A metal-supported carbon fiber structure catalyst, its preparation method and application
The metal-supported carbon fiber structure catalyst prepared by electrospinning solves the problem of low CO2 adsorption and activation efficiency of existing catalysts, and realizes efficient CO2 capture and in-situ conversion, especially promoting the conversion of CO2 to ethylene products in the electrochemical process.
Patent Information
- Application Number
- CN202310740977.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-21
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-06-21
AI Technical Summary
Existing catalysts are inefficient in CO2 molecule adsorption and activation, resulting in poor CO2 capture and in-situ conversion capabilities, making it difficult to achieve efficient carbon recycling.
Metal-supported carbon-based fiber catalysts were prepared by electrospinning. Polyacrylonitrile and divalent soluble metal salts were mixed and electrospun, followed by calcination in different atmospheres to form a carbon-based fiber structure with uniformly dispersed metal nanoparticles. This resulted in a highly active C=O quinone structure, which enhanced the adsorption and activation capacity of CO2.
It achieves efficient capture and in-situ conversion of CO2, significantly improves the activation and conversion efficiency of CO2, especially promotes CC coupling in the electrochemical process, and optimizes the performance of CO2 conversion into ethylene products.
Smart Images

Figure CN116876009B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst preparation, and particularly relates to a metal-supported carbon fiber structure catalyst, its preparation method, and its application in the process of carbon dioxide capture and conversion. Background Technology
[0002] Electrocatalytic reduction of carbon dioxide (CO2) is a promising carbon-negative technology that uses renewable electricity to electrochemically convert CO2 into high-value-added fuels and chemicals, making it an effective way to achieve carbon recycling. However, the CO2 molecule has a symmetrical carbon-oxygen double bond structure, is extremely thermodynamically stable, has weak interactions with metal surfaces, and is difficult to adsorb and activate, resulting in diverse products and difficulty in controlling product selectivity.
[0003] Patent CN202110872599.8 uses stable Cu as the base metal and a small-molecule organic solvent that acts as both a solvent and an organic ligand to uniformly disperse the transition metal in single-atom form within the Cu nanolattice, forming a single-atom alloy structure with bimetallic active sites. This structure is more conducive to the cleavage of C=C double bonds during the electrocatalytic CO2 reduction process, thereby increasing the CO generation rate. However, due to the difficulty in CO2 molecule adsorption, its selectivity in the electrocatalytic CO2 to CO production is insufficient, resulting in low catalytic efficiency. Therefore, improving the adsorption of CO2 molecules on the metal surface is more beneficial for subsequent CO2 activation and conversion.
[0004] Integrated CO2 capture and conversion technology is rapidly developing as a promising and cost-effective carbon neutralization technology. However, the lack of a long-sought molecular consensus regarding the synergistic effect between adsorption and in-situ catalytic reactions has hindered its development. Therefore, how to construct catalysts that possess both high CO2 capture and in-situ conversion capabilities, synergistically promoting improved system energy efficiency, is a pressing issue in the field of CO2 conversion. Summary of the Invention
[0005] The technical problem to be solved by the present invention is that existing catalysts do not support good adsorption capacity of CO2 molecules on metal surfaces, resulting in low catalytic efficiency and poor CO2 capture and in-situ conversion capabilities. Therefore, there is an urgent need to provide a catalyst with both high CO2 capture and in-situ conversion capabilities.
[0006] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows:
[0007] A method for preparing a metal-supported carbon-based fiber structured catalyst includes the following steps:
[0008] (1) Mix polyacrylonitrile and divalent soluble metal salt in a solvent to obtain an electrospinning solution;
[0009] (2) The electrospinning solution is placed in an electrospinning device for electrospinning, and electrospinning fibers are collected.
[0010] (3) The electrospun fibers are calcined to obtain a metal-supported carbon-based fiber structure catalyst.
[0011] Optionally, in a method for preparing a metal-supported carbon fiber structure catalyst, the divalent soluble metal salt is selected from at least one of soluble copper salt, cobalt salt, nickel salt, and zinc salt.
[0012] Optionally, the divalent soluble metal salt is selected from at least one of the chlorides, nitrates, sulfates or acetates of copper, cobalt, nickel and / or zinc;
[0013] Optionally, the metal nanoparticles formed from the divalent soluble metal salt in a metal-supported carbon-based fiber structure catalyst have a weight percentage of 5%-20%.
[0014] Optionally, in a method for preparing a metal-supported carbon fiber structure catalyst, the mass concentration of the polyacrylonitrile in the electrospinning solution is 8 wt% to 15 wt%.
[0015] Optionally, the solvent is N,N-dimethylformamide.
[0016] Optionally, in a method for preparing a metal-supported carbon fiber structure catalyst, the electrospinning conditions are: temperature of 20℃~40℃, humidity of 15%~35%, feed rate of 0.2-2ml / min, and spinning voltage of 10-20V.
