A method for producing non-chemically cross-linked ecological beach sheep fur

Through the combined treatment of sodium aluminum silicate non-metallic salts and water-repellent materials, the problems of harmful pollution and biodegradability in the tanning of tan sheepskin are solved, the low shrinkage temperature and good biodegradation performance of the skin board are achieved, and the ecological and environmental protection requirements are met. Complete degradation within 90 days under soil landfill conditions.

CN116855645BActive Publication Date: 2024-10-15NINGXIA YANG DOCTOR FUR TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310687544.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-12
Publication Date
2024-10-15
Estimated Expiration
2043-06-12

AI Technical Summary

Technical Problem

The existing tanning method of tan sheepskin has problems with the emission of harmful pollutants, ecological safety and biodegradability, and it is difficult to control the moisture of the skin collagen fibers, which affects the softness and whiteness of the skin.

Method used

The skin collagen fibers are coated with pre-treatment and high-performance water-repellent materials based on sodium aluminum silicate non-metal salts to achieve temporary dispersion and moisture retention, to avoid excessive water loss or water absorption of the skin collagen fibers, and use non-chemical cross-linking technology Improve the biodegradability of leather panels.

Benefits of technology

It achieves low shrinkage temperature, good biodegradability and softness of the skin board, meets ecological and environmental protection requirements, and achieves complete biodegradation within 90 days under soil landfill conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for making non-chemically cross-linked ecological beach sheep fur, comprising pretreatment, acid softening, pre-dispersion treatment of skin collagen fibers, water-repellent treatment and fixed rinsing steps, wherein the key lies in the pre-dispersion treatment of skin collagen fibers and the water-repellent treatment steps. On the basis of realizing temporary dispersion of collagen fibers in a leather plate, the skin collagen fibers are coated with high-performance water-repellent materials, which, on the one hand, improve the dispersion state of the skin collagen fibers, and on the other hand, improve the moisture retention or resistance of the skin collagen fibers, thereby preventing the skin collagen fibers from excessively losing water when drying or excessively absorbing water in a humid environment, thereby causing problems such as mutual adhesion between skin collagen fibers, reduced softness of the leather plate, and water absorption and decay of the leather plate, thereby improving the quality of the beach sheep fur.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of wool and leather tanning, and relates to a method for making non-chemically cross-linked ecological beach sheep fur. Background Art

[0002] Tan sheepskin, also known as two-hair fur, is a unique fur variety in my country. It is world-renowned for its spike-shaped and naturally curved fur and pure white fur. Traditional Tan sheepskin is mostly tanned with formaldehyde or formaldehyde-aluminum salt. Although it can obtain good softness and whiteness, there is a problem of serious excessive free formaldehyde, which will have an adverse effect on consumer health. There is also a method of combining aldehyde and chrome tanning. The leather obtained by this method has good heat stability, and the shrinkage temperature of the leather can reach above 90°C, which is conducive to improving the storage and service life of Tan sheepskin, and it is easy to dye the fur to obtain colors that satisfy consumers and enrich the variety of colors. However, the fur products obtained by chrome tanning are not convenient for further processing after their life cycle ends, and they are also difficult to degrade naturally. For example, Ding Shaolan et al. found through an 81-day soil burial experiment that fresh pig skin can be 100% degraded, the degradation rate of salted sheepskin is 50.87%, and the degradation rate of chrome-tanned leather is only 4.55% to 10.71% [Ding Shaolan et al. Study on the biodegradability of different types of leather, Journal of Shaanxi University of Science and Technology, 2013, 31(5): 35-38]. At the same time, chrome tanning will cause chromium compounds to be contained in the product, and there is also the problem of discharge of chromium-containing waste liquid. Its product safety and process environmental friendliness need to be improved.

[0003] In the article "Why do we choose natural fur?" published by the International Fur Federation (IFF) on August 19, 2020, the first reason mentioned is that natural fur can be "biodegraded". According to the biodegradation test of natural fur and artificial fur conducted by the Organic Waste System Biodegradation Laboratory in Ghent, Belgium, it was found that after three months of landfilling in the soil, the natural fur was basically completely degraded, indicating that natural fur is biodegradable. Of course, this mainly refers to fur products obtained by aluminum-oil tanning or aldehyde-oil tanning. However, oil tanning of beach sheepskin, such as tanning with kicking oil, will cause severe yellowing of the wool, which will affect the whiteness and natural color of the beach sheepskin. Moreover, the long and curved beach sheepskin wool is very easy to cause hair knotting when tanned with kicking oil. At the same time, the existing method of tanning beach sheepskin also has the problem of difficult control of moisture in the skin collagen fibers. For example, it is easy to cause the skin collagen fibers to lose moisture during drying, causing the skin collagen fibers to stick together, reducing the softness of the leather board. For example, when in an environment with a certain humidity, the skin collagen fibers are prone to absorb moisture in the air, which will not only cause the skin collagen fibers to stick together and reduce the softness of the leather board, but also cause the skin collagen fibers to rot and deteriorate over a long period of time.

