A modified fluorinated gypsum and its preparation method and application
By mixing and grinding quicklime and fluorogypsum, and adding naphthalene-based water-reducing agent, the problem of low grinding efficiency and poor activity of fluorogypsum is solved, and the efficient resource utilization of fluorogypsum and the application of environmentally friendly cementitious materials are realized.
Patent Information
- Application Number
- CN202310689669.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-06-12
AI Technical Summary
Due to its low grinding efficiency, strong acidity, and poor activity, fluorogypsum is difficult to be directly used as a cementing material, which limits its large-scale resource utilization, and its storage causes environmental pollution.
Modified fluorogypsum is prepared by mixing and grinding quicklime and fluorogypsum, and optionally adding a naphthalene-based water-reducing agent to improve grinding efficiency and hydration activity and inhibit the dissolution of fluoride ions.
It achieves efficient grinding and improved hydration activity of fluorogypsum, and can be directly used as cementing material, large-scale resource utilization, and reducing the risk of environmental pollution.
Smart Images

Figure CN116835896B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to modified fluorgypsum and a preparation method and application thereof. Background Art
[0002] Fluorogypsum is the waste residue produced by the fluoride salt plant using fluorite and concentrated sulfuric acid to produce hydrofluoric acid. Its main chemical composition is anhydrous calcium sulfate (type II), containing a certain amount of residual calcium fluoride, sulfuric acid, hydrofluoric acid, a small amount of silicon dioxide and trace amounts of Na + , K + Theoretically, every ton of hydrofluoric acid produced will produce 3.6 tons of fluorinated gypsum. According to relevant statistics, China ranks first in the world in the production of fluorinated gypsum waste residue, with an annual production of more than 10 million tons, of which Henan Province produces more than 500,000 tons of fluorinated gypsum each year, with a comprehensive utilization rate of about 10-15%.
[0003] Fluorogypsum has problems such as low grinding efficiency, strong acidity and poor activity, which restrict its direct use as a cementitious material, thus limiting its large-scale utilization. Currently, the treatment of fluorogypsum is still mainly in the form of stockpiling, which not only occupies a large amount of land, but also is a huge waste of resources; and long-term stockpiling of the acidic and soluble F contained in it will - The gradual leaching of toxic and harmful substances will cause serious pollution to the surrounding soil and groundwater; the density of fluorinated gypsum is relatively low, and the dust blown by the wind also greatly affects the air and environment. In recent years, although various places have basically achieved standardized storage, the maintenance cost of the storage site is high, which not only reduces the economic benefits of enterprises, but also has become a key factor restricting the sustainable development of enterprises.
[0004] At present, fluorinated gypsum is mainly used as an auxiliary cementitious material, or as a cement retarder instead of natural dihydrate gypsum, and its resource utilization rate is relatively low.
[0005] To this end, research on fluorgypsum modification has been carried out, with the aim of using fluorgypsum directly as a cementitious material through modification, thus providing technical support for the large-scale resource utilization of fluorgypsum.
[0006] Therefore, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention
[0007] The object of the present invention is to provide a modified fluorgypsum and a preparation method and application thereof, so as to help solve or alleviate the problem that fluorgypsum is not suitable for direct use as a cementitious material and is difficult to be utilized as a resource on a large scale.
[0008] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing modified fluorgypsum, comprising the following steps: mixing quicklime and fluorgypsum and grinding them.
[0009] Preferably, the method further comprises the step of adding a naphthalene-based water reducer.
[0010] Preferably, the mass ratio of the quicklime to the fluorgypsum is (0.5-1.0):100; the mass ratio of the naphthalene-based water reducer to the fluorgypsum is (0.3-1.5):100;
[0011] Preferably, the mass ratio of the naphthalene-based water reducer to the fluorinated gypsum is (0.3-0.9):100.
[0012] Preferably, the fluorgypsum is a by-product of the production of hydrogen fluoride; the particle size of the fluorgypsum is 0.3-1.5 cm, the pH value is 2.3, and the density is 2.59 g / cm 3 The main mineral component of the fluorgypsum is type II anhydrite, which also contains fluorite.
[0013] Preferably, the effective calcium oxide content of the quicklime is ≥80wt.%; and the naphthalene-based water reducer is a commercially available naphthalene-based water reducer.
[0014] Preferably, the mixing and grinding time is 15-45 minutes.
