A low-density, high-toughness, hard ablation-resistant heat-resistant coating and a preparation method thereof
By designing low-density and high-toughness hard ablative heat-proof coatings, high-temperature-resistant modified epoxy resin and multi-functional fillers and other components are used to achieve efficient heat protection and improve appearance quality on the new generation of space-based missiles, solving the current problems There are coating deficiencies in new thermal environments.
Patent Information
- Application Number
- CN202310685793.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-06-09
AI Technical Summary
Existing hard epoxy heat-proof coatings ablate too quickly, have poor shape stability, and have high density in new thermal environments; soft silicone rubber heat-proof coatings have low ablation efficiency, difficult to guarantee appearance quality, and cannot Meet the needs of the new generation of air-based missiles for high heat protection efficiency, lightweight and high appearance quality.
Design a low-density and high-toughness hard ablative heat-proof coating. Through formula design, the coating will undergo a ceramic reaction when heated to form a high-strength ceramic surface layer. It uses high-temperature-resistant and high-toughness modified epoxy resin and multifunctional organic Fillers, reinforcing fibers and insulating fillers, combined with curing agents and adhesion promoters, provide high temperature shear resistance and lightweight properties.
A heat-proof coating with small ablation amount, high heat protection efficiency, high toughness and excellent appearance quality has been realized, which solves the problems of low lightweight, thick coating, easy cracking, delamination, debonding and large ablation amount of existing coatings. As well as the problems of low thermal protection efficiency and poor appearance quality, it is suitable for structural thermal protection of high appearance quality for the new generation of aerospace vehicles.
Smart Images

Figure CN116875189B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low-density, high-toughness, hard ablative heat-resistant coating and a preparation method thereof. The coating can be used for aerodynamic heat protection of the outer surface of a spacecraft and belongs to the technical field of heat-resistant coating materials. Background Art
[0002] The new generation of air-based missile equipment has a faster flight speed and a longer flight distance. Compared with existing equipment, the thermal environment faced by the new generation of missile bodies has also changed significantly, with higher heat flux density and longer heating time. In addition, the new generation of equipment has higher and higher requirements for lightweight and appearance quality of thermal protection coatings. How to achieve high thermal protection efficiency, lightweight and high appearance quality thermal protection technology has become a new common problem.
[0003] Thermal protection coatings prevent aerodynamic heat or combustion heat from being conducted into the material through heat dissipation mechanisms such as heat blocking effect, chemical endothermic effect, and phase change endothermic effect generated at high temperatures. They have the characteristics of excellent heat protection, simple construction process, and low cost. They are the preferred engineering solution for thermal protection of air-based weapons and equipment. Existing ablative thermal protection coatings are mainly divided into two categories. One type is a hard organic thermal protection coating, which is a carbon-based ablative thermal protection coating based on epoxy resin. The appearance quality of this type of coating is generally good, but in a new thermal environment, the ablation rate of this type of thermal protection coating is too fast, the ablation amount is large, and the ablation shape stability is poor, so it is not suitable for long-term thermal protection. This problem can be improved by adding inorganic ceramic powders, but due to the large amount of inorganic ceramic powders added, the coating density is high. For example, the density of existing hard epoxy thermal protection coatings such as TR-48 and TR-28 of the Institute of Aerospace Materials and Technology is both greater than 1.1g / cm 3 . In addition, the existing epoxy-based ablative heat-resistant coating has poor toughness. When applied too thickly or on the surface of thin-walled composite materials with large deformation, it is prone to cracking, delamination and debonding of the material, which greatly reduces the reliability of the coating. Another type of soft organic heat-resistant coating is a silicon-based ablative heat-resistant coating with silicone rubber as the resin matrix. Although it can meet the needs of thermal protection, its ablation efficiency is low, the process performance is relatively poor, and the appearance quality is often difficult to guarantee.
[0004] Therefore, there is an urgent need to develop a low-density, high-toughness, hard ablative thermal protection coating that can achieve effective thermal protection while taking into account high thermal protection efficiency, light weight and high appearance quality, so as to meet the urgent needs of the new generation of air-based missiles for thermal protection of the missile body. It has good application prospects and significant military and social benefits. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art and provide a low-density and high-toughness hard ablative thermal protection coating. Through formula design, the thermal protection coating has excellent thermal protection performance. During the heating process, a ceramic reaction can occur to form a high-strength ceramic surface layer. It has the characteristics of small ablation, high heat protection efficiency and high-temperature shear resistance. The thermal protection coating has high toughness, high lightness and excellent appearance quality. It can effectively solve the problems of low lightness, easy cracking, delamination, debonding and large ablation of existing hard epoxy thermal protection coatings, and low heat protection efficiency and poor appearance quality of soft silicone rubber thermal protection coatings, and provide technical support for the high appearance quality structural thermal protection design of a new generation of aerospace vehicles.
[0006] Another object of the present invention is to provide a method for preparing a low-density, high-toughness, hard ablation-resistant heat-resistant coating.
[0007] The above-mentioned purpose of the present invention is mainly achieved through the following technical solutions:
[0008] A low-density, high-toughness, hard organic heat-resistant coating, wherein the heat-resistant coating is prepared on a substrate by heat-resistant coating, and the raw materials of the heat-resistant coating include component A and component B;
[0009] The component A comprises the following components by weight: 40-70 parts of high temperature resistant and high toughness modified epoxy resin, 15-45 parts of multifunctional organic filler, 5-20 parts of reinforcing fiber, 8-20 parts of heat insulation filler, 10-25 parts of functional additive, and 5-15 parts of diluent;
[0010] The B component includes a curing agent, a curing accelerator and an adhesion promoter, and the mass ratio of the curing agent, the curing accelerator and the adhesion promoter is 35-55:0.5-3:0.5-3.