[0017] Optionally, a method for preparing a metal-supported carbon-based fiber structure catalyst further includes: collecting electrospun fibers using aluminum foil at a fixed receiving distance of 12-20 cm, and then drying the collected electrospun fibers at room temperature for 24-72 h.
[0018] Optionally, in a method for preparing a metal-supported carbon fiber structure catalyst, the calcination heating rate is 2℃ / min-10℃ / min, the temperature is 700-1000℃, and the calcination time is 0.1-5h.
[0019] Optionally, the calcination atmosphere is one or a mixture of two of carbon dioxide and argon.
[0020] Optionally, in a method for preparing a metal-supported carbon fiber structure catalyst, the calcination involves first heating to 600℃ at a heating rate of 10℃ / min and holding for 1-2 hours, then heating to 700℃ at a heating rate of 5℃ / min and holding for 0.5-1 hours, and finally calcining to 700-1000℃ at a heating rate of 2℃ / min for 5-10 minutes.
[0021] Optionally, in a method for preparing a metal-supported carbon fiber structure catalyst, the calcination involves first heating to 600°C in an argon atmosphere at a heating rate of 10°C / min and holding for 1-2 hours, then heating to 700°C in a CO2 atmosphere at a heating rate of 5°C / min and holding for 0.5-1 hours, and finally calcining to 700-1000°C in a CO2 atmosphere at a heating rate of 2°C / min for 5-10 minutes.
[0022] The present invention also provides a metal-supported carbon-based fiber structure catalyst, which is prepared by any of the above methods.
[0023] The present invention also provides the application of metal-supported carbon-based fiber structure catalysts in the synergistic electrochemical CO2 capture and in-situ conversion. Optionally, the metal-supported carbon-based fiber structure catalysts can be used to achieve CO2 capture and in-situ conversion through electrocatalysis.
[0024] The above-described solution of the present invention has at least the following beneficial effects:
[0025] (1) The preparation method of the metal-supported carbon fiber structure catalyst provided in the embodiments of the present invention has high universality, is applicable to a variety of metals, has high repeatability, and is conducive to large-scale production.
[0026] (2) The method for preparing the metal-supported carbon fiber structure catalyst provided in the embodiments of the present invention allows for the modification of oxygen-containing groups on the surface of the carbon fiber while preparing the metal-supported carbon fiber structure, thereby achieving preparation and modification in one step and avoiding the complex process of subsequent modification.
[0027] (3) The metal-supported carbon-based fiber structure catalyst provided in the embodiments of the present invention can achieve synergistic electrochemical CO2 capture and in-situ conversion, and has dual functions of CO2 capture and conversion. The highly active C=O quinone structure of the carbon-based fiber structure has excellent carbon capture ability, which can optimize CO2 adsorption and facilitate CO2 capture, significantly enhance CO2 activation, increase the residence time of CO intermediate on Cu surface, promote CC coupling, and show excellent performance in electrochemical CO2 capture and in-situ conversion to prepare ethylene products. Attached Figure Description
[0028] Figure 1 This is a TEM image of Cu@C=O obtained in Example 1 of this invention;
[0029] Figure 2 This is a TEM image of Co@C=O obtained in Example 2 of the present invention.
[0030] Figure 3This is a TEM image of Ni@C=O obtained in Example 3 of the present invention.
[0031] Figure 4 The CO2- adsorption diagrams of Cu@C=O, Cu@C, C=O, and C obtained in Example 1, Comparative Examples 1, 2, and 3 of this invention are shown.
[0032] Figure 5 The image shows the Faraday efficiency distribution of different products C2+ and ethylene obtained by electrochemical CO2 conversion of Cu@C=O prepared in Example 1 of this invention under different current densities. Detailed Implementation
[0033] Exemplary embodiments of the invention will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the invention are shown in the drawings, it should be understood that the invention may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that this invention will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0034] The present invention provides a method for preparing a metal-supported carbon-based fiber structure catalyst, comprising the following steps:
[0035] (1) Mix polyacrylonitrile (PAN) and divalent soluble metal salt in a solvent to obtain an electrospinning solution;
[0036] (2) The electrospinning solution is placed in an electrospinning device for electrospinning, and electrospinning fibers are collected.
[0037] (3) The electrospun fibers are calcined to obtain a metal-supported carbon-based fiber structure catalyst.
[0038] In this embodiment, in step (1), the polyacrylonitrile and the divalent soluble metal salt are mixed evenly in a solvent. The solvent can be selected from N,N-dimethylformamide (DMF). Specifically, PAN is added to a sealed bottle containing the solvent and stirred at room temperature for 24 hours to fully dissolve it. Then, the divalent soluble metal salt is added to the above mixed solution and stirred at room temperature for 24 hours to obtain an electrospinning solution.