[0004] Therefore, there is an urgent need to develop a tanning method that is more in line with ecological and environmental protection requirements and can improve the quality of Tan sheepskin, so as to eliminate the problem of harmful pollutant emissions in the tanning process and the ecological safety of the end products from the source, improve the biodegradability of the tanned Tan sheepskin, and solve the problem that the water content of the skin collagen fibers is difficult to control and the tanning process has an adverse effect on the whiteness of the wool. Summary of the invention

[0005] In view of the shortcomings of the existing tanning methods of Tan sheepskin, such as chrome tanning causing the emission of harmful pollutants, problems with the safety and biodegradability of the tanned Tan sheepskin, oil tanning reducing the whiteness of the Tan sheepskin wool, and the existing methods easily causing the adhesion of the collagen fiber bundles of the Tan sheepskin, reducing the softness of the leather board, and the problem of collagen fiber water absorption, the present invention provides a method for producing non-chemically cross-linked ecological Tan sheepskin, so as to improve the biodegradability of the Tan sheepskin and the quality of the Tan sheepskin on the basis of eliminating the problem of harmful pollutant emissions in the tanning process and the ecological safety problem of the end product from the source.

[0006] In order to achieve the above-mentioned invention purpose, the technical concept adopted by the present invention is mainly: based on the pretreatment of sodium aluminum silicate non-metallic salt under appropriate regulation to achieve temporary dispersion of collagen fibers in the leather board, and then using high-performance water-repellent materials to achieve temporary dispersion of the skin collagen fibers, the skin collagen fibers are "coated" to improve the dispersion state of the skin collagen fibers on the one hand, and on the other hand, to improve the skin collagen fibers' ability to retain or resist moisture, to avoid excessive water loss when drying or excessive water absorption in a humid environment, thereby causing the skin collagen fibers to adhere to each other, reduce the softness of the leather board, and the leather board to absorb water and rot, thereby improving the quality of the beach wool blank. At the same time, the present invention does not rely on tanning agents that can cause chemical cross-linking of the skin collagen fibers, so the collagen fibers in the leather board are in a non-chemically cross-linked state, which is conducive to improving the biodegradability of the leather board, thereby better meeting ecological and environmental protection requirements. The technical scheme adopted by the present invention is as follows:

[0007] A method for making non-chemically cross-linked ecological beach sheep fur comprises the following steps:

[0008] (1) Pretreatment

[0009] The salt-dried Tan sheep skin is soaked, washed, degreased and fleshed to obtain the pre-treated Tan sheep skin;

[0010] (2) Acid softening

[0011] Add water to the scratching trough at a ratio of 10 to 15 L of water per piece of beach sheep skin, add sodium chloride to 6 to 6.5° Be', put the pretreated beach sheep skin into the scratching trough, add fatliquor to a concentration of 0.5 to 1.5 g / L, scratch the trough for 20 to 40 minutes, add formic acid to a pH of the bathing liquid of 4.2 to 4.5, scratch the trough for 20 to 40 minutes, add acid protease to a concentration of 1.6 to 3.0 g / L, scratch the trough for 60 to 90 minutes, add formic acid to a concentration of 4 to 5 g / L, scratch the trough for 20 to 40 minutes, then add sulfuric acid to a pH of the bathing liquid of 2.2 to 2.5, scratch the trough intermittently for 10 to 14 hours, and remove the skin; in this step, the temperature of the bathing liquid is controlled at 25 to 32°C;

[0012] (3) Pre-dispersion treatment of skin collagen fibers

[0013] Add water to the trough at a ratio of 10 to 15 L of water per piece of beach sheep skin, add sodium chloride to 6 to 6.5° Be', put the beach sheep skin that has been softened by acid soaking into the trough, add sodium aluminum silicate non-metallic salt to a concentration of 6 to 12 g / L, stroke the trough for 50 to 80 minutes, let it stand for 50 to 80 minutes, continue to stroke the trough for 20 to 40 minutes, let it stand for 20 to 40 minutes, then add baking soda to the trough several times until the pH value of the bath liquid reaches 4.5 to 4.7, let it stand for 10 to 14 hours, remove the skin, and let the obtained beach sheep skin stand for 24 to 48 hours to achieve temporary dispersion of the skin collagen fibers; in this step, the temperature of the bath liquid is controlled to be 25 to 35°C;

