Cardanol modified lignosulfonate dye dispersant and preparation method thereof
Through the condensation and lignin grafting technology of cashew phenol and lignin, the lignin structure is optimized, and the problem of insufficient dispersion of existing lignin sulfonate dye dispersants is solved, and efficient and economical dye dispersion performance is achieved, and green degradable is adopted. Modifier significantly improves dispersion performance and stability.
Patent Information
- Application Number
- CN202410944460.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-26
AI Technical Summary
There is room for improvement in the dispersion and stability of existing lignin sulfonate dye dispersants, and traditional modification methods lead to heavy pollution and high toxicity, increasing economic costs.
One-step grafting method is performed by condensation of C-C bond between cashewol and lignin benzene ring to optimize the lignin structure, and prepare cashewol modified lignin sulfonate dye dispersant, which utilizes the aromatic and fatty properties of cashewol Provide more sulfonic acid group grafting sites to improve dispersion performance.
The structural optimization of lignin sulfonate dye dispersant has been achieved, and the dispersion performance has been improved, especially in low temperature and high temperature conditions, which has excellent dispersion performance, avoids the complex coupling and grafting process in traditional modification methods, and adopts green Degraded cashew phenol modifier.
Smart Images

Figure CN119019709A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lignin sulfonate dye dispersants, and particularly relates to a cardanol-modified lignin sulfonate dye dispersant and a preparation method thereof. Background Art
[0002] As the most common terminal application product of lignin, lignin-based dye dispersants are of great significance for replacing expensive chemical dispersants and realizing the industrial application of lignin resources. However, with the continuous expansion of the global dye industry market size and the proportion of downstream application fields, the existing lignin-based dye dispersants can no longer meet the requirements of modern fiber dyeing due to limitations such as structural uncertainty, self-color pollution, and weak adsorption between dye particles. There is still a lot of room for improvement in dispersibility and stability.
[0003] Lignin is a natural aromatic polymer with abundant reserves in nature. It has rich functional properties and a unique aromatic skeleton structure. Through polymerization and self-assembly between active free radicals, the modified groups can be grafted into the lignin structure, showing great potential in regulating the structural properties of lignin and optimizing the dispersibility of lignin sulfonates. However, the existing modification strategies of lignin dye dispersants often use chemical modifiers, which inevitably cause heavy pollution and high toxicity, and the complex coupling-complexation modification methods undoubtedly increase the economic cost. These problems have greatly limited the industrialization process of lignin dye dispersants. Using commercial lignin as raw material, the development of efficient and economical lignin dye dispersant modification and upgrading strategies plays a vital role in the development of the printing and dyeing industry and the value-added utilization of lignin.
[0004] The dye dispersibility of lignin sulfonate is mainly related to the molecular weight and the degree of sulfonation. The steric hindrance effect of the complex three-dimensional structure of lignin and the electrostatic repulsion of the rich anionic groups obtained by the dissociation of the sulfonic acid group make the dye molecules tend to be dispersed evenly and stably. However, too high a molecular weight will reduce the reactivity of lignin sulfonate with dye particles, and the strong hydrophilicity accompanied by too high a degree of sulfonation will lead to a decrease in the adsorption of lignin sulfonate to dye particles, which will affect the dispersion performance.
[0005] As an economical biomass resource, cardanol has the characteristics of low toxicity and easy degradation. Cardanol has both aromatic and fatty properties. The benzene ring in the structure can form a CC bond with lignin to form more sulfonic acid group grafting sites, while the unsaturated C 15 Branching affects the surface tension, viscosity and molecular weight of the lignin structure. Summary of the invention
[0006] The present invention aims at the problem that the existing lignin sulfonate dye dispersant has large dispersibility limitations and still has a lot of room for improvement in high temperature and low temperature dispersibility. A preparation method of a cardanol-modified lignin sulfonate dye dispersant is provided. Cardanol contains benzene rings and aliphatic long chains, and is grafted into the lignin structure in one step by CC bond condensation between the benzene rings of lignin, thereby achieving structural optimization of lignin. Another technical problem to be solved by the present invention is to provide a cardanol-modified lignin sulfonate dye dispersant, which has excellent dispersing properties for dye Disperse Blue 79 in particular.