[0015] The present invention also provides a modified fluorgypsum, which adopts the following technical scheme: a modified fluorgypsum, wherein the modified fluorgypsum is prepared by the method as described above.
[0016] The present invention also provides a modified fluorgypsum product, which adopts the following technical scheme: a modified fluorgypsum product, wherein the modified fluorgypsum product is prepared by using the modified fluorgypsum as described above.
[0017] The present invention also provides a method for preparing a modified fluorgypsum product, which adopts the following technical scheme: the method for preparing the modified fluorgypsum product as described above comprises the following steps: (1) stirring and mixing the modified fluorgypsum and water to obtain a modified fluorgypsum slurry; (2) loading the modified fluorgypsum slurry into a mold and curing the mold to obtain the modified fluorgypsum product.
[0018] Preferably, the curing temperature is 20±5°C and the relative humidity is 70%±4%.
[0019] Beneficial effects:
[0020] The invention aims at the problems existing in using fluorgypsum directly as a cementitious material, and proposes a method for modifying it by using quicklime alone or quicklime and a naphthalene-based water reducer at the same time, which is low in cost, easy to implement and suitable for industrial production. The preparation method of the modified fluorgypsum of the invention adopts a single raw material with fewer types, has a very low production cost and is suitable for large-scale production.
[0021] The present invention is to mix fluorgypsum with a certain proportion of quicklime and naphthalene-based water reducer and then grind it, which not only improves the grinding efficiency, but also improves the hydration activity of fluorgypsum and effectively inhibits the dissolution of fluoride ions. The modified fluorgypsum of the present invention can be directly used as a cementitious material to achieve large-scale resource utilization of fluorgypsum. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:
[0023] Figure 1 The effect of quicklime dosage on the pH value of fluorite provided in the embodiment of the present invention;
[0024] Figure 2 Effect of grinding time on the particle size distribution of modified fluorgypsum particles: (a) particle size distribution; (b) cumulative volume;
[0025] Figure 3 SEM images of fluorinated gypsum after grinding for 15 min: (a) without quicklime; (b) with 0.75% quicklime;
[0026] Figure 4 This is an XRD comparison diagram of the modified fluorgypsum obtained by grinding for 15 minutes in Example 2 and the ground fluorgypsum in Comparative Example 1;
[0027] Figure 5 Effect of water reducer dosage on particle size distribution of modified fluorgypsum: (a) particle size distribution; (b) cumulative volume;
[0028] Figure 6 The results of setting time and water consumption of standard consistency of fluorgypsum modified with different water reducing agent dosages;
[0029] Figure 7 is the flexural strength of modified fluorgypsum products at different hydration ages;
[0030] Figure 8 is the compressive strength of modified fluorgypsum products at different hydration ages;
[0031] Fig. 9 The images of modified fluorgypsum products with different water reducing agent dosages after hydration for 3 days;
[0032] Fig.10 The hydration rate results of modified fluorgypsum with different water reducing agent dosages. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.
[0034] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.
[0035] The present invention aims to solve the problem that fluorgypsum is not suitable for direct use as a cementitious material and is difficult to be used as a resource on a large scale, and provides a method for preparing modified fluorgypsum. The method for preparing modified fluorgypsum in an embodiment of the present invention comprises the following steps: mixing quicklime and fluorgypsum with powder.
[0036] In the process of mixing quicklime with fluorgypsum for grinding, quicklime can play a role in grinding, which helps to improve the grinding effect of fluorgypsum, reduce the particle size of fluorgypsum, and make the particle size of the modified fluorgypsum more uniform; in addition, quicklime can also play a role in adjusting pH, solidifying free F - The effect of ions also helps to improve the mechanical properties and hydration rate of modified fluorgypsum products.
[0037] In a preferred embodiment of the present invention, the step of adding a naphthalene-based water reducer is also included. The naphthalene-based water reducer can also act as a grinding aid during the grinding process of fluorgypsum, shorten the setting time of the modified fluorgypsum and reduce the water consumption of the standard consistency, which is helpful to improve the mechanical properties of the modified fluorgypsum products and increase the hydration rate.
[0038] In a preferred embodiment of the present invention, the mass ratio of quicklime to fluorgypsum is (0.5-1.0):100 (for example, 0.5:100, 0.6:100, 0.7:100, 0.8:100, 0.9:100 or 1.0:100); the mass ratio of naphthalene-based water reducer to fluorgypsum is (0.3-1.5):100 (for example, 0.3:100, 0.5:100, 0.7:100, 0.9:100, 1.1:100, 1.2:100, 1.3:100, 1.4:100 or 1.5:100).