[0014] (4) Water repellent treatment

[0015] Add water to the trough at a ratio of 10 to 15 L of water per piece of beach sheep skin, put the beach sheep skin treated in step (3) into the trough, add aluminum salt to a concentration of 4 to 8 g / L, add water-repellent material to a concentration of 6 to 12 g / L, and row the trough for 120 to 150 minutes to coat the skin collagen fibers with the water-repellent material, add formic acid to adjust the pH value of the bath liquid to 3.8 to 4.0, remove the skin, and let it stand to control the water; in this step, the temperature of the bath liquid is controlled to be 35 to 40°C; the water-repellent material is a combination of a water-repellent material whose main component is a sulfonated synthetic ester and a water-repellent material whose main component is a silicon-containing compound;

[0016] (5) Fixed rinsing

[0017] Add water to the scratching trough at a ratio of 10 to 15 L of water per piece of beach sheep skin, put the beach sheep skin that has been treated with water repellent into the scratching trough, add sodium aluminum sulfate to a concentration of 1 to 3 g / L, scratch the trough for 30 to 60 minutes, add a hair care agent to a concentration of 1 to 3 g / L, add a hair bleaching agent to a concentration of 1.8 to 3 g / L, scratch the trough for 30 to 60 minutes, wash with water, and remove the skin; in this step, the temperature of the bath liquid is controlled at 30 to 40°C.

[0018] In the above technical solution, the water-repellent material is a combination of SYNCUROL MAX and OMBRELLON 072. Preferably, in step (4), the water-repellent material is added in a mass ratio of SYNCUROL MAX to OMBRELLON 072 of 1:(1-4).

[0019] In the above technical solution, the sodium aluminum silicate non-metallic salt is in powder form. The main purpose of the treatment with the sodium aluminum silicate non-metallic salt is to temporarily disperse the skin collagen fibers, so as to facilitate the subsequent effective coating of the skin collagen fibers with water-repellent materials.

[0020] In the above technical solution, the aluminum salt is at least one of aluminum sulfate, aluminum triformate, and ammonium aluminum sulfate.

[0021] In the above technical scheme, after the fixed rinsing operation in step (5), conventional finishing operations are also included. For example, the beach sheep fur obtained through the fixed rinsing operation in step (5) can be subjected to conventional finishing operations such as drying, hanging washing, skin shoveling and combing.

[0022] In step (2) of the above technical solution, the fatliquor and acid protease may be the fatliquor and acid protease commonly used in conventional fur tanning, for example, the fatliquor may be the fatliquor SYNTHOL MC-K, and the acid protease may be the Wiss softening enzyme ARS.

[0023] In step (5) of the above technical solution, the hair conditioner and hair bleaching agent are the hair conditioners and hair bleaching agents used in conventional fur tanning. For example, the hair conditioner can be Jiaweijia hair conditioner M-60, and the hair bleaching agent can be Jiaweijia bleaching agent F-IN.

[0024] The shrinkage temperature of the skin board of the tan sheep fur prepared by the above technical solution is between 66 and 69°C, that is, the above technical solution can control the shrinkage temperature of the skin board of the tan sheep fur to be below 70°C, which is very beneficial to improving the biodegradability of the tan sheep fur, and can better ensure that the products based on the tan sheep fur are easy to biodegrade after the life cycle ends, and better meet the ecological indicators. The present invention has verified through soil landfill tests that the skin board of the tan sheep fur prepared by the above technical solution can be completely biodegraded within 90 days after being landfilled in the soil under the conditions of room temperature and soil moisture of 60% to 70%.