[0011] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the high-temperature resistant and high-toughness modified epoxy resin includes: 20 to 60 parts of silicone-modified epoxy resin S1, 30 to 70 parts of silicone-modified epoxy resin S2, and 5 to 15 parts of phenolic epoxy resin.
[0012] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the preparation method of the organosilicon-modified epoxy resin S1 comprises:
[0013] Add 10-20 parts of diallyl bisphenol A glycidyl ether and 5-35 parts of catalyst into a reaction kettle equipped with a thermometer and a condensation reflux device, stir at room temperature for more than 15 minutes under the protection of a nitrogen atmosphere until the mixture is uniformly mixed, and then heat to 60-90°C;
[0014] Add dropwise a mixture of 10 to 30 parts of methyl-terminated hydrogen-containing silicone oil and toluene solvent. After the addition is complete, continue the reaction for more than 3 hours.
[0015] The residual solvent is removed under reduced pressure to obtain the organosilicon-modified epoxy resin.
[0016] Among them, the molecular structure of diallyl bisphenol A glycidyl ether is shown in the following formula:
[0017]
[0018] The molecular structure of methyl-terminated hydrogen silicone oil is shown below:
[0019]
[0020] Among them, the hydrogen content is 0.1-0.4%;
[0021] The catalyst is 5ppm to 20ppm platinum catalyst diluted with toluene.
[0022] In the above-mentioned low-density, high-toughness hard organic heat-resistant coating, the organic modified epoxy resin S2 is EPSI-3266X silicone-modified epoxy resin; the phenolic epoxy resin is one or a combination of Nan Ya F51, ARALDITE 8250 or Huntsman EPALLOY 8240.
[0023] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the multifunctional organic filler is an organic polymer powder, the organic polymer powder is lignin, or a combination of lignin and any one or two of polyphosphide silicon resin or boron phenolic resin powder, and the powder particle size is 75 to 250 microns.
[0024] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the reinforcing fiber is one or a combination of alkali-free glass fiber, high-silica fiber, carbon fiber or para-aramid fiber; the length of the reinforcing fiber is 2 to 8 mm.
[0025] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, when the reinforcing fiber is carbon fiber, it needs to be pretreated, and the pretreatment method is:
[0026] Soak the carbon fiber in distilled water for 2-6 hours, then dry it, and heat it in an oven at 115-125°C for 3-8 hours to dry it;
[0027] Place the treated fiber in a container, add concentrated nitric acid with a mass concentration of 65-70%, heat under reflux in a water bath for more than 4 hours, and after cooling, wash the fiber with distilled water until it is neutral;
[0028] Heat in an oven at 115-125℃ for 3-8 hours and dry for later use.
[0029] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the heat-insulating filler is one or a combination of hollow glass microspheres and hollow phenolic microspheres; the particle size of the hollow filler is 30-60 microns, and the density is 0.15-0.4 g / cm 3 .
[0030] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, when the thermal filler is hollow glass microspheres, pretreatment is required, and the pretreatment method includes:
[0031] The hollow microbeads were first washed with dilute hydrochloric acid, then rinsed with deionized water and dried at 100-120°C for 2-4h;
[0032] Add the prepared ethanol solution of KH550 with a mass ratio of 1:1 or the ethanol solution of KH560 with a mass ratio of 1:1 to the dried hollow microspheres, stir evenly, and heat at 60-80°C for 4-6 hours for use.
[0033] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the functional additives include a heat-resistant agent and a rheological agent, wherein the heat-resistant agent is ASIBO-R806CT, the rheological agent is hydrophobic silica, the specific surface area is ≥150 mg, and the pH value is 6-8; the diluent is one or a combination of butyl acetate, ethyl acetate or acetone.
[0034] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the preparation method of the curing agent in the B component includes:
[0035] Weigh 5 to 35 parts of amino silicone resin with an amine hydrogen equivalent of 200 to 300, 20 to 50 parts of modified polyamide with an amine hydrogen equivalent of 200 to 300, and 0.5 to 4.5 parts of multifunctional epoxy resin AG-80;
[0036] First, add amino silicone resin and modified polyamide into the container, heat to 60-100℃ under nitrogen protection, and stir evenly at 300-600r / min;
[0037] Slowly and evenly add multifunctional epoxy resin into the container and continue the reaction for 1 to 3 hours to obtain a curing agent.
[0038] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the curing accelerator in the B component is 2,4,6-tris(dimethylaminomethyl)phenol; the adhesion promoter is any one or a combination of Evonik Dynasylan@1189 or Dynasylan@1505.
[0039] In the above-mentioned low-density, high-toughness, hard organic heat-resistant coating, the ratio of the component A to the component B is determined by the epoxy equivalent of the epoxy resin: the amine hydrogen equivalent of the curing agent = 1 to 1.2:1.
[0040] The method for preparing the low-density, high-toughness, hard organic heat-resistant coating comprises:
[0041] (1) mixing and uniformly dispersing a high temperature resistant and high toughness modified epoxy resin, a multifunctional filler, a reinforcing fiber, a thermal insulation filler, a functional additive and a diluent according to a proportion to obtain a component A;
[0042] (2) Mix the curing agent, curing accelerator and adhesion promoter according to the proportion and stir evenly to obtain component B;
[0043] (3) Component A is diluted with a diluent. The ratio of component A to component B is prepared according to the epoxy equivalent of epoxy resin: amine hydrogen equivalent of curing agent = 1 to 1.2:1. After mixing evenly, ripen for 30 to 90 minutes, and then evenly apply it on the surface of the substrate.