[0007] Technical solution: In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a cardanol-modified lignin sulfonate dye dispersant comprises the following steps: using lignin as a raw material, reacting with formaldehyde and anhydrous sodium sulfite to obtain lignin sulfonate; then modifying the lignin sulfonate with cardanol to obtain a cardanol-modified lignin sulfonate dye dispersant; preferably, the dye is disperse blue 79. Specifically, the lignin and cardanol are mixed and added to deionized water, solid alkali is added to adjust the pH to completely liquefy the lignin, formaldehyde is added after heating, stirring at a constant temperature to react, anhydrous sodium sulfite is added to continue the reaction, and the cardanol-modified lignin sulfonate dye dispersant is obtained after precipitation, drying, and grinding.
[0009] The preparation method of the cardanol-modified lignin sulfonate dye dispersant comprises the following steps: the lignin is kraft lignin obtained from industrial pulping and papermaking, the weight percentage concentration of the lignin is 10% to 40%, and preferably, the weight percentage concentration of the lignin is 10%.
[0010] The preparation method of the cardanol-modified lignin sulfonate dye dispersant comprises the following steps: after the lignin is completely liquefied, the temperature is raised to 70-80° C., formaldehyde is added, the temperature is raised to 90-95° C. after constant temperature stirring for 1.5 hours, anhydrous sodium sulfite powder is added and the reaction is continued for 1.5-2.5 hours; preferably, after the lignin is completely liquefied, the temperature is raised to 75° C., formaldehyde is added, the temperature is raised to 95° C. after constant temperature stirring for 1.5 hours, and sulfonating agent powder is added and the reaction is continued for 2 hours.
[0011] In the preparation method of the cardanol-modified lignin sulfonate dye dispersant, the mass ratio of cardanol to lignin is 0.2:10 to 0.5:10; preferably, the mass ratio is 0.2:10 to 0.3:10; more preferably, the mass ratio is 0.3:10.
[0012] The preparation method of the cardanol-modified lignin sulfonate dye dispersant, the solid base is NaOH or KOH, the solid base is added to adjust the pH to 9-11; preferably, the pH is adjusted to 10; to ensure that the lignin is completely liquefied, the solid base is added to ensure that the lignin is fully liquefied, and at the same time, an alkaline environment is provided to promote the grafting process of the formaldehyde initiator. However, too high a pH value will lead to the occurrence of side reactions.
[0013] In the preparation method of the cardanol-modified lignin sulfonate dye dispersant, the mass ratio of the formaldehyde addition amount to the lignin is 2:25-3:25; the mass ratio of anhydrous sodium sulfite to lignin is 7:20-9:20; preferably, the mass ratio of the formaldehyde addition amount to the lignin is 2.5:25; the mass ratio of anhydrous sodium sulfite to lignin is 8:20-9:20; further preferably, the mass ratio of the formaldehyde addition amount to the lignin is 2.5:25; the mass ratio of anhydrous sodium sulfite to lignin is 8:20.
[0014] The preparation method of the cardanol-modified lignin sulfonate dye dispersant comprises the following steps: adding excess ethanol to the obtained lignin sulfonate solution to precipitate flocculent lignin sulfonate; filtering to obtain solid lignin sulfonate, drying at 60° C. overnight under vacuum conditions, and grinding to obtain the cardanol-modified lignin sulfonate dye dispersant.
[0015] The cardanol-modified lignin sulfonate dye dispersant prepared by the above method.
[0016] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0017] (1) The cardanol modifier used is green and biodegradable, with high economic efficiency, and can replace traditional petrochemical modifiers. In addition, cardanol contains benzene rings and aliphatic long chains, and can be grafted into the lignin structure in one step by condensing the CC bonds between the benzene rings of lignin, thereby achieving structural optimization of lignin and avoiding the expensive and complicated coupling grafting process in traditional modification methods.
[0018] (2) The hydrophobic phenylpropane structure in the lignin sulfonate of the present invention can adsorb dye particles, while the hydrophilic sulfonic acid group tends to the water phase, and the steric hindrance of the complex three-dimensional structure and the electrostatic repulsion generated by the dissociation of the sulfonic acid group make the dye particles uniformly dispersed in the water phase. The benzene ring in cardanol provides more sulfonic acid group grafting sites, and the unsaturated aliphatic long chain increases the steric hindrance effect, which greatly optimizes the dispersibility of lignin-based sulfonate.
[0019] (3) The cardanol-modified lignin sulfonate prepared by the present invention retains the structural properties of the original lignin, has a high degree of sulfonation at a low anhydrous sodium sulfite addition ratio, and has a uniform structure and a moderate molecular weight, which is conducive to the high activity and uniform dispersion of dye particles. It shows excellent levels in low-temperature and high-temperature dispersibility tests, which is higher than the ordinary lignin sulfonate dye dispersants on the market.