[0025] Compared with the prior art, the technical solution of the present invention produces the following beneficial technical effects:

[0026] 1. The present invention provides a method for making non-chemically cross-linked ecological beach sheep fur, which is based on the pretreatment of sodium aluminum silicate non-metallic salt under appropriate regulation to achieve temporary dispersion of collagen fibers in the leather board, and then the leather collagen fibers are "coated" on the basis of achieving temporary dispersion of the leather collagen fibers using high-performance water-repellent materials, on the one hand, the dispersion state of the leather collagen fibers is improved, and on the other hand, the moisture retention or resistance of the leather collagen fibers is improved, so as to avoid excessive water loss of the leather collagen fibers during drying, resulting in adhesion of the leather collagen fibers, or the skin collagen fibers absorbing water and causing adhesion of the skin collagen fibers, thereby reducing the softness of the leather board or the leather board rotting due to water absorption. The various reagents and additives used in the present invention do not contain harmful metals such as chromium, which can eliminate the pollutant emission problem of the tanning process and the ecological safety problem of the terminal product from the source. At the same time, the present invention does not rely on tanning agents that can cause chemical cross-linking of the leather collagen fibers, so the collagen fibers in the leather board are in a non-chemically cross-linked state, which is conducive to improving the biodegradability of the leather board. The product finally prepared by the method of the present invention can maintain good whiteness of the wool after slight rinsing without dyeing, and the heat stability of the leather board can be controlled within a lower range (shrinkage temperature is lower than 70°C), which makes the product easy to biodegrade after its life cycle and can better meet the requirements of ecological protection.

[0027] 2. The present invention has confirmed through soil landfill test that the skin of the beach sheep skin prepared by the method of the present invention can be completely biodegraded within 90 days after soil landfill under the conditions of room temperature and soil moisture of 60% to 70%, and has excellent biodegradability.

[0028] 3. The non-chemically cross-linked ecological beach sheep fur prepared by the method of the present invention has a white fur color and is free of stains, and the leather board has good softness, is easy to sand, and has uniform fluff, which can improve the sensory quality and performance of the product. Specific implementation methods

[0029] The following examples further illustrate the method for making a non-chemically cross-linked ecological beach sheep fur provided by the present invention. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The technical personnel in the relevant field can make some non-essential improvements and adjustments to the present invention based on the above invention content, which still fall within the scope of protection of the present invention.

[0030] In the following embodiments, the commercial reagents such as soaking aids, scouring agents, degreasing agents, bactericides, fatliquors, acid proteases, non-metallic salt tanning agents, water-repellent materials, hair care agents, hair bleaching agents, and aluminum tanning agents used are all commercial products on the market and can be directly purchased from the market, for example:

[0031] The soaking aid SPH is Daweilan SPH soaking aid, the shampoo DOWELLAN SWA is Daweilan SWA wetting and dispersing aid, and the degreasing agent DOWELLAN FG-C is Daweilan FG-C non-ionic degreasing agent, all of which are commercial products of Sichuan Dawei Technology Co., Ltd. The acidic protease Weisi softening enzyme ARS, aluminum sulfate, aluminum triformate, ammonium aluminum sulfate, Weijia hair care agent M-60, Weijia bleaching agent F-IN, etc. are all commercial products of Beijing Fanbo Technology Co., Ltd. The main component of the fatliquor Synthol MC-K is phosphorylated synthetic oil. The sodium aluminum silicate non-metallic salt is a commercial product of Langfang Guangshan Fine Chemical Co., Ltd. The main component of the water-repellent material SYNCUROL MAX is a sulfonated synthetic ester, and the main component of the water-repellent material OMBRELLON 072 is a silicon-containing polymer, both of which are commercial products of Zschimmer & Schwarz (Sima, Germany).

[0032] Example 1

[0033] In this embodiment, a method for making non-chemically cross-linked ecological beach sheep fur is provided, and the specific steps are as follows:

[0034] (1) Pretreatment

[0035] The salt-dried Tan sheep skin is subjected to soaking, washing, degreasing and fleshing operations to obtain the pre-treated Tan sheep skin, as follows:

[0036] ① Soaking: add water to the trough at the ratio of 15L for each beach sheep skin, put the salt-dried beach sheep skin into the trough, add soaking aid SPH to a concentration of 0.5g / L, soak at room temperature for 8h, take out the skin, and row the trough intermittently during the soaking period; control the temperature of the bath liquid at 20℃.

[0037] ② Wool washing: add water to the trough at the ratio of 15L of water to each beach sheep skin, put the soaked beach sheep skin into the trough, add scourer DOWELLAN SWA to a concentration of 1g / L, add degreasing agent DOWELLAN FG-C to a concentration of 1g / L, add soda ash to a concentration of 0.6g / L, slide the trough for 60min, at this time the pH value of the bath in the trough is 8.5, take out the skin, and then comb the hair to remove the dirt on the hair cover; control the temperature of the bath liquid at 36-38℃.