[0039] In a preferred embodiment of the present invention, the mass ratio of the naphthalene water reducer to the fluorgypsum is (0.3-0.9):100 (for example, 0.4:100, 0.6:100 or 0.8:100). When the mass ratio of the naphthalene water reducer to the fluorgypsum is (0.3-0.9):100, the surface of the modified fluorgypsum product is smooth, without obvious cracks, and has good mechanical properties and volume stability.
[0040] In a preferred embodiment of the present invention, the mass ratio of quicklime to fluorgypsum is 0.75:100; the mass ratio of naphthalene-based water reducer to fluorgypsum is 0.9:100.
[0041] In a preferred embodiment of the present invention, fluorgypsum is a by-product of the production of hydrogen fluoride; the particle size of fluorgypsum is 0.3-1.5 cm, the pH value is 2.3, and the density is 2.59 g / cm 3 ;The main mineral composition of fluorgypsum is type II anhydrite, which also contains fluorite.
[0042] In a preferred embodiment of the present invention, the effective calcium oxide content of quicklime is ≥80wt.%; and the naphthalene-based water reducer is a commercially available naphthalene-based water reducer.
[0043] In a preferred embodiment of the present invention, the mixed grinding is carried out in a ball mill, and the mixed grinding time is 15-45 min (for example, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min or 45 min).
[0044] Preferably, the ball mill is a Φ50 cm×50 cm ball mill.
[0045] The present invention also provides a modified fluorspar. The modified fluorspar in the embodiment of the present invention is prepared by the method as described above.
[0046] The present invention also provides a modified fluorgypsum product. The modified fluorgypsum product in the embodiment of the present invention is prepared by using the modified fluorgypsum as described above.
[0047] The present invention also proposes a method for preparing a modified fluorgypsum product. The method for preparing the modified fluorgypsum product of an embodiment of the present invention comprises the following steps: (1) stirring and mixing the modified fluorgypsum and water to obtain a modified fluorgypsum slurry; and (2) charging the modified fluorgypsum slurry into a mold and curing the mold to obtain the modified fluorgypsum product.
[0048] In a preferred embodiment of the method for preparing the modified fluorgypsum products of the present invention, the curing temperature is 20±5°C (for example, 15°C, 18°C, 20°C, 22°C, 24°C or 25°C), and the relative humidity is 70%±4% (for example, 66%, 68%, 70%, 72% or 74%).
[0049] The modified fluorgypsum and its preparation method and application of the present invention are described in detail below through specific embodiments.
[0050] In the following examples, the fluorinated gypsum used is a byproduct of the production of hydrogen fluoride, and is an off-white spherical particle with a particle size of 0.3 to 1.5 cm, a pH value of 2.3, and a density of 2.59 g / cm 3 , its main mineral is type II anhydrite, and it also contains a small amount of fluorite residue;
[0051] The quicklime is quicklime powder, and the technical requirements meet the requirements of qualified and above grades in the industry standard "Construction Quicklime Powder" (JC / T480-92);
[0052] Naphthalene-based water reducer is a commercially available powder in the form of brown-yellow powder.
[0053] Example 1
[0054] The preparation method of the modified fluorgypsum of the present embodiment comprises the following steps: mixing 100 parts of fluorgypsum with 0.5 parts, 0.75 parts, 1.0 parts and 1.5 parts of quicklime respectively by mass, placing the mixture in a Φ50cm×50cm ball mill and grinding it for 15 minutes to obtain the modified fluorgypsum of the present embodiment.
[0055] The preparation method of the modified fluorgypsum product of the present embodiment comprises the following steps: (1) weighing water and powdered modified fluorgypsum of the present embodiment according to a set water-to-material ratio, pouring them into a stirring pot in turn, and stirring them evenly to obtain modified fluorgypsum slurry; wherein the amount of water used in the preparation of the modified fluorgypsum slurry is determined according to the standard consistency water amount; when the amount of quicklime is 0.5 parts, 0.75 parts, 1.0 parts and 1.5 parts, the corresponding water-to-material ratios are 0.28, 0.31, 0.32 and 0.327 respectively;
[0056] (2) The modified fluorinated gypsum slurry in step (1) is respectively loaded into molds of predetermined specifications, and the setting time and compressive strength are tested respectively;
[0057] (3) Setting time and compressive strength: The setting time of gypsum slurry was tested using a Vicat instrument according to the national standard "Plastering Gypsum" (GB / T28627-2012). The mechanical properties test specimens of the hardened slurry were 40 mm × 40 mm × 160 mm in size. The curing conditions were: temperature 20 ± 5 °C, relative humidity (RH) 70 ± 4%. The flexural strength and compressive strength were tested at 3d, 7d and 28d, respectively. Three specimens were tested in each group, and the average value was taken as the final result.