[0020] (4) The present invention utilizes the aromatic properties of cardanol and the structural characteristics of lignin self-condensation, uses formaldehyde as an initiator, and introduces cardanol into the lignin sulfonate structure in the form of direct condensation with lignin, thereby avoiding the complicated coupling copolymerization grafting process. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 FTIR graphs of kraft lignin and lignin sulfonate modified by cardanol (Example 2);
[0022] Figure 2 Kraft lignin and cardanol modified lignin sulfonate (Example 2) 1 H NMR spectra. DETAILED DESCRIPTION
[0023] The present invention is further illustrated below in conjunction with specific examples. The examples are implemented based on the technical solutions of the present invention. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0024] Example 1
[0025] The preparation method of the cardanol-modified lignin sulfonate dye dispersant is specifically as follows:
[0026] Take 10g of absolute dry kraft lignin and 0.2g of cardanol, mix them and add them into 100mL of deionized water (the mass percentage concentration of kraft lignin is 10%), add NaOH to adjust the pH to 9, heat to 75°C while stirring, add 1g of formaldehyde and continue stirring for 1.5 hours;
[0027] After further heating to 95°C, 4 g of anhydrous sodium sulfite was added and maintained for 2 hours;
[0028] The cardanol modified lignin sulfonate solution was collected; after cooling, excess anhydrous ethanol was added to precipitate the flocculent insoluble sulfonate, which was filtered and further ground under vacuum conditions at 60° C. overnight to obtain the cardanol modified lignin sulfonate dye dispersant powder.
[0029] Example 2
[0030] The preparation method of the cardanol-modified lignin sulfonate dye dispersant is specifically as follows:
[0031] Take 10g of absolute dry kraft lignin and 0.3g of cardanol, mix them and add them into 100mL of deionized water (the mass percentage concentration of kraft lignin is 10%), add NaOH to adjust the pH to 10, heat to 75°C while stirring, add 1g of formaldehyde and continue stirring for 1.5 hours;
[0032] After further heating to 95°C, 4 g of anhydrous sodium sulfite was added and maintained for 2 hours;
[0033] The cardanol modified lignin sulfonate solution was collected, and after cooling, excess anhydrous ethanol was added to precipitate flocculent insoluble sulfonate, which was filtered and placed under vacuum at 60° C. overnight to obtain cardanol modified lignin sulfonate dye dispersant powder.
[0034] FTIR image of the above cardanol modified lignin sulfonate dye dispersant ( Figure 1 )and 1 H NMR spectra ( Figure 2 ), compared with the raw material kraft lignin, specifically:
[0035] like Figure 1 As shown, at 3402cm -1 The broad absorption band at 2939cm is believed to be caused by abundant hydroxyl groups. -1 and 2825cm -1 The absorption peaks at 1713cm are due to the stretching of carbon-hydrogen bonds in the -CH2 / -CH3 group and the -OCH3 group. -1 The peak at 1597 cm -1 、1513cm -1 、1425cm -1 The absorption band at 1451cm belongs to the stretching vibration of the aromatic ring. -1 The corresponding infrared peak is divided into the asymmetric vibration of the methyl and methylene CH bonds in the skeleton, 1267 cm -1 The absorption peaks near 1212 cm are assigned to the stretching vibration of the guaiacyl CO bond. -1 The peaks near 1027cm are caused by the stretching vibration of the CO bond in the phenolic hydroxyl group and the phenol ether. -1 The nearby bands are caused by COH and COC structures. In addition, 855cm -1 and 810cm -1 The absorption band is the typical absorption band of CH bonds in G-type and S-type units. It can be seen that the corresponding infrared absorption peaks before and after cardanol modification and sulfonation reaction have not changed significantly, indicating that the structural properties of the original lignin are retained.
[0036] Compared with kraft lignin, the introduction of cardanol increased the -1 and 1126cm -1 The intensity of the absorption band corresponding to the stretching vibration of the CH bond in the aromatic ring increased slightly, indicating that in addition to the aromatic rings (G-type and S-type units), cardanol containing aromatic rings was introduced into the lignin skeleton. -1 The increase in the absorption peak intensity at 964 cm is also considered to be caused by the -CH2=CH2- group in the unsaturated fatty chain of cardanol. This indicates that cardanol has been successfully grafted into the lignin structure. -1 、629cm -1 and 495cm -1 The absorption peak at is attributed to SO4 2- The group also further proves the occurrence of sulfonation reaction.