[0038] ③ Degreasing and fleshing: add water to the paddle trough at a ratio of 15L per piece of beach sheep skin, put the washed beach sheep skin into the paddle trough, add the soaking aid SPH to a concentration of 0.5g / L, add the degreasing agent LIPIDOL DA112 to a concentration of 1.2g / L, paddle the paddle trough for 60 minutes, then paddle the paddle trough intermittently for 14 hours in a manner of continuous paddle troughing for 5 minutes every 2 hours, and remove the skin; control the temperature of the bath liquid to 25℃. Mechanically flesh the obtained beach sheep skin to remove the subcutaneous meat membrane.

[0039] (2) Acid softening

[0040] Add water to the scratching trough at a ratio of 12L of water per piece of beach sheep skin, add sodium chloride to 6-6.5°Be', put the pretreated beach sheep skin into the scratching trough, add fatliquor Synthol MC-K to a concentration of 1.0g / L, scratch in the trough for 40min, add formic acid to the pH of the bath liquid to 4.2-4.5, scratch in the trough for 20min, add acid protease (Weiss softening enzyme ARS, enzyme activity 1200 units) to a concentration of 1.6g / L, scratch in the trough for 60min, add formic acid to a concentration of 5g / L, scratch in the trough for 30min, then add sulfuric acid to the pH of the bath liquid to 2.2-2.5, and then scratch intermittently for 12h with continuous scratching for 2min every 2h to remove the skin; in this step, the temperature of the bath liquid is controlled to be 25°C.

[0041] (3) Pre-dispersion treatment of skin collagen fibers

[0042] Add water to the scratching trough at a ratio of 12L of water per beach sheep skin, add sodium chloride to 6-6.5°Be', put the beach sheep skin that has been softened by acid soaking into the scratching trough, add sodium aluminum silicate non-metallic salt to a concentration of 8g / L, scratch the trough for 60min, let it stand for 60min, continue to scratch the trough for 30min, let it stand for 30min, then add baking soda to the scratching trough 4 times with an interval of 30min each time until the pH value of the bath liquid reaches 4.5-4.7, let it stand for 12h, remove the skin, and let the obtained beach sheep skin stand for 24h to achieve temporary dispersion of the skin collagen fibers; in this step, the temperature of the bath liquid is controlled to be 30°C.

[0043] (4) Water repellent treatment

[0044] Add water to the rowing trough at the ratio of 12L of water to each beach sheep skin, put the tanned beach sheep skin into the rowing trough, add aluminum triformate to a concentration of 5g / L, row the trough for 45 minutes, add water-repellent material SYNCUROL MAX to a concentration of 5g / L, add water-repellent material OMBRELLON 072 to a concentration of 8g / L, row the trough for 150 minutes to cover the skin collagen fibers with the water-repellent materials, add formic acid to adjust the pH value of the bath liquid to 3.8-4.0, remove the skin, and let it stand to control the water; in this step, the temperature of the bath liquid is controlled to 32°C.

[0045] (5) Fixed rinsing

[0046] Add water to the scratching trough at the ratio of 10L of water to each piece of beach sheep skin, put the beach sheep skin that has been treated with water repellent into the scratching trough, add sodium aluminum sulfate to the concentration of 1g / L, scratch in the trough for 45 minutes, add Weijia hair care agent M-60 to the concentration of 1g / L, add Weijia bleaching agent F-IN to the concentration of 2g / L, scratch in the trough for 45 minutes, wash with water, and remove the skin; in this step, the temperature of the bath liquid is controlled at 40°C.

[0047] The beach sheep fur that has been fixedly rinsed in step (5) is subjected to post-finishing processes such as drying, hanging washing, shoveling, combing, etc. according to conventional processes to obtain the beach sheep fur.

[0048] The fur of the beach sheepskin prepared in this embodiment is white and free of stains. After the post-finishing process, the skin of the beach sheepskin has good softness, and there is no problem of excessive loss of moisture due to drying, which causes the skin fibers to stick together and reduces the dispersion of the skin fibers, resulting in reduced softness of the skin. The beach sheepskin does not contain chromium and formaldehyde. After shrinkage temperature detection, it was found that the shrinkage temperature of the skin is about 68°C. Under room temperature and soil humidity of 60% to 70%, it was found through soil landfill tests that the skin can be completely biodegraded within 90 days.

[0049] Comparative Example 1

[0050] The operation of this comparative example is basically the same as that of Example 1, except that no water-repellent material is added in step (4).