[0039] In one optional embodiment, in the method for preparing the metal-supported carbon fiber structure catalyst, the divalent soluble metal salt is selected from at least one of soluble copper salt, cobalt salt, nickel salt, and zinc salt;
[0040] Optionally, the divalent soluble metal salt is selected from at least one of the chlorides, nitrates, sulfates or acetates of copper, cobalt, nickel and / or zinc;
[0041] Optionally, the metal nanoparticles formed from the divalent soluble metal salt in a metal-supported carbon-based fiber structure catalyst have a weight percentage of 5%-20%.
[0042] In the examples selected in this invention, the divalent soluble metal salt is preferably a copper salt. The Cu nanocrystal structure in transition metal materials has a high grain boundary density and defect sites that can optimize the binding energy of reaction intermediates such as CO. Moreover, the Cu microcrystal structure has strong chemical stability and is often used as a base metal to stabilize single atoms of transition metals.
[0043] In one optional embodiment, in a method for preparing a metal-supported carbon-based fiber structure catalyst, the mass concentration of the polyacrylonitrile in the electrospinning solution is 8 wt% to 15 wt%.
[0044] Optionally, the solvent is N,N-dimethylformamide.
[0045] In this embodiment,
[0046] In one optional embodiment, in a method for preparing a metal-supported carbon-based fiber structure catalyst, the electrospinning conditions are: temperature of 20℃~40℃, humidity of 15%~35%, feed rate of 0.2-2ml / min, and spinning voltage of 10-20V.
[0047] In this embodiment, the electrospinning device can be a commonly used spinning device. In this embodiment, a 10m syringe equipped with a 20G needle is used for spinning, the spinning solution propulsion rate is 0.5mL / h, and the spinning voltage is 20kV.
[0048] In one optional embodiment, a method for preparing a metal-supported carbon-based fiber structure catalyst further includes: collecting electrospun fibers using aluminum foil at a fixed receiving distance of 12-20 cm, and then drying the collected electrospun fibers at room temperature for 24-72 h.
[0049] In this example, the collection of electrospun fibers is not limited to aluminum foil; any material that facilitates the collection of electrospun fibers can be used. The collection conditions can be determined according to specific needs. In this embodiment, the receiving distance is 18 cm, the ambient temperature is 25°C, and the humidity is 25±5%. The collected electrospun fibers are dried in a ventilated environment at room temperature for 24-72 hours, preferably by forced air drying at 40°C for 24 hours.
[0050] In one optional embodiment, in a method for preparing a metal-supported carbon fiber structure catalyst, the calcination heating rate is 2℃ / min-10℃ / min, the temperature is 700-1000℃, and the calcination time is 0.1-5h.
[0051] Optionally, the calcination atmosphere is one or a mixture of two of carbon dioxide and argon.
[0052] In one optional embodiment, in a method for preparing a metal-supported carbon fiber structure catalyst, the calcination involves first heating to 600°C at a heating rate of 10°C / min and holding for 1-2 hours, then heating to 700°C at a heating rate of 5°C / min and holding for 0.5-1 hours, and finally calcining to 700-1000°C at a heating rate of 2°C / min and holding for 5-10 minutes.
[0053] In one optional embodiment, in a method for preparing a metal-supported carbon fiber structure catalyst, the calcination involves first heating to 600°C in an argon atmosphere at a heating rate of 10°C / min and holding for 1-2 hours, then heating to 700°C in a CO2 atmosphere at a heating rate of 5°C / min and holding for 0.5-1 hours, and finally calcining to 700-1000°C in a CO2 atmosphere at a heating rate of 2°C / min for 5-10 minutes.
[0054] In this embodiment, the electrospun fibers can be calcined in a tube furnace using segmented atmosphere control. The metal nanoparticles formed by the divalent soluble metal salt during calcination are uniformly dispersed within the carbon-based fiber structure. Specifically, the calcination conditions are as follows: first, the temperature is raised to 600°C in an Ar atmosphere at a heating rate of 10°C / min and held for 2 hours; then, the temperature is raised to 700°C in a CO2 atmosphere at a heating rate of 5°C / min and held for 0.5 hours; finally, the temperature is raised to 900°C in a CO2 atmosphere at a heating rate of 2°C / min and held for 10 minutes, maintaining the flow rates of Ar and CO2 at 30 sccm.
[0055] The present invention also provides a metal-supported carbon-based fiber structure catalyst, which is prepared by any of the above methods.
[0056] In this embodiment, when the divalent soluble metal salt is a soluble copper salt, the metal-supported carbon-based fiber structure catalyst includes Cu nanoparticles and a carbon-based fiber structure. While preparing the metal-supported carbon-based fiber structure, the surface of the carbon-based fiber can be modified with oxygen-containing groups, so that the preparation and modification can be completed in one step, avoiding the complicated process of subsequent modification.
