A time-controllable ultraviolet light curing system and its preparation method and application
The ultraviolet curing system adjusted by alcohol-modified epoxy carbamate solves the problem of uncontrollable curing time, achieves matching and stability of curing efficiency, and is suitable for underground pipeline repair and photocuring coatings.
Patent Information
- Application Number
- CN202310774651.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-06-28
AI Technical Summary
The curing time of ultraviolet light is uncontrollable, resulting in unstable curing efficiency and affecting the efficiency of underground pipeline repair process.
The preparation method of the ultraviolet curing system is prepared by using alcohol-modified epoxy carbamate as an activity regulator, combined with a specific proportion of matrix resin, photoinitiator, crosslinking agent, defoaming agent, leveling agent and accelerator. Adjust curing time and efficiency.
It realizes controllability of ultraviolet curing time, improves curing efficiency, and is suitable for non-excavation repair and photocuring coatings in underground pipelines, solving the problem of too fast or too slow curing time.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a time-controllable ultraviolet light curing system and a preparation method and application thereof, belonging to the technical field of ultraviolet light curing. Background Art
[0002] UV curing is different from the traditional drying process. Traditional drying generally relies on the volatilization of solvents in the coating material for curing, while UV curing is cross-linked without solvent volatilization. Therefore, UV curing is popular for its solvent-free and environmentally friendly characteristics. In the field of pipeline construction, it is an important construction technology to achieve trenchless repair of underground pipelines with the help of UV curing technology. During the pipeline construction process, the curing speed needs to be adjusted in time due to the influence of pipe wall thickness and fiber layer dosage. However, in actual construction, the light curing time cannot be effectively controlled, and more or less there will be problems such as too fast curing time is not conducive to construction, or too slow curing time reduces efficiency. Summary of the invention
[0003] The purpose of the present invention is to provide a time-controllable UV curing system, which can solve the problems of uncontrollable UV curing time and unstable curing efficiency. At the same time, based on the controllability of the curing time, it is applied to the field of non-excavation underground pipeline repair, and the formula of the UV curing system can be matched with the amount of paint used, the efficiency of photocuring non-excavation pipeline repair, the amount of fiber laying, etc., which is beneficial to on-site construction. The technical solution of the present invention can also be applied to fields such as photocuring coatings.
[0004] The second object of the present invention is to provide a method for preparing a time-controllable ultraviolet light curing system.
[0005] The third object of the present invention is to provide an application of a time-controllable UV curing system.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] A time-controllable ultraviolet curing system consists of the following components by mass percentage: 16-66% of base resin, 10-60% of alcohol-modified epoxy urethane, 1-3% of photoinitiator, 15-25% of crosslinking agent, 0.5-1.5% of defoamer, 0.5-1% of leveling agent and 0.2-1% of accelerator.
[0008] Preferably, a time-controllable UV curing system is composed of the following components by mass percentage: 46-66% base resin, 10-30% alcohol-modified epoxy urethane, 1-3% photoinitiator, 15-25% cross-linking agent, 0.5-1.5% defoaming agent, 0.5-1% leveling agent and 0.2-1% accelerator.
[0009] Further preferably, a time-controllable UV curing system is composed of the following components by mass percentage: 31-46% base resin, 30-45% alcohol-modified epoxy urethane, 1-3% photoinitiator, 15-25% cross-linking agent, 0.5-1.5% defoaming agent, 0.5-1% leveling agent and 0.2-1% accelerator.
[0010] Further preferably, a time-controllable UV curing system is composed of the following components by mass percentage: 16-31% base resin, 45-60% alcohol-modified epoxy urethane, 1-3% photoinitiator, 15-25% cross-linking agent, 0.5-1.5% defoaming agent, 0.5-1% leveling agent and 0.2-1% accelerator.
[0011] The base resin includes one of bisphenol A epoxy resin, alcohol-soluble phenolic resin, butyl acrylate, polyphenol glycidyl ether epoxy resin, and alkyd resin; the photoinitiator includes one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and benzil dimethyl ketal; the crosslinking agent includes one of polyamide, phthalic anhydride, maleic anhydride, and pyromellitic anhydride; the defoaming agent includes polydimethylsiloxane; the leveling agent includes fluorine-modified acrylic acid; and the accelerator includes one of cobalt cyclohexaneate and dimethylaniline.