[0051] The wool of the beach sheep skin obtained by tanning in this comparative example is pure white and free of stains. After the same post-finishing process as in Example 1, it is found that the beach sheep skin loses moisture seriously during the drying process, and the problems of skin fiber adhesion and reduced skin fiber dispersion occur. The softness of the skin board of the beach sheep skin obtained in this comparative example is significantly lower than that of Example 1.

[0052] Comparative Example 2

[0053] The operation of this comparative example is basically the same as that of Example 1, except that the water-repellent material in step (4) is replaced by the fatliquor SYNTHOL FL327, and the concentration of the fatliquor SYNTHOL FL327 in the bath liquid is 13 g / L.

[0054] The wool of the beach sheep skin obtained by tanning in this comparative example is white and free of stains. After the same post-finishing process as in Example 1, it is found that the beach sheep skin loses moisture excessively during the drying process, resulting in the problem of skin fiber adhesion and reduced skin fiber dispersion. The softness of the skin board of the beach sheep skin obtained in this comparative example is significantly lower than that of Example 1.

[0055] Comparative Example 3

[0056] In this comparative example, the shrinkage temperature of the lamb fur leather prepared in Example 1 of CN115216565A was tested and found to be greater than 85° C. Under the conditions of room temperature and soil humidity of 60% to 70% (the same conditions as in Example 1), it was found through a soil landfill test that the leather could only achieve partial biodegradation within 90 days, and it would take at least 120 days to achieve complete biodegradation.

[0057] Example 2

[0058] In this embodiment, a method for making non-chemically cross-linked ecological beach sheep fur is provided, and the specific steps are as follows:

[0059] (1) Pretreatment

[0060] The salt-dried Tan sheep skin is soaked, washed, degreased and fleshed to obtain a pretreated Tan sheep skin. The specific operation is the same as step (1) of Example 1.

[0061] (2) Acid softening

[0062] Add water to the scratching trough at the ratio of 12L of water to each beach sheep skin, add sodium chloride to a concentration of 55g / L, put the pretreated beach sheep skin into the scratching trough, add the fatliquor Synthol MC-K to a concentration of 0.8g / L, scratch in the trough for 20min, add formic acid to the pH of the bath solution to 4.2-4.5, scratch in the trough for 40min, add acid protease (Weiss softening enzyme ARS, enzyme activity 1200 units) to a concentration of 1.6g / L, scratch in the trough for 40min, add formic acid to a concentration of 5g / L, scratch in the trough for 40min, then add sulfuric acid to the pH of the bath solution to 2.2-2.5, and then scratch intermittently for 14h with continuous scratching for 2min every 2h to remove the skin; in this step, the temperature of the bath solution is controlled to be 28°C.

[0063] (3) Pre-dispersion treatment of skin collagen fibers

[0064] Add water to the scratching trough at the ratio of 14L of water to each beach sheep skin, put the beach sheep skin that has been softened by acid soaking into the scratching trough, add sodium aluminum silicate non-metallic salt to a concentration of 12g / L, scratch the trough for 80 minutes, let it stand for 80 minutes, continue to scratch the trough for 20 minutes, let it stand for 20 minutes, then add baking soda to the scratching trough 4 times with an interval of 30 minutes each time until the pH value of the bath liquid reaches 4.5-4.7, let it stand for 14 hours, remove the skin, and let the obtained beach sheep skin stand for 48 hours to achieve temporary dispersion of the skin collagen fibers; in this step, the temperature of the bath liquid is controlled to be 28°C.

[0065] (4) Water repellent treatment

[0066] Add water to the rowing trough at the ratio of 14 L of water to each beach sheep skin, put the tanned beach sheep skin into the rowing trough, add aluminum sulfate to a concentration of 8 g / L, row the trough for 60 minutes, add water-repellent material SYNCUROL MAX to a concentration of 5 g / L, add water-repellent material OMBRELLON 072 to a concentration of 6 g / L, row the trough for 120 minutes to cover the skin collagen fibers with the water-repellent material, add formic acid to adjust the pH value of the bath liquid to 3.8-4.0, take out the skin, and let it stand to control the water; in this step, the temperature of the bath liquid is controlled to 35°C.

[0067] (5) Fixed rinsing

[0068] Add water to the scratching trough at the ratio of 12L of water to each piece of beach sheep skin, put the beach sheep skin that has been treated with water repellent into the scratching trough, add sodium aluminum sulfate to the concentration of 1.5g / L, scratch in the trough for 30 minutes, add Weijia hair care agent M-60 to the concentration of 1.5g / L, add Weijia bleaching agent F-IN to the concentration of 2.5g / L, scratch in the trough for 50 minutes, wash with water, and remove the skin; in this step, the temperature of the bath liquid is controlled at 35°C.