[0057] The present invention also provides the application of metal-supported carbon-based fiber structure catalysts in the synergistic electrochemical CO2 capture and in-situ conversion. Optionally, the metal-supported carbon-based fiber structure catalysts can be used to achieve CO2 capture and in-situ conversion through electrocatalysis.
[0058] In this embodiment, the metal-supported carbon fiber structure catalyst is applied to achieve CO2 capture and in-situ conversion in an electrochemical manner. Specifically, at room temperature, the metal-supported carbon fiber structure catalyst is coated on a gas diffusion electrode as the working electrode, mercury-mercury oxide is used as the reference electrode, a platinum sheet is used as the counter electrode, and potassium hydroxide solution is used as the electrolyte to carry out electrochemical CO2 in-situ capture and conversion research in a flow electrolytic cell.
[0059] In this embodiment, the metal-supported carbon-based fiber structure catalyst has a dual function of CO2 capture and conversion. The highly active C=O quinone structure of the carbon-based fiber structure has excellent carbon capture ability, which can optimize CO2 adsorption and facilitate CO2 capture. It significantly enhances CO2 activation, increases the formation of CO intermediates, and promotes CC coupling. It shows excellent performance in electrochemical CO2 capture and in-situ conversion to prepare ethylene products.
[0060] The preparation method of the metal-supported carbon fiber structure catalyst provided by the present invention will be further explained and illustrated below through specific preparation examples and comparative examples.
[0061] Example
[0062]
[0063] Comparative Example
[0064]
[0065] Example 1
[0066] Depend on Figure 1 As shown, this embodiment provides a metal-supported carbon-based fiber structure catalyst, which is prepared by a method including the following specific steps:
[0067] (1) Weigh 1.0g PAN and add it to a 50ml sealed bottle containing 10g DMF. Stir at room temperature for 24h to dissolve it completely. Then add 1.0g Cu(CO2CH3)2·H2O to the above spinning solution and continue stirring at room temperature for 24h to obtain electrospinning solution.
[0068] (2) The above electrospinning solution was injected into a 10ml syringe equipped with a 20G needle for electrospinning. The electrospinning conditions were: the spinning solution feed rate was 0.5mL / h, the spinning voltage was 20kV, the receiving distance was 18cm, the electrospinned fibers were collected with aluminum foil, the ambient temperature was 25℃, and the humidity was 25±5%.
[0069] (3) The spun fibers were dried in a forced-air drying oven at 40 degrees for 24 hours. 250 mg of spun fibers were weighed and placed in the high-temperature zone of a tube furnace. The calcination was carried out by segmented heating atmosphere control, that is: first, the temperature was raised to 600 degrees in an Ar atmosphere at a heating rate of 10 degrees Celsius and held for 2 hours, then the temperature was raised from 600 degrees Celsius to 700 degrees Celsius in a CO2 atmosphere at a heating rate of 5 degrees Celsius and held for 0.5 hours, and finally the temperature was raised from 700 degrees Celsius to 900 degrees Celsius in a CO2 atmosphere at a heating rate of 2 degrees Celsius and held for 10 minutes. In step (3), the flow rate of Ar and CO2 was kept at 30 sccm. The system was then cooled to room temperature to obtain the metal-supported carbon fiber structure catalyst, denoted as Cu@C=O.
[0070] In this embodiment, Figure 1 The image shows a Cu@C=O TEM transmission electron microscope image. The carbon-based fiber structure possesses a unique porous structure, with Cu nanoparticles uniformly confined within it. The graphene-like shell thickness on the Cu nanoparticle surface is approximately 4-5 nm. Therefore, the metal-supported carbon-based fiber catalyst prepared using the above method comprises Cu nanoparticles and a carbon-based fiber structure, with the Cu nanoparticles uniformly dispersed within the carbon-based fiber structure. This forms a structurally stable metal-supported carbon-based fiber catalyst with high reproducibility, high loading efficiency, and good size controllability, which helps improve its catalytic performance in CO2 capture and conversion processes.
[0071] Example 2
[0072] like Figure 2 As shown, this embodiment provides a composite metal oxide catalyst, which is prepared by a method including the following specific steps:
[0073] (1) Weigh 1.0g PAN and add it to a 50ml sealed bottle containing 10g DMF. Stir at room temperature for 24h to dissolve it completely. Then add 1.0g Co(CO2CH3)2·4H2O to the above spinning solution and continue stirring at room temperature for 24h to obtain electrospinning solution.
[0074] (2) The above spinning solution was injected into a 10ml syringe equipped with a 20G needle for electrospinning. The electrospinning conditions were: the spinning solution feed rate was 0.5mL / h, the spinning voltage was 20kV, the receiving distance was 18cm, the electrospinned fibers were collected with aluminum foil, the ambient temperature was 25℃, and the humidity was 25±5%.