[0044] In the method for preparing the low-density, high-toughness, hard organic heat-resistant coating, when the spray coating is performed in step (3), the single spraying thickness is controlled to be 100 to 200 μm, and the interval between each spraying is 30 to 90 minutes;
[0045] When using the scraping method for coating, the single scraping thickness is controlled to be 200-300um, and the interval between each scraping is 30-60min;
[0046] The coating curing system is room temperature curing for more than 72 hours, or heating at 60-80℃ for more than 8 hours.
[0047] A low-density, high-toughness, hard organic heat-resistant coating, the raw materials of which include component A and component B;
[0048] The component A comprises the following components by weight: 40-70 parts of high temperature resistant and high toughness modified epoxy resin, 15-45 parts of multifunctional organic filler, 5-20 parts of reinforcing fiber, 8-20 parts of thermal insulation filler, 10-25 parts of functional additives, and 5-15 parts of diluent;
[0049] The B component includes a curing agent, a curing accelerator and an adhesion promoter, and the mass ratio of the curing agent, the curing accelerator and the adhesion promoter is 35-55:0.5-3:0.5-3.
[0050] Compared with the prior art, the present invention has at least the following beneficial effects:
[0051] (1) The present invention designs a low-density, high-toughness, hard ablative thermal protection coating. The formula design makes the thermal protection coating have excellent thermal protection performance. During the heating process, a ceramic reaction can occur to form a high-strength ceramic surface layer. The coating has the characteristics of small ablation, high thermal protection efficiency, and high-temperature shear resistance. In addition, the hard thermal protection coating has high toughness, high lightness, and excellent appearance quality. It can effectively solve the problems of existing hard epoxy thermal protection coatings such as low lightness, easy cracking, delamination, debonding, and large ablation due to thick coating, and low thermal protection efficiency and poor appearance quality of soft silicone rubber thermal protection coatings, and provide technical support for the high-appearance quality structural thermal protection design of a new generation of aerospace vehicles.
[0052] (2) The heat-resistant coating in the embodiment of the present invention uses a new modified epoxy resin as a matrix, which combines the advantages of both epoxy resin and silicone, and has the characteristics of high temperature resistance, high toughness and high residual carbon. By introducing organic multifunctional fillers, the surface of the heat-resistant coating is ceramicized after ablation, which effectively improves the coating ablation shape stability and long-term thermal protection performance, while taking into account lightweight performance. By reinforcing the design of functional components such as fiber and thermal insulation fillers, the heat-resistant coating has both high heat protection efficiency and appearance quality, which can meet the urgent needs of the new generation of air-based missiles for thermal protection of the missile body.
[0053] (3) The resin matrix prepared by the present invention has the advantages of high carbon residue and high toughness. The carbon residue of the resin matrix at 800°C is greater than 20%, and the elongation at break is greater than 60%. Studies have shown that only when the carbon residue is greater than 20% and the curing agent is used in combination, can it work synergistically with multifunctional organic fillers, hollow microspheres and other components to enable the heat-resistant coating to obtain excellent ablation strength and ablation appearance smoothness.
[0054] (4) The hard heat-resistant coating in the embodiment of the present invention has the characteristic of high lightness, and the density of the heat-resistant coating is 0.60-0.70 g / cm 3 . The reasons for achieving low density are: ① The present invention uses an organic multifunctional filler with low density to replace the commonly used ceramic inorganic fillers with high density such as mica powder, talcum powder, zinc borate, etc., for example, an organic polymer powder including lignin, or a combination of lignin and any one of polyphosphide silicone resin or boron phenolic resin powder, ② The toughness of the coating decreases with the increase of lightweight hollow fillers. Since the resin prepared by the present invention has the characteristics of high toughness, more lightweight hollow fillers can be added compared with the resin matrix with poor toughness while ensuring that the coating has a certain mechanical strength and elongation at break. ③ In general, the introduction of hollow microspheres will greatly reduce the mechanical properties of the coating. The present invention can fill part of the hollow microspheres in a porous structure constructed by fibers and organic powders through the reasonable combination of organic powder fillers, fiber fillers and hollow microsphere sizes, thereby effectively reducing the influence of hollow microspheres on the mechanical properties of the coating.
[0055] (5) Compared with the traditional epoxy resin-based hard organic heat-resistant coating, the heat-resistant coating of the present invention has a higher ablation thermal efficiency per unit surface weight under the action of aerodynamic heating. This is because the heat-resistant coating prepared by the present invention has a low density and uses an organic multifunctional filler that can undergo pyrolysis in a high-temperature environment to replace the inorganic ceramic filler, which effectively improves the ability of the heat-resistant material to dissipate aerodynamic heat through mass loss.
[0056] (6) After the ablative heat-resistant coating provided by the present invention is applied to the surface of the product, in a non-flight service environment, the coating has high toughness (elongation at break>10%), which effectively reduces the risk of cracking, delamination and substrate debonding of the coating. In a flight environment, the components such as the silicone-modified epoxy resin matrix, functional organic powder, and hollow microspheres in the coating work synergistically, and the coating can form a ceramic layer with a certain strength during the ablation process, and the ablation dimensional performance is excellent.
[0057] (7) The resin matrix of the heat-resistant coating of the present invention contains a variety of polar groups and highly active epoxy groups. At the same time, an adhesion promoter is added to the formula, so that the coating has excellent adhesion on the surfaces of various substrates such as steel, aluminum alloy, titanium alloy, carbon epoxy composite materials, etc. The application substrate has a wide range of applicability and can be used for the outer surface of the body and engine structure of air-based missile weapons.