[0012] The alcohol-modified epoxy urethane is obtained by the following steps:
[0013] Step 1: Mix epoxy resin and triethylene glycol in a mass ratio of 0.2:1, control the temperature to 75-85°C, react for 1-2h, and obtain a mixed solution a;
[0014] Step 2: adding a polymerization inhibitor hydroquinone equivalent to 0.02-0.05% by weight of the mixed solution a and a catalyst dodecylbenzylmethylamine equivalent to 0.2-0.5% by weight of the mixed solution a to the mixed solution a, stirring evenly, heating to 85-100° C., reacting for 2-3 hours, to obtain a mixed solution b;
[0015] Step 3: Add carbamic acid to the mixed solution b, the molar ratio of carbamic acid to epoxy resin is 1.05:1, maintain the reaction temperature at 100-110°C, react for 1-2 hours, adjust the acid value to 4-6 with an ethanol solution of NaOH, obtain alcohol-modified epoxy carbamate, and store in a sealed container.
[0016] The preparation method of NaOH ethanol solution is as follows: 2 g NaOH solid is dissolved in 200 mL 95% by mass ethanol.
[0017] A method for preparing a time-controllable ultraviolet curing system comprises the following steps:
[0018] S01, adding a photoinitiator to the alcohol-modified epoxy urethane, and shaking and stirring to obtain a uniformly dispersed mixed solution A;
[0019] S02, adding an accelerator and a cross-linking agent to a base resin, mixing them evenly, and then sequentially adding a defoamer and a leveling agent, mixing them evenly to obtain a mixture B;
[0020] S03, mixing the mixed solution A and the mixed solution B evenly, coating the mixed solution on a substrate, and irradiating the substrate with a 500W high pressure mercury lamp to solidify the mixed solution into a polymer film with a thickness of 6 mm.
[0021] The invention discloses a time-controllable ultraviolet light curing system for trenchless repair of underground pipelines.
[0022] Application of a time-controllable ultraviolet light curing system as a light-curing coating
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] The alcohol-modified epoxy carbamate provided by the present invention can be used as an active regulator, and has the advantages of light activity, low viscosity (its viscosity range is 230-250cp (60°C)), and good flexibility. The dosage can be adjusted according to the application of the system and the curing efficiency can be further adjusted.
[0025] The curing time of the UV curing system decreases with the increase of alcohol-modified epoxy urethane, and the curing efficiency is getting faster and faster. Therefore, the UV curing system of the present invention has the advantage of controllable curing time. It can be used in the field of trenchless repair of underground pipelines, effectively avoiding the problem that too fast curing time is not conducive to construction, or too slow curing time reduces efficiency, and has good film-forming properties. The UV curing system of the present invention can also be used in fields such as light-curing coatings.
[0026] The technical solution provided by the present invention can solve the problems of uncontrollable UV curing time and unstable curing efficiency. Based on the photoactive characteristics of the active regulator (alcohol-modified epoxy urethane), its curing time is controllable. It is applied to the field of trenchless underground pipeline repair, and can achieve the problem of matching the formula of the UV curing system with the amount of paint used, the efficiency of photocuring trenchless pipeline repair, the amount of fiber laying, etc., which is beneficial to on-site construction. The technical solution of the present invention can also be applied to fields such as photocuring coatings. DETAILED DESCRIPTION
[0027] The present invention will be further described in detail below in conjunction with specific examples. The following examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0028] The present invention provides a method for preparing a time-controllable ultraviolet curing system as follows:
[0029] Step (1): adding a photoinitiator to the alcohol-modified epoxy urethane, and shaking and stirring to obtain a uniformly dispersed mixed solution A;
[0030] Step (2): adding an accelerator and a cross-linking agent to the base resin, mixing them uniformly, and then adding a defoamer and a leveling agent in sequence to obtain a uniformly mixed mixture B;
[0031] Step (3): The mixed solution A and the mixed solution B are mixed evenly, applied on a substrate, and irradiated with a 500W high-pressure mercury lamp at a distance of 30cm to cure into a 6mm polymer film.
[0032] Example 1
[0033] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 50% of bisphenol A epoxy resin, 21% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 25% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0034] The manufacturer of fluorine-modified acrylic acid is Foshan Ona Polymer Co., Ltd., and the name and model are fluorine-modified acrylic leveling agent F370A.
[0035] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0036] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0037] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0038] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0039] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0040] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0041] Example 2
[0042] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 50% of bisphenol A epoxy resin, 26% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0043] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0044] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0045] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0046] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value (pH) of 5, obtain alcohol-modified epoxy carbamate, and store in a brown bottle.