[0075] (3) The spun fibers were dried in a forced-air drying oven at 40 degrees for 24 hours. 250 mg of spun fibers were weighed and placed in the high-temperature zone of a tube furnace. The calcination was carried out by segmented heating atmosphere control, that is: first, the temperature was raised to 600 degrees in an Ar atmosphere at a heating rate of 10 degrees Celsius and held for 2 hours, then the temperature was raised from 600 degrees Celsius to 700 degrees Celsius in a CO2 atmosphere at a heating rate of 5 degrees Celsius and held for 0.5 hours, and finally the temperature was raised from 700 degrees Celsius to 900 degrees Celsius in a CO2 atmosphere at a heating rate of 2 degrees Celsius and held for 10 minutes. In step (3), the flow rate of Ar and CO2 was kept at 30 sccm. The system was then cooled to room temperature to obtain the metal-supported carbon fiber structure catalyst, denoted as Co@C=O.
[0076] In this embodiment, Figure 2 The image shows a transmission electron microscope (TEM) image of Co@C=O. As can be seen, the carbon-based fiber structure possesses a unique porous structure, with Co nanoparticles uniformly confined within it. The graphene-like shell layer on the surface of the Co nanoparticles is approximately 4-5 nm thick. This indicates that the metal-supported carbon-based fiber catalyst obtained using the above preparation method comprises Co nanoparticles and a carbon-based fiber structure, with the Co nanoparticles uniformly dispersed within the carbon-based fiber structure, forming a structurally stable metal-supported carbon-based fiber catalyst. This catalyst exhibits high loading efficiency, good size controllability, and contributes to improved catalytic performance. Furthermore, in this embodiment, using a Co metal salt as the divalent soluble metal salt also yields a catalyst with good stability. Therefore, the preparation method of the metal-supported carbon-based fiber catalyst in this invention has high versatility, is applicable to various metals, has high reproducibility, and is conducive to large-scale production.
[0077] Example 3
[0078] like Figure 3 As shown, this embodiment provides a composite metal oxide catalyst, which is prepared by a method including the following specific steps:
[0079] (1) Weigh 1.0g PAN and add it to a 50ml sealed bottle containing 10g DMF. Stir at room temperature for 24h to dissolve it completely. Then add 1.0g Ni(OCOCH3)2·4H2O to the above spinning solution and continue stirring at room temperature for 24h to obtain electrospinning solution.
[0080] (2) The above spinning solution was injected into a 10ml syringe equipped with a 20G needle for electrospinning. The electrospinning conditions were: the spinning solution feed rate was 0.5mL / h, the spinning voltage was 20kV, the receiving distance was 18cm, the electrospinned fibers were collected with aluminum foil, the ambient temperature was 25℃, and the humidity was 25±5%.
[0081] (3) The spun fibers were dried in a forced-air drying oven at 40 degrees for 24 hours. 250 mg of spun fibers were weighed and placed in the high-temperature zone of a tube furnace. The calcination was carried out by segmented heating atmosphere control, that is: first, the temperature was raised to 600 degrees in an Ar atmosphere at a heating rate of 10 degrees Celsius and held for 2 hours, then the temperature was raised from 600 degrees Celsius to 700 degrees Celsius in a CO2 atmosphere at a heating rate of 5 degrees Celsius and held for 0.5 hours, and finally the temperature was raised from 700 degrees Celsius to 900 degrees Celsius in a CO2 atmosphere at a heating rate of 2 degrees Celsius and held for 10 minutes. In step (3), the flow rate of Ar and CO2 was kept at 30 sccm. The system was then cooled to room temperature to obtain the metal-supported carbon fiber structure catalyst, denoted as Ni@C=O.
[0082] In this embodiment, as Figure 3 The image shown is a transmission electron microscope (TEM) image of Ni@C=O. It can be seen from the image that the carbon-based fiber structure has a unique porous structure, and the Ni nanoparticles are uniformly confined within the carbon-based fiber structure. The thickness of the graphene-like shell on the surface of the Ni nanoparticles is approximately 4-5 nm. The metal-supported carbon-based fiber structure catalyst obtained by the above preparation method includes Co nanoparticles and a carbon-based fiber structure, with Ni nanoparticles uniformly dispersed within the carbon-based fiber structure, forming a structurally stable metal-supported carbon-based fiber structure catalyst. This catalyst exhibits high loading efficiency, good size controllability, and contributes to improved catalytic performance. Furthermore, in this example, using a Ni metal salt as the divalent soluble metal salt also yields a catalyst with good stability. Therefore, the preparation method of the metal-supported carbon-based fiber structure catalyst of this invention has good versatility, applicable not only to Cu but also to Co, Ni, and other metals. In other words, the preparation method of the metal-supported carbon-based fiber structure catalyst of this invention has high versatility, is applicable to multiple metals, has high reproducibility, and is conducive to large-scale production.