[0058] (8) The ablative thermal protection coating provided by the present invention has better ablation efficiency, mechanical properties, substrate adhesion performance and appearance quality than traditional soft silicone rubber-based thermal protection coatings. The thermal protection coating of the present invention is designed through thermal protection mechanism, coordinated design of coating resin matrix structure and multifunctional filler components, and screening and optimization research. The coating has high thermal protection efficiency, light weight and appearance quality on the basis of meeting the thermal protection performance, providing technical support for the structural thermal protection design of the new generation of air-based missile weapons. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 This is a coating state diagram after the quartz lamp ablation test of the heat-resistant coating in Example 1 of the present invention;
[0060] Figure 2 This is an infrared image of the organosilicon-modified epoxy resin provided in Example 1 of the present invention;
[0061] Figure 3 This is the thermal weight loss diagram of the high temperature resistant and high toughness modified epoxy resin provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0062] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0063] The present invention provides a low-density, high-toughness, hard ablative heat-resistant coating, which is formed by coating the heat-resistant coating on a substrate. The raw materials of the heat-resistant coating include a heat-resistant coating component A and a heat-resistant coating component B. Component A includes the following components in parts by mass: 100 parts of high-temperature resistant and high-toughness modified epoxy resin, 35 to 50 parts of multifunctional organic filler, 15 to 35 parts of reinforcing fiber, 5 to 15 parts of heat-insulating filler, 5 to 20 parts of functional additives, and 5 to 15 parts of diluent; Component B includes a curing agent, a curing accelerator and an adhesion promoter, and the mass ratio of the curing agent, the curing accelerator and the adhesion promoter is 35 to 55: 0.5 to 3: 0.5 to 3.
[0064] In an optional embodiment, the high temperature resistant and high toughness modified epoxy resin includes 20 to 60 parts of silicone modified epoxy resin S1, 30 to 70 parts of silicone modified epoxy resin S2, and 5 to 15 parts of phenolic epoxy resin.
[0065] The silicone-modified epoxy resin S1 was prepared as follows:
[0066] ① Weigh diallyl bisphenol A glycidyl ether, methyl-terminated hydrogen-containing silicone oil and a catalyst, wherein the molar ratio of active hydrogen to vinyl can be 20 to 100:100.
[0067] The molecular structure of diallyl bisphenol A glycidyl ether is shown below:
[0068]
[0069] The methyl-terminated hydrogen-containing silicone oil is a methyl-terminated hydrogen-containing silicone oil or a side methyl-terminated hydrogen-containing silicone oil. Preferably, the methyl-terminated hydrogen-containing silicone oil has a molecular structure as shown below:
[0070]
[0071] Among them, the hydrogen content is 0.1-0.4%;
[0072] The catalyst is 5ppm to 20ppm platinum catalyst diluted with toluene.
[0073] ② Add 10-20 parts of diallyl bisphenol A glycidyl ether and 5-35 parts of catalyst weighed in step 1 to a reaction kettle equipped with a thermometer and a condensation reflux device, and stir at room temperature for more than 15 minutes under the protection of a nitrogen atmosphere until the mixture is evenly mixed, and then heat to 60-90°C. Under this condition, drop a mixture of 10-30 parts of methyl-terminated hydrogenated silicone oil and a certain amount of toluene solvent. After the dropwise addition is completed, continue the reaction for more than 3 hours. Finally, remove the residual solvent under reduced pressure to obtain a silicone-modified epoxy resin.
[0074] In an optional embodiment, the organic modified epoxy resin S2 is a complex high-tech material EPSI-3266X, wherein the phenolic epoxy resin is one or a combination of Nan Ya F51, ARALDITE 8250, and Huntsman EPALLOY 8240.
[0075] In an optional embodiment, the multifunctional organic filler is an organic polymer powder, which has the functions of flame retardancy and auxiliary porcelain formation in the resin system. The multifunctional organic filler is an organic polymer powder, and the organic polymer powder is lignin, or lignin + polyphosphide silicon resin, or lignin + boron phenolic resin, or lignin + polyphosphide silicon resin + boron phenolic resin, and the particle size of the above powder is 75 to 250 microns.
[0076] In an optional embodiment, the reinforcing fiber is one or a combination of alkali-free glass fiber, high silica fiber, carbon fiber or para-aramid fiber. The fiber length is 2 to 8 mm. Carbon fiber needs to be pretreated when used. The pretreatment method is: soak the carbon fiber in distilled water for 2-6 hours, then dry it, and heat it in a 120°C oven for 3-8 hours to dry. Put the treated fiber in a container, add a certain amount of 65-70% concentrated nitric acid (200-300ml / L), and heat it in a water bath for reflux for more than 4 hours. After cooling, wash the fiber with distilled water until it is neutral. Finally, heat it in a 120±5°C oven for 3 to 8 hours to dry it for use.
[0077] In an optional embodiment, the heat insulating filler is one or a combination of hollow glass microspheres and hollow phenolic microspheres. The particle size of the hollow filler is 30-60 microns and the density is 0.15-0.4 g / cm 3 . Hollow glass microspheres need to be pretreated when used. The pretreatment method is: wash the hollow microspheres with dilute hydrochloric acid, rinse with deionized water, and dry at 100-120℃ for 2-4h. Add a certain proportion of the prepared KH550 or KH560 ethanol solution (mass ratio 1:1) to the dried hollow microspheres, stir evenly, and heat at 60-80℃ for 4-6h for use.