[0058] The pH values of fluorgypsum and the modified fluorgypsum prepared in this example were measured to determine the effect of quicklime content on the pH value of fluorgypsum. The experimental results are shown in FIG. Figure 1 shown.
[0059] Depend on Figure 1 It can be seen that the pH of the modified fluorgypsum prepared by adding quicklime at 0.5%, 0.75%, 1.0% and 1.5% of the mass of fluorgypsum respectively increases with the increase of quicklime addition; when the addition amount is 0.75%, the pH value reaches neutral, which is 7.3.
[0060] Example 2
[0061] The preparation method of the modified fluorgypsum of the present embodiment comprises the following steps: 100 parts of fluorgypsum and 0.75 parts of quicklime are mixed by mass, and the mixture is placed in a Φ50cm×50cm ball mill and ground for 15min, 30min and 45min respectively to obtain the modified fluorgypsum of the present embodiment.
[0062] The preparation method of the modified fluorgypsum product of the present embodiment comprises the following steps: (1) weighing water and powdered modified fluorgypsum of the present embodiment according to a set water-to-material ratio, pouring them into a stirring pot in turn, and stirring them evenly to obtain modified fluorgypsum slurry; wherein the amount of water used in the preparation of the modified fluorgypsum slurry is determined according to the standard consistency water amount; when the grinding time is 15 min, 30 min and 45 min, the corresponding water-to-material ratio is 0.31, 0.35 and 0.38 respectively;
[0063] (2) The modified fluorinated gypsum slurry in step (1) is respectively loaded into molds of predetermined specifications, and the setting time and compressive strength are tested respectively;
[0064] (3) Setting time and compressive strength: The setting time of gypsum slurry was tested using a Vicat instrument according to the national standard "Plastering Gypsum" (GB / T28627-2012). The mechanical properties test specimens of the hardened slurry were 40 mm × 40 mm × 160 mm in size and were cured at 20 ± 5 °C and 70 ± 4% relative humidity (RH). The flexural strength and compressive strength were tested at 3d, 7d, and 28d, respectively. Three specimens were tested in each group, and the average value was taken as the final result.
[0065] Example 3
[0066] The preparation method of the modified fluorgypsum of the present embodiment comprises the following steps: by weight, 100 parts of fluorgypsum and 0.75 parts of quicklime are mixed with 0.3, 0.6, 0.9, 1.2 and 1.5 parts of naphthalene-based water reducer respectively, and the mixture is placed in a Φ50cm×50cm ball mill and ground for 15 minutes respectively to obtain the modified fluorgypsum of the present embodiment.
[0067] The preparation method of the modified fluorgypsum product of the present embodiment comprises the following steps: (1) weighing water and powdered modified fluorgypsum of the present embodiment according to a set water-to-material ratio, pouring them into a stirring pot in turn, and stirring them evenly to obtain modified fluorgypsum slurry; wherein the amount of water used in the preparation of the modified fluorgypsum slurry is determined according to the standard consistency water amount; when the amount of naphthalene-based water reducer is 0.3 parts, 0.6 parts, 0.9 parts, 1.2 parts and 1.5 parts respectively, the corresponding water-to-material ratios are 0.396, 0.382, 0.37, 0.312 and 0.232 respectively;
[0068] (2) The modified fluorinated gypsum slurry in step (1) is respectively loaded into molds of predetermined specifications, and the setting time and compressive strength are tested respectively;
[0069] (3) Setting time and compressive strength: The setting time of gypsum slurry was tested using a Vicat instrument according to the national standard "Plastering Gypsum" (GB / T28627-2012). The mechanical properties test specimens of the hardened slurry were 40 mm × 40 mm × 160 mm in size and were cured at 20 ± 5 °C and 70 ± 4% relative humidity (RH). The flexural strength and compressive strength were tested at 3d, 7d, and 28d, respectively. Three specimens were tested in each group, and the average value was taken as the final result.