[0047] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0048] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0049] Example 3
[0050] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 50% of bisphenol A epoxy resin, 31% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 15% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0051] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0052] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0053] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0054] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0055] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0056] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0057] Example 4
[0058] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 40% of bisphenol A epoxy resin, 36% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0059] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0060] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0061] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0062] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0063] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0064] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0065] Example 5
[0066] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 30% of bisphenol A epoxy resin, 46% of alcohol-modified epoxy urethane, 3% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 18% of polyamide, 1.5% of polydimethylsilyl ether, 1% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0067] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0068] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0069] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0070] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0071] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0072] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0073] Example 6
[0074] A time-controllable ultraviolet curing system consists of the following components by mass percentage: 66% of bisphenol A epoxy resin, 10% of alcohol-modified epoxy urethane, 2% of benzil dimethyl ketal, 20% of polyamide, 1% of polydimethylsiloxane, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0075] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0076] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0077] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0078] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0079] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0080] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0081] Example 7
[0082] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 16% of bisphenol A epoxy resin, 60% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0083] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0084] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0085] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0086] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0087] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the amount is 0.04%, and the catalyst is dodecylbenzylmethylamine, the amount is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200ml of 95% by mass ethanol.
[0088] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0089] Example 8
[0090] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 40% of bisphenol A epoxy resin, 36% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0091] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0092] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 85°C, and react for 2 hours to obtain a mixed solution a;
[0093] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 100°C, react for 3 hours, and obtain a mixed solution b;
[0094] Step ③: slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 110°C, react for 2 hours, adjust with an ethanol solution of NaOH to an acid value of 5, obtain alcohol-modified epoxy carbamate, and store in a brown bottle.
[0095] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.05%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.5%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0096] The viscosity of the alcohol-modified epoxy urethane is 250 cp (60° C.).
[0097] Example 9
[0098] A time-controllable ultraviolet curing system is composed of the following components by mass percentage: 46% of bisphenol A epoxy resin, 30% of alcohol-modified epoxy urethane, 1% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 21.3% of phthalic anhydride, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.2% of dimethylaniline.
[0099] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0100] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 75°C, and react for 1 hour to obtain a mixed solution a;
[0101] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 85°C, react for 2h, and obtain a mixed solution b;
[0102] Step ③: slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 100°C, react for 1 hour, adjust with an ethanol solution of NaOH to an acid value of 4, obtain alcohol-modified epoxy carbamate, and store in a brown bottle.
[0103] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.02%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.2%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0104] The viscosity of the alcohol-modified epoxy urethane is 230 cp (60° C.).
[0105] Example 10
[0106] A time-controllable ultraviolet light curing system is composed of the following components by mass percentage: 31% of bisphenol A epoxy resin, 45% of alcohol-modified epoxy urethane, 3% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 17.5% of polyamide, 1.5% of polydimethylsilyl ether, 1% of fluorine-modified acrylic acid and 1% of cobalt naphthenate.
[0107] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0108] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0109] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0110] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 6, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0111] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the amount is 0.04%, and the catalyst is dodecylbenzylmethylamine, the amount is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200ml of 95% by mass ethanol.
[0112] The viscosity of the alcohol-modified epoxy urethane is 240 cp (60° C.).
[0113] Comparative Example 1
[0114] A UV curing system consists of the following components by mass percentage: 66% of bisphenol A epoxy resin, 10% of epoxy carbamate, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0115] Comparative Example 2
[0116] A UV curing system consists of the following components by mass percentage: 66% of bisphenol A epoxy resin, 10% of acid-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0117] Wherein, the acid-modified epoxy carbamate is obtained by the following steps:
[0118] Step ①: Mix appropriate amounts of epoxy resin and dimer fatty acid, control the temperature to 80°C, react for 1.5 hours, and obtain a mixed solution a;
[0119] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0120] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, obtain an acid-modified epoxy carbamate, and store it in a brown bottle.
[0121] Among them, in step ①, the mass ratio of epoxy resin to dimer fatty acid is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g NaOH solid in 200mL of 95% by mass ethanol.
[0122] The viscosity of the acid-modified epoxy urethane is 425 cp (60° C.).
[0123] Comparative Example 3
[0124] A UV curing system consists of the following components by mass percentage: 40% of bisphenol A epoxy resin, 36% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0125] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0126] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 60°C, and react for 0.5h to obtain a mixed solution a;
[0127] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 80°C, react for 1 hour, and obtain a mixed solution b;
[0128] Step ③: slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 90°C, react for 0.5h, adjust with an ethanol solution of NaOH to an acid value of 3, obtain alcohol-modified epoxy carbamate, and store in a brown bottle.
[0129] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.01%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.1%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0130] The viscosity of the alcohol-modified epoxy urethane is 355 cp (60° C.).