[0083] Comparative Example 1
[0084] This comparative example provides a metal-supported carbon-based fiber structured catalyst, which is prepared by a method including the following specific steps:
[0085] (1) Weigh 1.0g PAN and add it to a 50ml sealed bottle containing 10g DMF. Stir at room temperature for 24h to dissolve it completely. Then add 1.0g Cu(CO2CH3)2·H2O to the above spinning solution and continue stirring at room temperature for 24h to obtain electrospinning solution.
[0086] (2) The above spinning solution was injected into a 10ml syringe equipped with a 20G needle for electrospinning. The electrospinning conditions were: the spinning solution feed rate was 0.5mL / h, the spinning voltage was 20kV, the receiving distance was 18cm, the electrospinned fibers were collected with aluminum foil, the ambient temperature was 25℃, and the humidity was 25±5%.
[0087] (3) The spun fibers were dried in a forced-air drying oven at 40 degrees for 24 hours. 250 mg of spun fibers were weighed and placed in the high-temperature zone of a tube furnace. The calcination was carried out by segmented heating atmosphere control, that is: first, the temperature was raised to 600 degrees in an Ar atmosphere at a heating rate of 10 degrees Celsius and held for 2 hours, then the temperature was raised from 600 degrees Celsius to 700 degrees Celsius in an Ar atmosphere at a heating rate of 5 degrees Celsius and held for 0.5 hours, and finally the temperature was raised from 700 degrees Celsius to 900 degrees Celsius in an Ar atmosphere at a heating rate of 2 degrees Celsius and held for 10 minutes. In step (3), the Ar flow rate was kept at 30 sccm. The system was then cooled to room temperature to obtain the metal-supported carbon fiber structure catalyst, denoted as Cu@C.
[0088] Compared with Example 1, the difference in Comparative Example 1 lies in the segmented heating atmosphere control method during calcination. In the Comparative Example, the three calcination atmospheres were all Ar, and the resulting catalyst was Cu@C. In Example 1, the first heating atmosphere was Ar, and the second and third heating atmospheres were all CO2, and the resulting catalyst was Cu@C=O. This proves that CO2 atmosphere control can form a highly active oxygen-containing functional group structure with C=O on the surface of the carbon-based fiber structure, and the C=O structure is not affected after metal loading. In contrast, a simple Ar atmosphere is not conducive to the formation of a highly active oxygen-containing functional group structure with C=O.
[0089] Comparative Example 2
[0090] This comparative example provides a metal-supported carbon-based fiber structured catalyst, which is prepared by a method including the following specific steps:
[0091] (1) Weigh 1.0g PAN and add it to a 50ml sealed bottle containing 10g DMF. Stir at room temperature for 24 hours to dissolve it completely.
[0092] (2) The above spinning solution was injected into a 10ml syringe equipped with a 20G needle for electrospinning. The electrospinning conditions were: the spinning solution feed rate was 0.5mL / h, the spinning voltage was 20kV, the receiving distance was 18cm, the electrospinned fibers were collected with aluminum foil, the ambient temperature was 25℃, and the humidity was 25±5%.
[0093] (3) The spun fibers were dried in a forced-air drying oven at 40 degrees for 24 hours. 250 mg of spun fibers were weighed and placed in the high-temperature zone of a tube furnace. The calcination was carried out by segmented heating atmosphere control, that is: first, the temperature was raised to 600 degrees in an Ar atmosphere at a heating rate of 10 degrees Celsius and held for 2 hours, then the temperature was raised from 600 degrees Celsius to 700 degrees Celsius in a CO2 atmosphere at a heating rate of 5 degrees Celsius and held for 0.5 hours, and finally the temperature was raised from 700 degrees Celsius to 900 degrees Celsius in a CO2 atmosphere at a heating rate of 2 degrees Celsius and held for 10 minutes. In step (3), the flow rate of CO2 and Ar was kept at 30 sccm. The system was then cooled to room temperature to obtain the metal-supported carbon fiber structure catalyst, denoted as C=O.
[0094] Compared with Example 1, Comparative Example 2 did not involve the participation of soluble metal salts, and therefore did not form a metal-loaded carbon-based fiber structure, resulting in a C=O catalyst.
[0095] Comparative Example 3
[0096] This comparative example provides a metal-supported carbon-based fiber structured catalyst, which is prepared by a method including the following specific steps:
[0097] (1) Weigh 1.0g PAN and add it to a 50ml sealed bottle containing 10g DMF. Stir at room temperature for 24 hours to dissolve it completely.
[0098] (2) The above spinning solution was injected into a 10ml syringe equipped with a 20G needle for electrospinning. The electrospinning conditions were: the spinning solution feed rate was 0.5mL / h, the spinning voltage was 20kV, the receiving distance was 18cm, the electrospinned fibers were collected with aluminum foil, the ambient temperature was 25℃, and the humidity was 25±5%.