[0037] like Figure 2 As shown, the chemical shifts near 0.8-1.5ppm and 1.9-2.2ppm are attributed to aliphatic hydrogen protons, and the signals near 3.1-4.4ppm are related to H in the methyl group. In addition, the signal values near 6.25-6.80ppm correspond to H2 and H6 of the S-type unit, and the signals near 6.80-7.25ppm belong to H2, H5, and H6 in the G-type unit. By comparing the response levels of different signals, it was found that with the introduction of sulfonic acid groups, the signal values of 6-7.5ppm in kraft lignin decreased significantly, indicating the lack of H protons in the aromatic ring, which also marked the occurrence of lignin condensation and sulfonation substitution reactions.
[0038] The lignin sulfonate modified by cardanol showed a strong aliphatic H signal, which was due to the bridging condensation (5-5') between the aromatic ring in lignin and the benzene ring in cardanol induced by HCHO. Among them, a new signal peak appeared near 4.06ppm in the lignin after sulfonation, which was considered to be caused by the H in the sulfonyl group, further indicating that the sulfonic acid grafting reaction occurred in the structure of the kraft lignin.
[0039] As shown in Table 1, the S content in the cardanol-modified lignin sulfonate is 116000 mg / Kg, proving the occurrence of the grafting reaction of the sulfonic acid group. In addition, the modified Mn and Mw changed from 634 g / mol and 1912 g / mol to 1385 g / mol and 2045 g / mol, respectively, and the PDI decreased from 3.016 to 1.477. The molecular weight increased slightly, and the PDI dropped to a lower state. The increase in the molecular weight of lignin indicates the occurrence of condensation and sulfonation reactions. A higher molecular weight is believed to provide sufficient steric hindrance.
[0040] Table 1 GPC and ICP results of kraft lignin and cardanol modified lignin sulfonate
[0041]
[0042] Example 3
[0043] The preparation method of the cardanol-modified lignin sulfonate dye dispersant is specifically as follows:
[0044] Take 10g of absolute dry kraft lignin and 0.3g of cardanol, mix them and add them into 50mL of deionized water (the mass percentage concentration of kraft lignin is 20%), add NaOH to adjust the pH to 10, heat to 75°C while stirring, add 1g of formaldehyde and continue stirring for 1.5 hours;
[0045] After further heating to 95°C, 4 g of anhydrous sodium sulfite was added and maintained for 2 hours;
[0046] The cardanol modified lignin sulfonate solution was collected, and after cooling, excess anhydrous ethanol was added to precipitate flocculent insoluble sulfonate, which was filtered and placed under vacuum at 60° C. overnight to obtain cardanol modified lignin sulfonate dye dispersant powder.
[0047] Example 4
[0048] The preparation method of the cardanol-modified lignin sulfonate dye dispersant is specifically as follows:
[0049] Take 10g of absolute dry kraft lignin and 0.3g of cardanol, mix them and add them into 50mL of deionized water (the mass percentage concentration of kraft lignin is 20%), add NaOH to adjust the pH to 10, heat to 75°C while stirring, add 1g of formaldehyde and continue stirring for 1.5 hours;
[0050] After further heating to 95°C, 4.5 g of anhydrous sodium sulfite was added and maintained for 2 hours;
[0051] The cardanol modified lignin sulfonate solution was collected, and after cooling, excess anhydrous ethanol was added to precipitate flocculent insoluble sulfonate, which was filtered and placed under vacuum at 60° C. overnight to obtain cardanol modified lignin sulfonate dye dispersant powder.
[0052] Example 5
[0053] The preparation method of the cardanol-modified lignin sulfonate dye dispersant is specifically as follows:
[0054] Take 10g of absolute dry kraft lignin and 0.3g of cardanol, mix them and add them into 50mL of deionized water (the mass percentage concentration of kraft lignin is 20%), add NaOH to adjust the pH to 10, heat to 75°C while stirring, add 0.8g of formaldehyde and continue stirring for 1.5 hours;
[0055] After further heating to 95°C, 4.5 g of anhydrous sodium sulfite was added and maintained for 2 hours;
[0056] The cardanol modified lignin sulfonate solution was collected, and after cooling, excess anhydrous ethanol was added to precipitate flocculent insoluble sulfonate, which was filtered and placed under vacuum at 60° C. overnight to obtain cardanol modified lignin sulfonate dye dispersant powder.