[0069] The beach sheep fur that has been fixedly rinsed in step (5) is subjected to post-finishing processes such as drying, hanging washing, shoveling, combing, etc. according to conventional processes to obtain white ecological beach sheep fur.

[0070] The white eco-Tan sheepskin prepared in this example has a pure white color and no stains, and the leather is soft and has good resistance to moisture in the air, which can effectively prevent the leather fibers from absorbing moisture in the air, thereby avoiding rotting and deterioration due to moisture absorption by the leather fibers. The white eco-Tan sheepskin does not contain chromium and formaldehyde. After shrinkage temperature detection, it was found that the shrinkage temperature of the leather was about 69°C. The soil landfill test was carried out under the same experimental conditions as in Example 1, and it was found that the leather could be completely biodegraded within 90 days.

[0071] Example 3

[0072] In this embodiment, a method for making non-chemically cross-linked ecological beach sheep fur is provided, and the specific steps are as follows:

[0073] (1) Pretreatment

[0074] The salt-dried Tan sheep skin is soaked, washed, degreased and fleshed to obtain a pretreated Tan sheep skin. The specific operation is the same as step (1) of Example 1.

[0075] (2) Acid softening

[0076] Add water to the scratching trough at the ratio of adding 10L of water to each beach sheep skin, add sodium chloride to the concentration of 45g / L, put the pretreated beach sheep skin into the scratching trough, add the fatliquor Synthol MC-K to the concentration of 1.3g / L, scratch in the trough for 30min, add formic acid to the pH of the bath liquid to 4.2-4.5, scratch in the trough for 30min, add acid protease (Weiss softening enzyme ARS, enzyme activity 1200 units) to the concentration of 1.8g / L, scratch in the trough for 45min, add formic acid to the concentration of 4g / L, scratch in the trough for 20min, then add sulfuric acid to the pH of the bath liquid to 2.2-2.5, and then scratch intermittently for 10h with continuous scratching for 2min every 2h to remove the skin; in this step, the temperature of the bath liquid is controlled to 26°C.

[0077] (3) Pre-dispersion of collagen fibers: Add water to the trough at a ratio of 10 L of water per piece of beach sheep skin. Put the beach sheep skin that has been softened by acid soaking into the trough, add non-metallic sodium aluminum silicate to a concentration of 6 g / L, stroke the trough for 50 min, let it stand for 50 min, continue to stroke the trough for 40 min, let it stand for 40 min, then add baking soda to the trough 4 times with an interval of 30 min each time until the pH value of the bath liquid reaches 4.5-4.7, let it stand for 10 h, remove the skin, and let the obtained beach sheep skin stand for 48 h to achieve temporary dispersion of the collagen fibers. In this step, the temperature of the bath liquid is controlled to be 26°C.

[0078] (4) Water repellent treatment

[0079] Add water to the rowing trough at the ratio of adding 10L of water to each beach sheep skin, put the tanned beach sheep skin into the rowing trough, add aluminum triformate to a concentration of 4g / L, row the trough for 80min, add water-repellent material SYNCUROL MAX to a concentration of 2g / L, add water-repellent material OMBRELLON 072 to a concentration of 6g / L, row the trough for 90min to cover the skin collagen fibers with the water-repellent material, add formic acid to adjust the pH value of the bath liquid to 3.8-4.0, take out the skin, and let it stand to control the water; in this step, the temperature of the bath liquid is controlled to 32°C.

[0080] (5) Fixed rinsing

[0081] Add water to the scratching trough at the ratio of 12L of water to each piece of beach sheep skin, put the beach sheep skin that has been treated with water repellent into the scratching trough, add sodium aluminum sulfate to the concentration of 2g / L, scratch in the trough for 60 minutes, add hair protector Weijia Hair Protector M-60 to the concentration of 1.5g / L, add Weijia bleaching agent F-IN to the concentration of 1.8g / L, scratch in the trough for 60 minutes, wash with water, and remove the skin; in this step, the temperature of the bath liquid is controlled at 35°C.

[0082] The beach sheep fur that has been fixedly rinsed in step (5) is subjected to post-finishing processes such as drying, hanging washing, shoveling, combing, etc. according to conventional processes to obtain white ecological beach sheep fur.