[0078] In an optional embodiment, the functional additives include a heat resistant agent and a rheological agent. The heat resistant agent is ASIBO-R806CT. The rheological agent is white carbon black (specific surface area ≥ 150 mg, pH value 6-8). The diluent is one or a combination of butyl acetate, ethyl acetate or acetone.
[0079] In an optional embodiment, the raw material curing agent of component B of the heat-resistant coating is prepared by the following method:
[0080] Weigh 5-35 parts of amino silicone resin, 20-50 parts of modified polyamide and 0.5-4.5 parts of multifunctional epoxy resin by weight; first add the amino silicone resin and polyamide into a container, heat to 60-100°C under nitrogen protection, and stir evenly at 300-600r / min.
[0081] Slowly and evenly add multifunctional epoxy resin into the container and continue the reaction for 1 to 3 hours to obtain a curing agent.
[0082] The curing accelerator is 2,4,6-tris(dimethylaminomethyl)phenol. The adhesion accelerator is any one or a combination of Evonik's Dynasylan@1189 and Dynasylan@1505.
[0083] The method for preparing the above-mentioned low-density, high-toughness, hard organic heat-resistant coating comprises the following steps:
[0084] (1) Mix and evenly disperse the high temperature resistant and high toughness modified epoxy resin, multifunctional filler, reinforcing fiber, thermal insulation filler, functional additive and diluent to obtain heat resistant coating component A. The mass ratio of each component is: 40-70 parts of high temperature resistant and high toughness modified epoxy resin, 15-45 parts of multifunctional organic filler, 5-20 parts of reinforcing fiber, 8-20 parts of thermal insulation filler, 10-25 parts of functional additive and 5-15 parts of diluent;
[0085] (2) The curing agent, curing accelerator and adhesion promoter are mixed in a mass ratio of 35-55:0.5-3:0.5-3, and stirred evenly to obtain a heat-resistant coating component B:
[0086] (3) Use a diluent to dilute the heat-resistant coating component A. The heat-resistant coating component A and the heat-resistant coating component B are prepared in a ratio of epoxy equivalent of epoxy resin: amine hydrogen equivalent of curing agent = 1 to 1.2:1, mixed evenly, aged for 30 to 90 minutes, and then evenly applied to the surface of the substrate. The amount of diluent can be adjusted according to different coating methods.
[0087] When spraying is used in step (3), the single spraying thickness is controlled to be 100-200 um, and the interval between each spraying is 30-90 minutes; when scraping is used, the single scraping thickness is controlled to be 200-300 um, and the interval between each spraying is 30-60 minutes. The coating curing system is room temperature curing for more than 72 hours, or heating at 60-80°C for more than 8 hours.
[0088] Example 1
[0089] The raw materials of component A of the heat-resistant coating include the following components in parts by mass: 55 parts of high-temperature resistant and high-toughness modified epoxy resin, 30 parts of multifunctional organic filler, 15 parts of reinforcing fiber, 15 parts of thermal insulation filler, 11.5 parts of functional additives, and 12 parts of diluent; the raw materials of component B of the heat-resistant coating include curing agent, curing accelerator and adhesion promoter, including 45 parts of curing agent, 1.5 parts of curing accelerator, and 1.0 part of adhesion promoter.
[0090] In the above heat-resistant coating, the high-temperature-resistant and high-toughness modified epoxy resin is composed of 10 parts of silicone-modified epoxy resin S1, 45 parts of silicone-modified epoxy resin S2, and 5 parts of phenolic epoxy resin.
[0091] (1) The organosilicon-modified epoxy resin S1 is prepared according to the following method:
[0092] Weigh diallyl bisphenol A glycidyl ether, methyl-terminated hydrogen-containing silicone oil and catalyst in sequence. The molar ratio of active hydrogen to vinyl is 40:100. The methyl-terminated hydrogen-containing silicone oil has a hydrogen content of 0.11-0.15%. The catalyst is 10ppm platinum catalyst.
[0093] Diallyl bisphenol A glycidyl ether and catalyst were added to a reaction kettle equipped with a thermometer and a condensation reflux device. Under the protection of nitrogen atmosphere, the mixture was stirred at room temperature for more than 15 minutes until it was evenly mixed, and then the temperature was raised to 80°C. Under this condition, a mixture of methyl-terminated hydrogen-containing silicone oil and some toluene solvent was added dropwise. After the addition was completed, the reaction was continued for 8 hours. Finally, the residual solvent was removed under reduced pressure to obtain the organosilicon-modified epoxy resin S1.
[0094] In the above heat-resistant coating, 30 parts of multifunctional organic fillers include 30 parts of 100-150 micron lignin powder, 15 parts of reinforcing fibers including 5 parts of high-silica fibers and 10 parts of carbon fibers, 5 parts of phenolic hollow microspheres and 10 parts of glass hollow microspheres as heat-insulating fillers, and 11.5 parts of functional additives including 10 parts of hydrophobic white carbon black and 1.5 parts of heat-resistant agents. When lignin powder is used as a multifunctional organic filler, it can work synergistically with the resin matrix, hollow microspheres, etc., and form a carbon layer with stable structure and excellent mechanical properties after ablation.
[0095] In the above heat-resistant coating, the curing agent is 45 parts. The curing agent is prepared by the following method: weigh 8 parts of amino silicone resin (amine hydrogen equivalent 230-250), 45 parts of modified polyamide (amine hydrogen equivalent 220-240) and 1.0 part of multifunctional epoxy resin AG-80. First, add the amino silicone resin and polyamide into the container, heat to 75°C under nitrogen protection, and stir evenly at 300-600r / min. Slowly and evenly add the multifunctional epoxy resin to the container, continue to react for 3 hours, and obtain the curing agent. The curing accelerator is 2,4,6-tris(dimethylaminomethyl)phenol. The adhesion promoter is Dynasylan@1189.