[0070] Comparative Example 1
[0071] The preparation method of the ground fluorgypsum of this comparative example comprises the following steps: 100 parts by mass of fluorgypsum are placed in a Φ50cm×50cm ball mill and ground for 15 minutes to obtain the ground fluorgypsum of this comparative example.
[0072] The preparation method of the ground fluorite product of the comparative example comprises the following steps: (1) weighing water and powdered ground fluorite of the comparative example respectively according to a set water-to-material ratio (0.2), pouring them into a stirring pot in sequence, and stirring them evenly to obtain ground fluorite slurry;
[0073] (2) The ground fluorinated gypsum slurry in step (1) is respectively loaded into molds of pre-set specifications, and the setting time and compressive strength are tested respectively;
[0074] (3) Setting time and compressive strength: The setting time of gypsum slurry was tested using a Vicat instrument according to the national standard "Plastering Gypsum" (GB / T28627-2012). The mechanical properties test specimens of the hardened slurry were 40 mm × 40 mm × 160 mm in size and were cured at 20 ± 5 °C and 70 ± 4% relative humidity (RH). The flexural strength and compressive strength were tested at 3d, 7d, and 28d, respectively. Three specimens were tested in each group, and the average value was taken as the final result.
[0075] Comparative Example 2
[0076] The fluorinated gypsum is modified by using a polycarboxylic acid water reducer instead of a naphthalene water reducer, comprising the following steps: 100 parts of fluorinated gypsum and 0.75 parts of quicklime are respectively mixed with 0.3 parts of the polycarboxylic acid water reducer, and the mixture is placed in a Ф50cm×50cm ball mill and ground for 15 minutes to obtain the modified fluorinated gypsum of this comparative example.
[0077] The preparation method of the modified fluorgypsum product of the comparative example comprises the following steps: (1) weighing water and powdered modified fluorgypsum of the comparative example respectively according to a set water-to-material ratio (0.26, determined according to the water consumption of the standard consistency), and pouring them into a stirring pot in sequence, stirring them evenly, to obtain modified fluorgypsum slurry;
[0078] (2) The modified fluorinated gypsum slurry in step (1) is respectively loaded into molds of predetermined specifications, and the setting time and compressive strength are tested respectively;
[0079] (3) Setting time and compressive strength: The setting time of gypsum slurry was tested using a Vicat instrument according to the national standard "Plastering Gypsum" (GB / T28627-2012). The mechanical properties test specimens of the hardened slurry were 40 mm × 40 mm × 160 mm in size and were cured at 20 ± 5 °C and 70 ± 4% relative humidity (RH). The flexural strength and compressive strength were tested at 3d, 7d, and 28d, respectively. Three specimens were tested in each group, and the average value was taken as the final result.
[0080] Experimental example
[0081] 1. The particle size distribution of the modified fluorgypsum prepared in Example 2 and the ground fluorgypsum prepared in Comparative Example 1 was tested:
[0082] Particle size distribution diagram Figure 2 The particle size characterization parameters are shown in Table 1 below;
[0083] Table 1 Characterization of particle size of modified fluorgypsum and ground fluorgypsum
[0084]
[0085] Depend on Figure 2 As shown in Table 1, the addition of quicklime significantly reduced the particle size of fluorgypsum when grinding for 15 min. v (90) The particle size of the particles was reduced from 176 μm to 60.2 μm, which improved the grinding efficiency. The quicklime played a good role in aiding the grinding and dispersing. However, as the grinding time increased, the small particles gradually agglomerated due to the collision and extrusion of the grinding body, and the particle size gradually increased.
[0086] 2. The microscopic morphology of the modified fluorgypsum (with quicklime content of 0.75%) prepared by grinding for 15 min in Example 2 and the ground fluorgypsum (without quicklime) prepared by grinding for 15 min in Comparative Example 1 were observed, and the XRD patterns, main chemical compositions and soluble F - content.
[0087] The SEM images of the modified fluorgypsum (with quicklime content of 0.75%) prepared by grinding for 15 min in Example 2 and the ground fluorgypsum (without quicklime) prepared by grinding for 15 min in Comparative Example 1 are shown as follows: Figure 3 (b) and 3(a); XRD patterns are shown in Figure 4 As shown; chemical composition and solubility F - The contents are shown in Table 3 below.