[0083] The white eco-Tan sheepskin prepared in this example has a pure white color and no stains, and the leather is soft and good. The leather has good resistance to moisture in the air, which can effectively prevent the leather fibers from absorbing moisture in the air, thereby avoiding rotting and deterioration due to moisture absorption by the leather fibers. The white eco-Tan sheepskin does not contain chromium and formaldehyde. After shrinkage temperature detection, it was found that the shrinkage temperature of the leather was about 68°C. The soil landfill test was carried out under the same experimental conditions as in Example 1, and it was found that the leather could be completely biodegraded within 90 days.

Claims

1. A method for producing non-chemically cross-linked ecological beach sheep fur, characterized in that: The following steps are involved: (1) Preprocessing The salt-dried Tan sheep skin is soaked, washed, degreased and fleshed to obtain the pre-treated Tan sheep skin; (2) Acid softening Add water to the scratching trough at a ratio of 10-15 L of water per piece of beach sheep skin, add sodium chloride to 6-6.5°Be', put the pretreated beach sheep skin into the scratching trough, add fatliquor to a concentration of 0.5-1.5 g / L, scratch the trough for 20-40 min, add formic acid to a pH of the bathing liquid of 4.2-4.5, scratch the trough for 20-40 min, add acid protease to a concentration of 1.6-3.0 g / L, scratch the trough for 60-90 min, add formic acid to a concentration of 4-5 g / L, scratch the trough for 20-40 min, then add sulfuric acid to a pH of the bathing liquid of 2.2-2.5, scratch the trough intermittently for 10-14 h, and remove the skin; in this step, the temperature of the bathing liquid is controlled at 25-32°C; (3) Pre-dispersion treatment of skin collagen fibers Add water to the scratching trough at a ratio of 10-15 L of water per piece of beach sheep skin, add sodium chloride to 6-6.5°Be', put the beach sheep skin that has been softened by acid soaking into the scratching trough, add sodium aluminum silicate non-metallic salt to a concentration of 6-12 g / L, scratch the trough for 50-80 min, let it stand for 50-80 min, continue to scratch the trough for 20-40 min, let it stand for 20-40 min, then add baking soda to the scratching trough several times until the pH value of the bath liquid reaches 4.5-4.7, let it stand for 10-14 h, remove the skin, and let the obtained beach sheep skin stand for 24-48 h to achieve temporary dispersion of the skin collagen fibers; in this step, the temperature of the bath liquid is controlled to be 25-35 ℃; (4) Water repellent treatment Add water to the trough at a ratio of 10 to 15 L of water per piece of beach sheep skin, put the beach sheep skin treated in step (3) into the trough, add aluminum salt to a concentration of 4 to 8 g / L, add water-repellent material to a concentration of 6 to 12 g / L, row the trough for 120 to 150 minutes to coat the skin collagen fibers with the water-repellent material, add formic acid to adjust the pH value of the bath liquid to 3.8 to 4.0, remove the skin, and let it stand to control the water; in this step, the temperature of the bath liquid is controlled to be 35 to 40°C; the water-repellent material is a combination of a water-repellent material whose main component is a sulfonated synthetic ester and a water-repellent material whose main component is a silicon-containing compound; (5) Fixed rinsing Add water to the scratching trough at a ratio of 10-15 L of water per piece of beach sheep skin, put the beach sheep skin that has been treated with water repellent into the scratching trough, add sodium aluminum sulfate to a concentration of 1-3 g / L, scratch the trough for 30-60 min, add a hair conditioner to a concentration of 1-3 g / L, add a hair bleaching agent to a concentration of 1.8-3 g / L, scratch the trough for 30-60 min, wash with water, and remove the skin; in this step, control the temperature of the bath liquid to be 30-40 °C; The water-repellent material in step (4) is a combination of SYNCUROL MAX and OMBRELLON 072, and the water-repellent material is added in a mass ratio of SYNCUROL MAX to OMBRELLON 072 of 1:(1-4) in step (4); the aluminum salt is at least one of aluminum sulfate, aluminum triformate, and ammonium aluminum sulfate; The shrinkage temperature of the skin board of the beach sheep fur prepared by the method is between 66 and 69°C; the skin board of the beach sheep fur prepared by the method can be completely biodegraded within 90 days after being landfilled in the soil under the conditions of room temperature and soil moisture of 60% to 70%.

2. The method for making the non-chemically cross-linked ecological Tan sheep fur according to claim 1, characterized in that: After the fixed rinsing operation in step (5), a finishing operation is also included.

3. The method for making the non-chemically cross-linked ecological Tan sheep fur according to claim 2, characterized in that: The post-finishing operations include drying, hanging washing, skinning and combing operations.