[0057] Comparative Example 1
[0058] The preparation method of lignin sulfonate dye dispersant is specifically as follows:
[0059] Take 10g of absolute dry kraft lignin, add it to 50mL of deionized water (the mass percentage concentration of kraft lignin is 20%), add NaOH to adjust the pH to 10, heat it to 75°C while stirring, add 0.8g of formaldehyde and continue stirring for 1.5 hours;
[0060] After further heating to 95°C, 4.5 g of anhydrous sodium sulfite was added and maintained for 2 hours;
[0061] The cardanol modified lignin sulfonate solution was collected, and after cooling, excess anhydrous ethanol was added to precipitate flocculent insoluble sulfonate, which was filtered and placed under vacuum at 60° C. overnight to obtain cardanol modified lignin sulfonate dye dispersant powder.
[0062] The samples prepared in Examples 1-5 and Comparative Example 1 were tested for high temperature and low temperature dispersibility and dispersing force. The low temperature dispersibility and high temperature dispersibility were measured by the double filter paper method of GB / T 5540-2017 and GB / T 5541, respectively. The disperse dye used was Disperse Blue 79, and the dispersing force test was performed according to GB / T 5550-2016. The results are shown in Table 2.
[0063] As can be seen from Table 2, Examples 1-5 all show excellent performance in the dispersion performance test. The low temperature and high temperature dispersion data represent the filtration time level / residue level, respectively, and are rated according to the national standard "filtration time level" and "residue five-level card". The filtration time of Examples 1-5 basically reaches the A-level in the low temperature and high temperature tests, and the residue level of the best Example 2 can reach good, and the other examples also reach medium and above levels. Examples 1-5 all have better performance in the dispersion force determination, which is higher than the level of lignin sulfonate dye dispersants on the market. As a control sample, in the dispersibility test of Comparative Example 1 without adding cardanol modifier, the filtration time and residue standards are poor, which further highlights the necessity of cardanol additives in the preparation of lignin sulfonate dye dispersants with industrial pulping wastewater.
[0064] Table 2 Low-temperature and high-temperature dispersibility and dispersibility test results of cardanol modified lignin sulfonate
[0065]
[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a cardanol-modified lignin sulfonate dye dispersant, characterized in that: Lignin is used as a raw material and reacted with formaldehyde and anhydrous sodium sulfite to obtain lignin sulfonate; then the lignin sulfonate is modified by cardanol to obtain a cardanol-modified lignin sulfonate dye dispersant.
2. The method for preparing the cardanol-modified lignin sulfonate dye dispersant according to claim 1, characterized in that: Specifically, lignin and cardanol are mixed and added into deionized water to prepare an aqueous solution, solid alkali is added to adjust the pH value so that the lignin is completely liquefied, formaldehyde is added after heating, stirring at a constant temperature, heating to react, anhydrous sodium sulfite is added and the reaction is continued, and after precipitation, drying and grinding, a cardanol-modified lignin sulfonate dye dispersant is obtained.
3. The method for preparing the cardanol-modified lignin sulfonate dye dispersant according to claim 1 or 2, characterized in that: The lignin is kraft lignin obtained from industrial pulping and papermaking, and its weight percentage concentration in the aqueous solution is 10% to 40%.
4. The method for preparing the cardanol-modified lignin sulfonate dye dispersant according to claim 2, characterized in that: After the lignin is completely liquefied, the temperature is raised to 70-80°C, formaldehyde is added, and the temperature is raised to 90-95°C after constant temperature stirring for 1.5 hours. After adding anhydrous sodium sulfite powder, the reaction is continued for 1.5-2.5 hours.
5. The method for preparing the cardanol-modified lignin sulfonate dye dispersant according to claim 1 or 2, characterized in that: The mass ratio of the cardanol to the lignin is 0.2:10 to 0.5:
10.
6. The method for preparing the cardanol-modified lignin sulfonate dye dispersant according to claim 2, characterized in that: The solid base is NaOH or KOH, and the pH is adjusted to 9-11.
7. The method for preparing the cardanol-modified lignin sulfonate dye dispersant according to claim 1 or 2, characterized in that: The mass ratio of the formaldehyde addition amount to lignin is 2:25 to 3:25; the mass ratio of anhydrous sodium sulfite to lignin is 7:20 to 9:
20.
8. The method for preparing the cardanol-modified lignin sulfonate dye dispersant according to claim 2, characterized in that: Excessive ethanol is added to the obtained lignin sulfonate solution to precipitate flocculent lignin sulfonate; solid lignin sulfonate is obtained by filtration, dried at 60° C. overnight under vacuum conditions, and ground to obtain a cardanol-modified lignin sulfonate dye dispersant.
9. The cardanol-modified lignin sulfonate dye dispersant prepared by the method of claim 1 or 2.