[0096] like Figure 1 The figure shows the coating state after the quartz lamp ablation test of the heat-resistant coating in Example 1 of the present invention. Environment 1: 110kw / m 2 , the total heating time is 65s, the coating surface after ablation is relatively smooth, not powdery, no receding ablation, the surface is ceramicized, and the ablation dimension is good (Figure a). Environment 2: 400kw / m 2 The total heating time is 45s. After ablation, the coating surface is relatively smooth, not powdery, without receding ablation, the surface is ceramicized, and the ablation dimension is good (Figure b). Figure 2 The infrared image of the organosilicon-modified epoxy resin provided in Example 1 of the present invention is shown; Figure 3 Shown is the thermal weight loss diagram of the high temperature resistant and high toughness modified epoxy resin provided in Example 1 of the present invention.
[0097] Example 2
[0098] The raw materials of component A of the heat-resistant coating include the following components in parts by mass: 55 parts of high-temperature resistant and high-toughness modified epoxy resin, 25 parts of multifunctional organic filler, 10 parts of reinforcing fiber, 10 parts of thermal insulation filler, 16 parts of functional additives, and 15 parts of diluent: The raw materials of component B of the heat-resistant coating include curing agent, curing accelerator and adhesion promoter, including 40 parts of mixed amine curing agent, 1.0 part of curing accelerator, and 1.5 parts of adhesion promoter.
[0099] In the above heat-resistant coating, the high-temperature-resistant and high-toughness modified epoxy resin is composed of 12 parts of silicone-modified epoxy resin S1, 43 parts of silicone-modified epoxy resin S2, and 5 parts of phenolic epoxy resin.
[0100] (1) The organosilicon-modified epoxy resin is prepared by the following method:
[0101] Weigh diallyl bisphenol A glycidyl ether, methyl-terminated hydrogen-containing silicone oil and catalyst in sequence. The molar ratio of active hydrogen to vinyl is 60:100. The methyl-terminated hydrogen-containing silicone oil has a hydrogen content of 0.17-0.20%. The catalyst is 8ppm platinum catalyst.
[0102] Add diallyl bisphenol A glycidyl ether and catalyst into a reaction flask equipped with a thermometer and a condensation reflux device. Stir at room temperature for more than 15 minutes under the protection of nitrogen atmosphere until the mixture is evenly mixed, and then heat to 75°C. Under this condition, drop a mixture of methyl-terminated hydrogen-containing silicone oil and some toluene solvent. After the dropwise addition is completed, continue the reaction for 6 hours. Finally, remove the residual solvent under reduced pressure to obtain a silicone-modified epoxy resin.
[0103] In the above-mentioned heat-resistant coating, 25 parts of multifunctional organic fillers include 5 parts of 100-150 micron phosphide silicone resin powder, 10 parts of 100-150 micron lignin powder, and 10 parts of 100-150 micron boron phenolic powder; 10 parts of reinforcing fibers include 10 parts of carbon fibers; the heat-insulating filler includes 10 parts of hollow glass microspheres; 16 parts of the functional additives include 15 parts of hydrophobic silica and 1.0 part of a heat-resistant agent.
[0104] In the above heat-resistant coating, there are 40 parts of curing agent. The curing agent is prepared by the following method: weigh 18 parts of amino silicone resin (amine hydrogen equivalent 250-270), 48 parts of modified polyamide (amine hydrogen equivalent 220-240) and 1.0 part of multifunctional epoxy resin AG-80. First, add amino silicone resin and polyamide into the container, heat to 80°C under nitrogen protection, and stir evenly at 300-600r / min. Slowly and evenly add multifunctional epoxy resin to the container, continue to react for 2h, and obtain curing agent. The curing accelerator is 2,4,6-tris(dimethylaminomethyl)phenol. The adhesion promoter is Dynasylan@1505.
[0105] Example 3
[0106] The raw materials of component A of the heat-resistant coating include the following components in parts by mass: 55 parts of high-temperature resistant and high-toughness modified epoxy resin, 20 parts of multifunctional organic filler, 15 parts of reinforcing fiber, 10 parts of thermal insulation filler, 21.5 parts of functional additives, and 14 parts of diluent; the raw materials of component B of the heat-resistant coating include a mixed amine curing agent, a curing accelerator and an adhesion promoter, including 46 parts of the curing agent, 1.0 parts of the curing accelerator, and 1.5 parts of the adhesion promoter.
[0107] In the above heat-resistant coating, the high-temperature-resistant and high-toughness modified epoxy resin is composed of 13 parts of silicone-modified epoxy resin S1, 42 parts of silicone-modified epoxy resin S2, and 5 parts of phenolic epoxy resin.
[0108] (1) The organosilicon-modified epoxy resin is prepared by the following method:
[0109] Weigh diallyl bisphenol A glycidyl ether, methyl-terminated hydrogen-containing silicone oil and catalyst in sequence. The molar ratio of active hydrogen to vinyl is 50:100. The hydrogen content of the methyl-terminated hydrogen-containing silicone oil is 0-22-0.30%. The catalyst is 12ppm platinum gold catalyst.
[0110] Add diallyl bisphenol A glycidyl ether and catalyst into a reaction flask equipped with a thermometer and a condensation reflux device. Stir at room temperature for more than 15 minutes under the protection of nitrogen atmosphere until the mixture is evenly mixed, and then heat to 85°C. Under this condition, drop a mixture of methyl-terminated hydrogen-containing silicone oil and some toluene solvent. After the dropwise addition is completed, continue the reaction for 5 hours. Finally, reduce the pressure to remove the residual solvent to obtain a silicone-modified epoxy resin.