[0088] Table 3 Main chemical composition of modified fluorgypsum ground for 15 min in Example 2 and ground fluorgypsum ground for 15 min in Comparative Example 1 (wt.%)
[0089]
[0090] Depend on Figure 3 It can be seen that the addition of quicklime makes the size of fluorgypsum particles more uniform after grinding, the particle surface is rough, and the shape tends to be spherical.
[0091] Depend on Figure 4 It can be seen that the characteristic diffraction peak of fluorgypsum is significantly enhanced after grinding, and its grain size and structural regularity are also significantly improved due to the grinding effect of quicklime; and the diffraction peak of fluorite is significantly enhanced, and the content increases from 3.63% of fluorgypsum to 8.48%. The increase in fluorite content is also beneficial to the grinding of fluorgypsum.
[0092] It can be seen from Table 3 that the solubility of modified fluorgypsum is - The ion content was reduced by 80.7%. The following reactions may have occurred during the grinding process:
[0093] CaO+2H + +2F - →CaF2↓+H2O (1)
[0094] 3. Investigate the influence of quicklime on the performance of fluorgypsum:
[0095] (1) The setting and hardening properties of the modified fluorgypsum prepared by grinding for 15 minutes with a quicklime content of 0.75% in Example 2 and the ground fluorgypsum prepared by grinding for 15 minutes without quicklime in Comparative Example 1 were compared; the test results are shown in Table 4 below:
[0096] Table 4 Comparison of physical properties of fluorgypsum products obtained by grinding with and without quicklime
[0097]
[0098] Table 4 shows the effect of quicklime on the setting and hardening properties of fluorgypsum. The grinding aid of quicklime significantly reduces the particle size of fluorgypsum, resulting in an increase in the water consumption of the standard consistency; and a smaller particle size means that the specific surface area of fluorgypsum is larger, which is conducive to the hydration reaction, increases the hydration and hardening rate, and shortens the setting time. The mechanical properties of fluorgypsum products are also improved. The effect of quicklime on the strength of fluorgypsum products is more obvious at 28 days, and it can inhibit the occurrence of strength shrinkage of fluorgypsum products in the later stage.
[0099] (2) The hydration rates of the modified fluorgypsum prepared by grinding for 15 min in Example 2 with a quicklime content of 0.75% and the ground fluorgypsum prepared by grinding for 15 min without quicklime in Comparative Example 1 were respectively tested;
[0100] The test method is: the hydration rate is tested by a muffle furnace according to the national standard "Building gypsum-Determination of crystal water content" (GB / T17669.2-1999), and the dihydrate gypsum content and fluorinated gypsum hydration rate are calculated. The test results are shown in Table 5 below:
[0101] Table 5 Comparison of hydration rate of fluorinated gypsum with and without quicklime during grinding
[0102]
[0103] The hydration rate of fluorgypsum increased after adding quicklime grinding aid, as shown in Table 5. However, the hydration rate increased slightly within 1 day, and increased significantly after 1 day of curing; this rule is consistent with the mechanical properties.
[0104] 4. Water reducer is a common additional component in the application of cementitious materials. The particle size distribution of fluorgypsum is smaller after grinding, but it leads to an increase in the water consumption of standard consistency, which is not conducive to the development of performance. Grinding aids can not only improve the grinding efficiency of materials during the grinding process, but also reduce energy consumption, thereby improving the performance of powders. Therefore, the effect of naphthalene-based water reducer as a grinding aid on the performance of fluorgypsum is explored, and its grinding aid modification mechanism is revealed.
[0105] The particle size distribution of the modified fluorgypsum of Example 3 was tested, and the effect of different water reducing agent contents on the particle size distribution of fluorgypsum after grinding was shown in Figure 5 and Table 6 below.
[0106] Table 6 Effect of water reducing agent on grinding aid effect of fluorinated gypsum
[0107]
[0108]
[0109] The results show that naphthalene-based water reducers can play a "grinding aid" role in the grinding process of fluorgypsum. The particle size distribution of fluorgypsum first gradually optimizes to fine particles with the increase of water reducer dosage, and the distribution is more concentrated; when the water reducer dosage is 0.6%, the particle size distribution reaches the minimum, and then with the excessive water reducer particles gradually agglomerate, the particle size increases; the specific surface area of fluorgypsum particles also increases first and then decreases with the increase of water reducer dosage.
