: According to the test method of anionic and non-ionic polyacrylamide for water treatment agents of the National Standard of the People's Republic of China GB / T17514-2017, the sample is prepared into a dilute solution using 1.0 mol / L sodium chloride solution, and its limiting viscosity is determined by an Ubbelohde viscometer, and the molecular weight of the sample is calculated according to the empirical formula.
[0104] Determination of sulfonation degree: Since only the sulfonic acid group in the purified sample contains sulfur, the sulfonation degree of the sample can be calculated based on the sulfur content in the sample. The sulfur determination method is as follows: Take about 1g of the sample and put it into a clean weighing bottle, then dry it in a (120±2)℃ constant temperature drying oven for 2h to a constant weight, and put it into the element analyzer for determination according to the operating requirements.
[0105] Table 1
[0106] Molecular weight (w) Sulfonation degree (%) Example 1 2120 29 Example 2 2086 47 Example 3 2098 65 Example 4 2569 48 Example 5 2405 66 Example 6 2080 47 Example 7 2085 48 Example 8 2094 47 Comparative Example 1 1378 29 Comparative Example 2 1132 48
[0107] As can be seen from the data in Table 1, based on Examples 1 to 3, it can be found that adjusting the amount of modifier has little effect on the molecular weight, but the degree of sulfonation increases with the increase in the amount of modifier. At the same time, based on Examples 2 and 4, it can be found that the change in molecular weight mainly depends on the molecular weight of the polyacrylamide colloid synthesized by the polymerization reaction, so by adjusting the amount of molecular weight regulator and molecular weight extender, an ultra-high molecular weight product with a molecular weight of more than 20 million can be prepared, so that the purpose of high-sulfonation ultra-high molecular weight products can be achieved through subsequent sulfonation modification. As shown in Comparative Examples 1 and 2, the free radical polymerization method commonly used in existing production, although the content of sulfonated monomers used in Comparative Example 2 is higher than that in Comparative Example 1, the molecular weight of the prepared sulfonated modified polyacrylamide is lower, and a sulfonated modified polyacrylamide with both high molecular weight and high degree of sulfonation cannot be obtained. In summary, the preparation method of the present invention can prepare a sulfonated modified polyacrylamide with a molecular weight of not less than 2000w and a degree of sulfonation of more than 50%, and is more suitable for industrial production, while reducing energy consumption and further improving production efficiency.
[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. The parts not described in detail in the present invention are well-known technologies of those skilled in the art.
Claims
1. A method for preparing sulfonated modified polyacrylamide, It is characterized in that The preparation method comprises: (1) adding acrylamide, a dissolving agent, and a molecular weight extender into water and mixing them uniformly to obtain a mixed solution; adding a composite initiator into the mixed solution to initiate a polymerization reaction to obtain the polyacrylamide colloid; the dissolving agent is a non-ionic surfactant with an HLB value of 12 to 18; the molecular weight extender is at least one of dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and polyether polyol; the composite initiator includes a high temperature initiator, an oxidant, a reducing agent, and a molecular weight regulator; The weight proportions of the components for preparing the polyacrylamide colloid are as follows: 15-30 parts of acrylamide, 0.1-2 parts of the dissolution promoter, 0.01-2 parts of the molecular weight extender and 66-84 parts of water; wherein the mass ratio of the composite initiator to acrylamide is (0.013-3.5):100; (2) adding hexamethylenetetramine and a sulfonating agent into water to obtain a modified solution; (3) Adding the polyacrylamide colloid into the modified liquid to carry out a sulfonation reaction to obtain the sulfonated modified polyacrylamide.
2. The preparation method according to claim 1, Features: The high temperature initiator is at least one of azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, and azobisisopropylimidazoline; The oxidant is at least one of persulfate, peroxydiphosphate, peroxydicarbonate, hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene peroxide, di-tert-butyl peroxide and tert-butyl perbenzoate; The reducing agent is at least one of sulfite, pyrosulfite, hydroxylamine, ferrous salt, thiourea and ascorbic acid.
3. The preparation method according to claim 1, Features: The molecular weight regulator is at least one of isopropanol, isobutyl alcohol, tert-butyl alcohol, thioglycolic acid, mercaptan, sodium formate, and sodium hypophosphite.
4. The preparation method according to claim 1, It is characterized in that In step (1), it also includes: Adjusting the pH of the mixed solution to 6-8; and / or Nitrogen is introduced into the mixed solution, and the composite initiator is added into the mixed solution at -5 to 20° C. to initiate a polymerization reaction.
5. The preparation method according to claim 1, It is characterized in that In step (2): The molar ratio of hexamethylenetetramine to the sulfonated reagent is 1:(2-8); and / or The sulfonating agent is at least one of sulfite, pyrosulfite and bisulfite.
6. The preparation method according to claim 1, It is characterized in that In step (2): The pH of the modified liquid is 2-6.
7. The preparation method according to claim 6, It is characterized in that In step (2): adjusting the pH of the modified solution using a pH adjusting agent; The pH adjuster is at least one of phosphoric acid, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium hydroxide.
8. The preparation method according to claim 1, It is characterized in that In step (3): The particle size of the polyacrylamide colloid is 10-40 meshes.
9. The preparation method according to any one of claims 1 to 8, It is characterized in that In step (3): The temperature of the sulfonation reaction is 70-100° C., and the reaction time is 2-8 hours.
10. A sulfonated modified polyacrylamide, It is characterized in that The method is prepared by any one of claims 1 to 9.