[0111] In the above-mentioned heat-resistant coating, 20 parts of multifunctional organic fillers include 5 parts of 100-150 micron lignin powder and 15 parts of 100-150 micron boron phenolic powder; 15 parts of reinforcing fibers include 5 parts of carbon fibers and 10 parts of glass fibers; the heat-insulating fillers include 10 parts of hollow microspheres, including 10 parts of glass hollow microspheres; the functional additives include 21.5 parts of hydrophobic silica and 1.5 parts of heat-resistant agents.
[0112] In the above heat-resistant coating, there are 46 parts of curing agent. The curing agent is prepared by the following method: weigh 14 parts of amino silicone resin (amine hydrogen equivalent 230-250), 40 parts of modified polyamide (amine hydrogen equivalent 220-240) and 1.2 parts of multifunctional epoxy resin AG-80. First, add amino silicone resin and polyamide into the container, heat to 75°C under nitrogen protection, and stir evenly at 300-600r / min. Slowly and evenly add multifunctional epoxy resin to the container, continue to react for 3 hours, and obtain the curing agent. The curing accelerator is 2,4,6-tris(dimethylaminomethyl)phenol. The adhesion promoter is Dynasylan@1189.
[0113] Table 1 Coating performance test results in Examples 1 to 3
[0114]
[0115]
[0116] The above description is only the best specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
[0117] The contents not described in detail in the specification of the present invention belong to the common knowledge of the professionals in this field.
Claims
1. A low-density, high-toughness, hard organic heat-resistant coating, characterized in that: The heat-resistant coating is formed by preparing a heat-resistant coating on a substrate, and the raw materials of the heat-resistant coating include component A and component B; The component A comprises the following components by weight: 40-70 parts of high temperature resistant and high toughness modified epoxy resin, 15-45 parts of multifunctional organic filler, 5-20 parts of reinforcing fiber, 8-20 parts of heat insulation filler, 10-25 parts of functional additive, and 5-15 parts of diluent; The B component includes a curing agent, a curing accelerator and an adhesion promoter, and the mass ratio of the curing agent, the curing accelerator and the adhesion promoter is 35-55:0.5-3:0.5-3; The high temperature resistant and high toughness modified epoxy resin comprises: 20 to 60 parts of organosilicon modified epoxy resin S1, 30 to 70 parts of organosilicon modified epoxy resin S2, and 5 to 15 parts of phenolic epoxy resin; The preparation method of the curing agent in the B component comprises: Weigh 5 to 35 parts of amino silicone resin with an amine hydrogen equivalent of 200 to 300, 20 to 50 parts of modified polyamide with an amine hydrogen equivalent of 200 to 300, and 0.5 to 4.5 parts of multifunctional epoxy resin AG-80; First, add amino silicone resin and modified polyamide into the container, heat to 60-100℃ under nitrogen protection, and stir evenly at 300-600r / min; Slowly and evenly add multifunctional epoxy resin to the container and continue the reaction for 1 to 3 hours to obtain a curing agent; The preparation method of the organosilicon-modified epoxy resin S1 comprises: Add 10-20 parts of diallyl bisphenol A glycidyl ether and 5-35 parts of catalyst into a reaction kettle equipped with a thermometer and a condensation reflux device, stir at room temperature for more than 15 minutes under the protection of a nitrogen atmosphere until the mixture is uniformly mixed, and then heat to 60-90°C; Add dropwise a mixture of 10 to 30 parts of methyl-terminated hydrogen-containing silicone oil and toluene solvent. After the addition is complete, continue the reaction for more than 3 hours. The residual solvent is removed under reduced pressure to obtain the organosilicon-modified epoxy resin. Among them, the molecular structure of diallyl bisphenol A glycidyl ether is shown in the following formula: The molecular structure of methyl-terminated hydrogen silicone oil is shown below: Among them, the hydrogen content is 0.1-0.4%; The catalyst is 5ppm to 20ppm platinum catalyst diluted with toluene; The organic modified epoxy resin S2 is EPSI-3266X silicone modified epoxy resin.
2. The low-density, high-toughness, hard organic heat-resistant coating according to claim 1, characterized in that: The phenolic epoxy resin is one or a combination of Nan Ya F51, ARALDITE 8250 or Huntsman EPALLOY 8240.
3. The low-density, high-toughness, hard organic heat-resistant coating according to claim 1, characterized in that: The multifunctional organic filler is an organic polymer powder, the organic polymer powder is lignin, or a combination of lignin and boron phenolic resin powder, and the particle size of the powder is 75 to 250 microns.
4. The low-density, high-toughness, hard organic heat-resistant coating according to claim 1, characterized in that: The reinforcing fiber is one or a combination of alkali-free glass fiber, high-silica fiber, carbon fiber or para-aramid fiber; The length of the reinforcing fiber is 2 to 8 mm.
5. The low-density, high-toughness, hard organic heat-resistant coating according to claim 4, characterized in that: When the reinforcing fiber is carbon fiber, it needs to be pretreated, and the pretreatment method includes: Soak the carbon fiber in distilled water for 2-6 hours, then dry it, and heat it in an oven at 115-125℃ for 3-8 hours to dry it; Place the treated fiber in a container, add concentrated nitric acid with a mass concentration of 65-70%, heat under reflux in a water bath for more than 4 hours, and after cooling, wash the fiber with distilled water until it is neutral; Heat in an oven at 115-125℃ for 3-8 hours and dry for later use.