[0131] Comparative Example 4
[0132] A UV curing system consists of the following components by mass percentage: 40% of bisphenol A epoxy resin, 36% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0133] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0134] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 90°C, and react for 3 hours to obtain a mixed solution a;
[0135] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 110°C, react for 2.5 hours, and obtain a mixed solution b;
[0136] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 120°C, react for 3 hours, adjust with an ethanol solution of NaOH to an acid value of 7, obtain alcohol-modified epoxy carbamate, and store in a brown bottle.
[0137] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.07%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.7%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0138] The viscosity of the alcohol-modified epoxy urethane is 370 cp (60° C.).
[0139] Comparative Example 5
[0140] A UV curing system consists of the following components by mass percentage: 10% of bisphenol A epoxy resin, 66% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0141] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0142] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0143] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0144] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0145] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0146] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0147] Comparative Example 6
[0148] A UV curing system consists of the following components by mass percentage: 71% of bisphenol A epoxy resin, 5% of alcohol-modified epoxy urethane, 2% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 20% of polyamide, 1% of polydimethylsilyl ether, 0.5% of fluorine-modified acrylic acid and 0.5% of cobalt naphthenate.
[0149] Wherein, the alcohol-modified epoxy carbamate is obtained by the following steps:
[0150] Step ①: Mix appropriate amounts of epoxy resin and triethylene glycol, control the temperature to 80°C, and react for 1.5 hours to obtain a mixed solution a;
[0151] Step ②: Add a certain amount of inhibitor and catalyst to the mixed solution a, stir evenly, heat to 95°C, react for 2.5 hours, and obtain a mixed solution b;
[0152] Step ③: Slowly add a certain amount of carbamic acid to the mixed solution b, maintain the reaction temperature at 105°C, react for 1.5 hours, adjust with an ethanol solution of NaOH to an acid value of 5, and obtain alcohol-modified epoxy carbamate, which is stored in a brown bottle.
[0153] Among them, in step ①, the mass ratio of epoxy resin to triethylene glycol is 0.2:1; in step ②, the inhibitor is hydroquinone, the dosage is 0.04%, and the catalyst is dodecylbenzylmethylamine, the dosage is controlled at 0.4%; in step ③, the optimal ratio of the amount of carbamic acid to epoxy group is 1.05:1, and the ethanol solution of NaOH is prepared by dissolving 2g of NaOH solid in 200mL of 95% by mass ethanol.
[0154] The viscosity of the alcohol-modified epoxy urethane is 235 cp (60° C.).
[0155] The performance test of Shore hardness was carried out in accordance with GB / T 2411-2008; the performance test of Barcol hardness was carried out in accordance with GB / T 3854-2017; the curing time was determined by the finger touch method in accordance with GB / T1728-2020; the performance of flexural strength was determined in accordance with GB / T 2567-2021; the viscosity was determined by Brookfield RVDL-II+ viscometer.
[0156] The performance test results of Examples 1 to 10 and Comparative Examples 1 to 6 are compared in Table 1 below.
[0157] Table 1 Performance test results
[0158]
[0159] Example 1-Example 10 is a time-controllable UV curing system provided by the present invention. Comparative Examples 1-Example 2 do not use an active regulator, while Comparative Examples 3-Example 4 change the preparation conditions of the active regulator alcohol-modified epoxy urethane, and the amount of active regulator used in Comparative Examples 5-Example 6 is not within the specified range. It can be seen from the performance test results that compared with the examples, the comparative examples have decreased in many performance indicators, and the overall adjustable range of curing time is not wide. It is found from Examples 1-Example 5 that the curing time of the UV curing system decreases with the increase of alcohol-modified epoxy urethane, and the curing efficiency is getting faster and faster. When the amount of alcohol-modified epoxy urethane added is from 10% to 60%, the curing time is gradually shortened from 13s to 6s. The technical solution provided by the present invention can solve the problems of uncontrollable UV curing time and unstable curing efficiency. At the same time, based on the controllability of the curing time, it is applied to the field of non-excavation underground pipeline repair, and can achieve the problem of matching the formula of the UV curing system with the amount of paint used, the efficiency of photocuring non-excavation pipeline repair, the amount of fiber laying, etc., which is beneficial to on-site construction. The technical solution of the present invention can also be applied to fields such as photocuring coatings.
[0160] It should be understood that in order to streamline the present disclosure and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, various features of the present invention are sometimes grouped together into a single embodiment or description thereof. More specifically, as the claims reflect, inventive aspects lie in less than all of the features of the previously disclosed embodiments. Therefore, the claims following the detailed description are hereby expressly incorporated into this detailed description, with each claim standing on its own as a separate embodiment of the present invention.