[0110] The results in Table 6 show that when the water reducer dosage is 0.6%, the median particle size of fluorgypsum particles is D v (90) is reduced to 37.8 μm, D v (50) is reduced to 3.76 μm, D v (10) decreased to 0.394 μm, and the specific surface area increased to 472.1 m 2 / kg.
[0111] The presence of an appropriate amount of water reducer makes the fluorgypsum particles more dispersed during the grinding process. The water reducer gradually adheres to the surface of the particles, reducing the mutual extrusion and collision between the particles, reducing the occurrence of particle agglomeration and paste grinding. However, excessive water reducer in the same grinding time will cause the fine particles to increase in surface roughness, increase in specific surface area, and increase in surface energy, which will cause mechanical meshing between each other and induce agglomeration, which is not conducive to grinding efficiency.
[0112] 5. Investigate the effect of naphthalene-based water reducer on the setting and hardening properties of modified fluorgypsum
[0113] (1) The standard consistency water requirement and setting time of the modified fluorgypsum with different water reducing agent dosages in Example 3 were tested:
[0114] The grinding aid effect of water reducer improves the grinding efficiency of fluorgypsum. Therefore, the water consumption of fluorgypsum slurry with standard consistency increases first and then decreases with the increase of water reducer dosage. Figure 6 When the water reducer dosage is low, the fluorite particles are finer. Although the water reducer adhering to the particle surface can increase the charge repulsion between particles, the increase in water demand caused by the increase in specific surface area is the main factor. As the water reducer dosage gradually increases, the degree of dispersion between particles increases and the water demand decreases.
[0115] The setting time of fluorinated gypsum shortens with the increase of water reducer dosage. When the water reducer dosage is low, the particle size of fluorinated gypsum is refined, thereby increasing the dissolution rate and the nucleation rate of dihydrate gypsum, accelerating the crystallization and growth of dihydrate gypsum, and accelerating the hydration process, resulting in a shortened setting time. As the water reducer dosage increases, the water consumption of standard consistency decreases, the distance between slurry particles is smaller, and it is easier to form a hardened structure between dihydrate gypsum after the hydration reaction, and the setting time is shortened. The initial setting time and final setting time of the slurry are shortened from 421min and 554min in the control group to 104min and 237min when the water reducer dosage is 1.5%, respectively.
[0116] Among them, the water demand and setting time tests are carried out in accordance with the national standard "Plaster Gypsum" (GB / T28627-2012).
[0117] (2) The mechanical properties of hardened fluorgypsum (modified fluorgypsum products) of different ages in Example 3 were tested:
[0118] The mechanical properties of hardened fluorinated gypsum at different ages showed a trend of first increasing and then decreasing with the increase of water reducer dosage, and both reached the maximum when the water reducer dosage was 0.9%.
[0119] Figure 7 In the test, when the dosage was 0.9%, the flexural strength of fluorinated gypsum increased from 1.9 MPa of the control group (the dosage of naphthalene-based water-reducing agent was 0; i.e., the sample numbered 1 in Table 6) to 5.4 MPa after hydration for 3 days, an increase of 184.2%; after hydration for 7 days, the flexural strength increased from 5.2 MPa of the control group to 9.1 MPa, an increase of 75.0%; after hydration for 28 days, the flexural strength increased from 7.9 MPa of the control group to 11.2 MPa, an increase of 41.8%.
[0120] Figure 8 The compressive strength of the control group at 3d, 7d and 28d of hydration was 3.5MPa, 7.6MPa and 10.0MPa respectively. When the water reducer dosage was 0.9%, the compressive strength of fluorinated gypsum at 3d, 7d and 28d of hydration was increased to 12.0MPa, 21.1MPa and 28.9MPa respectively, which was increased by 243%, 178% and 189% respectively.
[0121] Fig. 9In the test, the samples with water reducer dosage of 0-0.9% had a smooth surface without obvious cracks after hydration for 3 days; the samples with water reducer dosage of 1.2% and 1.5% had obvious cracks on the surface of modified fluorgypsum products after hydration for 3 days. The larger the water reducer dosage, the shorter the setting time of fluorgypsum slurry, and the easier it is for fluorgypsum to form a hardened structure; but the volume of dihydrate gypsum crystals generated by hydration is much larger than that of fluorgypsum, so after forming a stable hardened structure, as hydration continues, dihydrate gypsum crystals continue to grow, and the internal volume continues to expand, resulting in the destruction of the hardened structure and reduced volume stability, until obvious cracks appear on the surface of the sample, and the mechanical properties of the sample are also significantly reduced. This is the main reason why the setting time of fluorgypsum is shortened and the mechanical properties decrease after the water reducer dosage increases.