6. The low-density, high-toughness, hard organic heat-resistant coating according to claim 1, characterized in that: The heat-insulating filler is one or a combination of hollow glass microspheres and hollow phenolic microspheres; The particle size of the thermal insulation filler is 30-60 microns and the density is 0.15-0.4 g / cm 3 .
7. The low-density, high-toughness, hard organic heat-resistant coating according to claim 6, characterized in that: When the heat insulating filler is hollow glass microspheres, pretreatment is required, and the pretreatment method includes: The hollow glass microspheres were first washed with dilute hydrochloric acid, then rinsed with deionized water and dried at 100-120°C for 2-4h; Add the prepared ethanol solution of KH550 with a mass ratio of 1:1 or the ethanol solution of KH560 with a mass ratio of 1:1 into the dried hollow glass microspheres, stir evenly, and heat at 60-80°C for 4-6 hours for use.
8. The low-density, high-toughness, hard organic heat-resistant coating according to claim 1, characterized in that: The functional additives include a heat resistant agent and a rheological agent, wherein the heat resistant agent is ASIBO-R806CT, and the rheological agent is hydrophobic white carbon black, with a specific surface area of ≥150 mg and a pH value of 6-8; The diluent is one or a combination of butyl acetate, ethyl acetate or acetone.
9. The low-density, high-toughness, hard organic heat-resistant coating according to claim 1, characterized in that: The curing accelerator in the B component is 2,4,6-tris(dimethylaminomethyl)phenol; the adhesion promoter is any one or a combination of Evonik Dynasylan@1189 or Dynasylan@1505.
10. The low-density, high-toughness, hard organic heat-resistant coating according to claim 1, characterized in that: The ratio of the component A to the component B is determined by the epoxy equivalent of the epoxy resin: the amine hydrogen equivalent of the curing agent = 1 to 1.2:
1.
11. The method for preparing a low-density, high-toughness, hard organic heat-resistant coating according to any one of claims 1 to 10, characterized in that: include: (1) mixing and uniformly dispersing a high temperature resistant and high toughness modified epoxy resin, a multifunctional filler, a reinforcing fiber, a thermal insulation filler, a functional additive and a diluent according to a proportion to obtain a component A; (2) Mix the curing agent, curing accelerator and adhesion promoter according to the proportion and stir evenly to obtain component B; (3) Component A is diluted with a diluent. The ratio of component A to component B is prepared according to the epoxy equivalent of epoxy resin: amine hydrogen equivalent of curing agent = 1 to 1.2:
1. After mixing evenly, ripen for 30 to 90 minutes, and then evenly apply it on the surface of the substrate.
12. The method for preparing a low-density, high-toughness, hard organic heat-resistant coating according to claim 11, characterized in that: When the spray coating is performed in step (3), the single spraying thickness is controlled to be 100 to 200 μm, and the interval between each spraying is 30 to 90 minutes; When using the scraping method for coating, the single scraping thickness is controlled to be 200-300um, and the interval between each scraping is 30-60min; The coating curing system is room temperature curing for more than 72 hours, or heating at 60-80℃ for more than 8 hours.
13. A low-density, high-toughness, hard organic heat-resistant coating, characterized in that: The raw materials of the heat-resistant coating include component A and component B; The component A comprises the following components by weight: 40-70 parts of high temperature resistant and high toughness modified epoxy resin, 15-45 parts of multifunctional organic filler, 5-20 parts of reinforcing fiber, 8-20 parts of thermal insulation filler, 10-25 parts of functional additives, and 5-15 parts of diluent; The B component includes a curing agent, a curing accelerator and an adhesion promoter, and the mass ratio of the curing agent, the curing accelerator and the adhesion promoter is 35-55:0.5-3:0.5-3; The high temperature resistant and high toughness modified epoxy resin comprises: 20 to 60 parts of organosilicon modified epoxy resin S1, 30 to 70 parts of organosilicon modified epoxy resin S2, and 5 to 15 parts of phenolic epoxy resin; The preparation method of the curing agent in the B component comprises: Weigh 5 to 35 parts of amino silicone resin with an amine hydrogen equivalent of 200 to 300, 20 to 50 parts of modified polyamide with an amine hydrogen equivalent of 200 to 300, and 0.5 to 4.5 parts of multifunctional epoxy resin AG-80; First, add amino silicone resin and modified polyamide into the container, heat to 60-100℃ under nitrogen protection, and stir evenly at 300-600r / min; Slowly and evenly add multifunctional epoxy resin to the container and continue the reaction for 1 to 3 hours to obtain a curing agent; The preparation method of the organosilicon-modified epoxy resin S1 comprises: Add 10-20 parts of diallyl bisphenol A glycidyl ether and 5-35 parts of catalyst into a reaction kettle equipped with a thermometer and a condensation reflux device, stir at room temperature for more than 15 minutes under the protection of a nitrogen atmosphere until the mixture is uniformly mixed, and then heat to 60-90°C; Add dropwise a mixture of 10 to 30 parts of methyl-terminated hydrogen-containing silicone oil and toluene solvent. After the addition is complete, continue the reaction for more than 3 hours. The residual solvent is removed under reduced pressure to obtain the organosilicon-modified epoxy resin. Among them, the molecular structure of diallyl bisphenol A glycidyl ether is shown in the following formula: The molecular structure of methyl-terminated hydrogen silicone oil is shown below: Among them, the hydrogen content is 0.1-0.4%; The catalyst is 5ppm to 20ppm platinum catalyst diluted with toluene; The organic modified epoxy resin S2 is EPSI-3266X silicone modified epoxy resin.