[0161] Although the present invention has been described according to a limited number of embodiments, it will be apparent to those skilled in the art, with the benefit of the above description, that other embodiments may be envisioned within the scope of the invention thus described. In addition, it should be noted that the language used in this specification is selected primarily for readability and teaching purposes, rather than for explaining or defining the subject matter of the present invention. Therefore, many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the appended claims. The disclosure of the present invention is illustrative, not restrictive, with respect to the scope of the present invention, which is defined by the appended claims.
[0162] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A time-controllable UV curing system, characterized in that: The composition is as follows by mass percentage: base resin 16~66%, alcohol-modified epoxy urethane 10~60%, photoinitiator 1~3%, cross-linking agent 15~25%, defoamer 0.5~1.5%, leveling agent 0.5~1% and accelerator 0.2~1%; Alcohol-modified epoxy urethane is used as an active regulator, which is photoactive and low-viscosity, with a viscosity range of 230~250cp at 60℃; the curing time of the UV-curing system decreases with the increase of alcohol-modified epoxy urethane, and the curing efficiency becomes faster and faster; The alcohol-modified epoxy urethane is obtained by the following steps: Step 1: Mix epoxy resin and triethylene glycol in a mass ratio of 0.2:1, control the temperature to 75-85°C, react for 1-2 hours, and obtain a mixed solution a; Step 2: Adding a polymerization inhibitor hydroquinone equivalent to 0.02-0.05% of the weight of the mixed solution a and a catalyst dodecylbenzylmethylamine equivalent to 0.2-0.5% of the weight of the mixed solution a to the mixed solution a, stirring evenly, heating to 85-100° C., reacting for 2-3 hours, and obtaining a mixed solution b; Step 3: Add carbamic acid to the mixed solution b, the molar ratio of carbamic acid to epoxy resin is 1.05:1, maintain the reaction temperature at 100-110°C, react for 1-2 hours, adjust the acid value to 4-6 with an ethanol solution of NaOH, and obtain alcohol-modified epoxy carbamate, which is sealed and stored.
2. A time-controllable UV curing system according to claim 1, characterized in that: The composition is composed of the following components by mass percentage: 46-66% base resin, 10-30% alcohol-modified epoxy urethane, 1-3% photoinitiator, 15-25% cross-linking agent, 0.5-1.5% defoamer, 0.5-1% leveling agent and 0.2-1% accelerator.
3. The time-controllable UV curing system according to claim 1, characterized in that: The composition is composed of the following components by mass percentage: 31-46% base resin, 30-45% alcohol-modified epoxy urethane, 1-3% photoinitiator, 15-25% cross-linking agent, 0.5-1.5% defoaming agent, 0.5-1% leveling agent and 0.2-1% accelerator.
4. The time-controllable UV curing system according to claim 1, characterized in that: The composition is composed of the following components by mass percentage: 16-31% base resin, 45-60% alcohol-modified epoxy urethane, 1-3% photoinitiator, 15-25% cross-linking agent, 0.5-1.5% defoamer, 0.5-1% leveling agent and 0.2-1% accelerator.
5. The time-controllable UV curing system according to claim 1, characterized in that: The base resin includes one of bisphenol A epoxy resin, butyl acrylate, and polyphenol glycidyl ether epoxy resin; the photoinitiator includes one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and benzil dimethyl ketal; the crosslinking agent includes one of polyamide, phthalic anhydride, maleic anhydride, and pyromellitic anhydride; the defoaming agent includes polydimethylsilyl ether; the leveling agent includes fluorine-modified acrylic acid; and the accelerator includes one of cobalt cyclohexaneate and dimethylaniline.
6. The time-controllable UV curing system according to claim 1, characterized in that: The preparation method of NaOH ethanol solution is as follows: 2g NaOH solid is dissolved in 200mL 95% by mass ethanol.
7. The method for preparing a time-controllable ultraviolet curing system according to any one of claims 1 to 5, characterized in that: The following steps are involved: S01, adding a photoinitiator to the alcohol-modified epoxy urethane, and shaking and stirring to obtain a uniformly dispersed mixed solution A; S02, adding an accelerator and a cross-linking agent to a base resin, mixing them evenly, and then sequentially adding a defoamer and a leveling agent, mixing them evenly to obtain a mixture B; S03, mixing the mixed solution A and the mixed solution B evenly, coating the mixed solution on a substrate, and irradiating the substrate with a 500W high pressure mercury lamp to solidify the mixed solution into a polymer film with a thickness of 6 mm.
8. Use of a time-controllable ultraviolet curing system according to any one of claims 1 to 5 in trenchless repair of underground pipelines.
9. Use of a time-controllable ultraviolet light curing system according to any one of claims 1 to 5 as a light-curing coating.