[0099] (3) The spun fibers were dried in a forced-air drying oven at 40 degrees for 24 hours. 250 mg of spun fibers were weighed and placed in the high-temperature zone of a tube furnace. The calcination was carried out by segmented heating atmosphere control, that is: first, the temperature was raised to 600 degrees in an Ar atmosphere at a heating rate of 10 degrees Celsius and held for 2 hours, then the temperature was raised from 600 degrees Celsius to 700 degrees Celsius in a CO2 atmosphere at a heating rate of 5 degrees Celsius and held for 0.5 hours, and finally the temperature was raised from 700 degrees Celsius to 900 degrees Celsius in an Ar atmosphere at a heating rate of 2 degrees Celsius and held for 10 minutes. In step (3), the Ar flow rate was kept at 30 sccm. The system was then cooled to room temperature to obtain the metal-supported carbon-based fiber structure catalyst, denoted as C.
[0100] Compared with Comparative Example 2, Comparative Example 3 had the same atmosphere in the first two stages of the segmented heating process during calcination as Comparative Example 2. In the third stage, Comparative Example 3 obtained C as the catalyst in Ar atmosphere, while Comparative Example 2 obtained C=O as the catalyst in CO2 atmosphere. This further proves that CO2 atmosphere regulation can form a structure with highly active oxygen-containing functional groups of C=O on the surface of carbon-based fiber structure.
[0101] In summary, among the above examples and comparative examples, our CV scanning revealed that only Example 1 and Comparative Example 2 showed redox peaks at 0.41V and 0.49V (compared to the reversible hydrogen electrode), demonstrating that CO2 atmosphere-induced energy can introduce highly active oxygen-containing functional groups (C=O quinone structures) onto the carbon fiber surface.
[0102] In summary, in the above embodiments and comparative examples, through Figure 4 This demonstrates that C=O quinone structures have the ability to capture CO2.
[0103] Figure 4 The CO2 adsorption diagram shown demonstrates that, under the same conditions, the CO2 adsorption capacity of the carbon fiber catalyst with the C=O quinone structure is significantly increased. This indicates that there is a strong interaction between the C=O quinone structure carbon fiber and CO2 molecules, meaning that the C=O quinone structure can effectively capture and activate CO2 molecules, reducing their reaction energy barrier.
[0104] Application examples
[0105] The Cu@C=O provided in Example 1 and Comparative Examples 1, 2, and 3 were used as examples for electrochemical CO2 capture and in-situ conversion to ethylene. The electrochemical CO2 capture and in-situ conversion process was carried out in a flow electrolyzer with anion exchange membrane as the diaphragm. The specific steps are as follows:
[0106] The metal-supported carbon fiber structure catalyst was coated on a gas diffusion electrode as the working electrode, a platinum sheet electrode was used as the anode, a mercury-mercury oxide electrode was used as the reference electrode, and electrochemical CO2 in-situ capture and conversion was studied in a flow electrolytic cell using potassium hydroxide solution as the cathode / anodic electrolyte.
[0107] The reaction was then carried out under the following conditions for 1 hour: a constant current of 100-500 mA cm⁻², a CO₂ flow rate of 50 sccm throughout the reaction, a cathode electrolyte circulation rate of 10 sccm, an anolyte circulation rate of 200 sccm, and a test temperature of 25℃. After 1 hour of reaction, the electrochemical products were detected.
[0108] In this application example, the specific preparation method of the working electrode is as follows: 5 mg of the catalyst as described above is mixed with 470 g of isopropanol, and the resulting mixed solution is ultrasonicated at room temperature for 35 min to form a homogeneous solution. Then, 20 μL of 5 wt% Nafion solution is added dropwise to the homogeneous solution, and ultrasonication continues for 40 min to obtain a catalyst slurry. Subsequently, 100 μL of the catalyst slurry is drop-coated onto the gas diffusion electrode using a pipette and dried under an infrared lamp to complete the fabrication of the working electrode. The effective area of the working electrode (cathode) is 1 cm². 2 In the working electrode, the catalyst loading is 1 mg cm⁻².
[0109] In this application example, the KOH electrolyte is a 1M solution with a volume of 30mL.
[0110] In this application example, the Faradaic efficiency diagrams of the products obtained from the Cu@C=O catalyst prepared in Example 1 at different current densities are shown below. Figure 5 As shown in the figure, it can be seen that the Faraday efficiency of the multi-carbon product (C2+) significantly improves with increasing current density, and even at a current density of 400 mA cm⁻¹, the efficiency increases significantly. -2 At that time, the overall Faraday efficiency of C2 products was greater than 73%, with ethylene having a Faraday efficiency as high as 63%.
[0111] For the Cu@C catalyst prepared in Comparative Example 1, after 1 h of reaction, the total Faradaic efficiency of C2+ was less than 30% at a current density of 400 mA cm-2, while the Faradaic efficiency of methane was as high as 55%.