[0122] 6. Investigate the effect of naphthalene-based water reducer on the hydration rate of fluorinated gypsum at different hydration ages
[0123] like Fig.10 As shown. The hydration rate of fluorgypsum is affected by the water reducer and can be divided into two stages according to the hydration time. Before 3 days of hydration, the hydration rate increases with the increase of the water reducer dosage, from 37.68% in the control group to 66.81% when the water reducer dosage is 0.9%, and the maximum is 69.28% when the water reducer dosage is 1.5%, which is also in line with the result of setting time. The increase in the dissolution rate of fluorgypsum and the nucleation rate of dihydrate gypsum is the main reason for the increase in the hydration rate.
[0124] After hydration for 3 days, the hydration rate of fluorinated gypsum with a water-reducing agent content higher than 0.9% slowed down, while the hydration rate of fluorinated gypsum with a content not higher than 0.9% increased steadily. At 28 days, the hydration rate reached a maximum of 84.21% when the water-reducing agent content was 0.9%; at this time, the hydration rates of the control group and the 1.5% content were 45.37% and 75.71%, respectively. This result is the same as the result of mechanical properties. The cracking of fluorinated gypsum samples after the water-reducing agent content was higher than 0.9% caused the water inside the sample to dissipate outward, and the initial liquid phase environment was destroyed, which hindered the sustainability of the hydration reaction and was not conducive to the improvement of the hydration rate.
[0125] 7. The particle size, mechanical properties and hydration rate of the product obtained by modifying fluorinated gypsum with polycarboxylate water-reducing agent in Comparative Example 2 were tested respectively. The test results are shown in Tables 7-9 below:
[0126] Table 7 Characterization of particle size of modified fluorgypsum when the dosage of polycarboxylate water reducer is 0.3%
[0127]
[0128] Table 8 Performance of modified fluorinated gypsum when the dosage of polycarboxylate water reducer is 0.3%
[0129]
[0130] Table 9 Hydration rate of modified fluorinated gypsum when the dosage of polycarboxylate water reducer is 0.3%
[0131]
[0132] It can be seen from Tables 7-9 above that polycarboxylic acid has a high water-reducing efficiency. Although it can also play an obvious role in aiding the grinding and modification of fluorinated gypsum, it will inhibit the mechanical properties of the modified product and have a low hydration rate.
[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing modified fluorgypsum, characterized in that: The method comprises the following steps: mixing quicklime, naphthalene-based water reducing agent and fluorinated gypsum and grinding the mixture; The mass ratio of the quicklime to the fluorgypsum is 0.75:100, and the mass ratio of the naphthalene-based water reducer to the fluorgypsum is (0.3-0.9):100; The fluorite is a byproduct of the production of hydrogen fluoride. The particle size of the fluorite is 0.3-1.5 cm, the pH value is 2.3, and the density is 2.59 g / cm 3 The main mineral composition of the fluorgypsum is type II anhydrite, which also contains fluorite; The effective calcium oxide content of the quicklime is ≥80wt.%; The mixing and grinding time is 15 min.
2. The method for preparing modified fluorgypsum according to claim 1, characterized in that: The naphthalene-based water reducer is a commercially available naphthalene-based water reducer.
3. A modified fluorgypsum, characterized in that: The modified fluorgypsum is prepared by the method according to claim 1 or 2.
4. A modified fluorgypsum product, characterized in that: The modified fluorgypsum product is prepared using the modified fluorgypsum as claimed in claim 3.
5. The method for preparing the modified fluorgypsum product according to claim 4, characterized in that: The steps include: (1) stirring and mixing the modified fluorgypsum and water to obtain a modified fluorgypsum slurry; (2) The modified fluorgypsum slurry is placed in a mold and cured to obtain the modified fluorgypsum product.
6. The method for preparing the modified fluorgypsum product according to claim 5, characterized in that: The curing temperature is 20±5°C and the relative humidity is 70%±4%.
Citation Information
Patent Citations
Fluorogypsum-based mine filling material and use method thereof
CN105712688A