[0112] For the C=O catalyst prepared in Comparative Example 2, after 1 hour of reaction, some CO was generated at a current density of 400 mA cm⁻², and the Faraday efficiency of CO was greater than 30%.
[0113] For the C catalyst prepared in Comparative Example 3, after 1 hour of reaction, only trace amounts of CO were generated at a current density of 400 mA cm⁻², and the Faraday efficiency of H₂ was greater than 80%.
[0114] Faraday efficiency
[0115]
[0116] As can be seen from the table above, the catalyst with the highest Faraday efficiency is Cu@C=O obtained by the method of preparing the metal-supported carbon-based fiber structure catalyst of the present invention in Example 1. The catalyst obtained by adding a divalent soluble metal salt of Cu to a mixed reagent of PAN and DMF, and calcining it in a CO2 atmosphere during the second and third stages of the three-stage calcination process, exhibits the highest Faraday efficiency. Next is Comparative Example 1. In the three-stage calcination, when it is entirely placed in Ar, the Faraday efficiency is slightly weaker. This is because the CO2 atmosphere regulation can form a structure with highly active oxygen-containing functional groups of C=O on the surface of the carbon-based fiber structure. This is not conducive to the formation of C=O structures, but it optimizes CO2 adsorption, which is beneficial for CO2 capture, increases the formation of CO intermediates, and facilitates electrochemical CO2 capture and in-situ conversion. Compared to Comparative Example 2, Comparative Example 3 has a very weak carbon capture ability due to the lack of a C=O highly active oxygen-containing functional group structure, resulting in extremely low CO Faraday efficiency. The metal catalyst is supported on a carbon-based fiber structure. Due to the excellent CO2 capture ability of C=O, intermediate CO is enriched on the surface of metal Cu, increasing the local CO concentration and promoting CC coupling to improve C2 Faraday efficiency.
[0117] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a metal-supported carbon-based fibrous structure catalyst, characterized by, Includes the following steps: (1) Mix polyacrylonitrile and divalent soluble metal salt in a solvent to obtain an electrospinning solution; (2) The electrospinning solution is placed in an electrospinning device for electrospinning, and electrospinning fibers are collected. (3) The electrospun fibers are calcined to obtain a metal-supported carbon-based fiber structure catalyst. The divalent soluble metal salt is selected from at least one of soluble copper salt, cobalt salt, and nickel salt; The calcination process involves first heating the temperature to 600℃ in an argon atmosphere at a heating rate of 10℃ / min and holding it there for 1-2 hours, then heating the temperature to 700℃ in a CO2 atmosphere at a heating rate of 5℃ / min and holding it there for 0.5-1 hours, and finally calcining the temperature to 900-1000℃ in a CO2 atmosphere at a heating rate of 2℃ / min for 5-10 minutes.
2. The method of claim 1, wherein the metal-loaded carbon-based fibrous structure catalyst is prepared by the steps of: The divalent soluble metal salt is selected from at least one of the chlorides, nitrates, sulfates, or acetates of copper, cobalt, and nickel.
3. The method for preparing the metal-supported carbon-based fiber structure catalyst according to claim 1, characterized in that, The metal nanoparticles formed by calcination of the divalent soluble metal salt in the metal-supported carbon fiber structure catalyst comprise 5%-20% by weight.
4. The method for preparing the metal-supported carbon-based fiber structure catalyst according to claim 1, characterized in that, The mass concentration of polyacrylonitrile in the electrospinning solution is 8 wt% to 15 wt%.
5. The method for preparing the metal-supported carbon-based fiber structure catalyst according to claim 1, characterized in that, The solvent is N,N-dimethylformamide.
6. The method for preparing the metal-supported carbon-based fiber structure catalyst according to claim 1, characterized in that, The electrospinning conditions are: temperature of 20℃~40℃, humidity of 15%~35%, feed rate of 0.2-2mL / min, and spinning voltage of 10-20kV.
7. The method for preparing the metal-supported carbon-based fiber structure catalyst according to claim 6, characterized in that, Further includes: Electrospun fibers were collected using aluminum foil at a fixed receiving distance of 12-20 cm, and then dried at room temperature for 24-72 hours.
8. A metal-supported carbon-based fiber structured catalyst, characterized in that, The metal-supported carbon-based fiber structure catalyst was prepared using any one of the methods described in claims 1 to 7.
9. The application of the metal-supported carbon-based fiber structure catalyst of claim 8 in the synergistic electrochemical CO2 capture and in-situ conversion, characterized in that, The metal-supported carbon-based fiber structure catalyst can be used to achieve CO2 capture and in-situ conversion through electrocatalysis.
Citation Information
Patent Citations
Cu-based single-atom alloy catalyst for electrocatalytic reduction of CO2 and preparation method thereof
CN115679373B
Carbon fiber-based CH4-CO2 reforming catalyst and preparation method thereof
CN116078441A
Process for producing carbon fibers having high strand strength
US5348719A