A method for preparing a copper-supported silica catalyst for dehydrogenation of mixed alcohols
By modifying zinc-modified copper-supported silica catalyst, combining β-cyclodextrin and rare earth element additives, the problems of prone to poisoning and inactivation and high cost of precious metal catalysts are solved, and the catalytic activity and selectivity of the mixed alcohol dehydrogenation reaction are improved. , realize the effective preparation of high value-added ester fuels.
Patent Information
- Application Number
- CN202311130304.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-09-04
AI Technical Summary
In the prior art, noble metal catalysts are prone to poisoning and inactivated in the mixed alcohol dehydrogenation reaction and are costly, and traditional copper-based catalysts have shortcomings in catalytic activity and selectivity, making it difficult to effectively prepare high value-added ester fuels.
Using zinc-modified copper-supported silica catalyst, the dispersion of the catalyst is improved by combining β-cyclodextrin and rare earth elements Ce and La as additives. and activity, forming a catalyst with high selectivity and conversion rate.
The catalytic activity and selectivity of the mixed alcohol dehydrogenation reaction are significantly improved, the catalyst cost is reduced, and the methyl formate generation rate and ester product yield is achieved, with good industrial application prospects.
Smart Images

Figure BDA0004429882020000061 
Figure BDA0004429882020000071
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a zinc-modified copper-loaded silicon dioxide catalyst for mixed alcohol dehydrogenation. Background Art
[0002] At present, the problems of fossil energy shortage and atmospheric pollution are becoming increasingly serious. Seeking clean energy is the key to solving this problem. Among them, some oxygen-containing components can be used as diesel mixed fuels, and can be mixed with diesel and show good emission performance. The oxygen-containing characteristics of oxygen-containing fuels can significantly reduce emissions that pollute the environment under the premise of ensuring the combustion performance of diesel engines. Relevant studies have shown that when a small amount of oxygen-containing fuel is added, smoke emissions increase rapidly, but in order to avoid the reduction of diesel combustion performance, the oxygen content of oxygen-containing fuels should not exceed 10%. Therefore, oxygen-containing compounds have become a component of engine clean fuels and play an important role in PM emission reduction. In addition, oxygen-containing fuels not only have abundant raw material sources, but also can be recycled and regenerated in large quantities. Therefore, their research at home and abroad is relatively extensive, mainly including alcohol ethers, esters, biodiesel, oxygen-containing wide fractions, etc. Esters have a place in the research of alternative fuels, so it is crucial to prepare high value-added oxygen-containing compounds.
[0003] In recent years, methanol as a fuel has attracted the attention of a large number of researchers. As one of the alternative fuels, it has the characteristics of wide sources, diverse uses, and low prices. Although the coal-to-methanol industry has developed rapidly, the traditional downstream demand is weak, mainly methyl formate, formaldehyde, dimethyl ether, dimethyl carbonate (DMC) and methyl tert-butyl ether, but the amount is limited. Therefore, converting methanol into higher value-added oil products and chemicals has become an urgently needed technology. The main conversion methods include methanol to low-carbon olefins, methanol carbonylation to acetic acid, methyl formate and DMC, methanol oxidation to methylal and methyl formate, methanol direct dehydrogenation to methyl formate, etc. Among them, methyl formate is a chemical intermediate with great application value. It can be used to produce formic acid, formamide, ethylene glycol, etc., and is expected to replace methyl tert-butyl ether (MTBE) as a gasoline additive. In addition, methyl formate has aroused great interest as an emission-reducing fuel additive. Methyl formate can be synthesized directly by dehydrogenation of methanol. In addition to producing methyl formate, the methanol dehydrogenation reaction also produces a small amount of CO and H2, which can be used to synthesize methanol. Such a cycle proves that methanol dehydrogenation reaction is a green utilization method for synthesizing methyl formate.
[0004] The selection and design of catalysts for the mixed alcohol dehydrogenation reaction are crucial. Among them, both noble metals and transition metals can be used in this reaction as active catalysts. Noble metal catalysts have excellent catalytic activity, but are easily poisoned and deactivated, and are expensive, which limits their wide application in industry. In contrast, copper-based catalysts have excellent performance and economy and can be used as suitable catalysts for the mixed alcohol dehydrogenation reaction. In addition, copper-based catalysts can also be widely used in other alcohol dehydrogenation reactions and ester exchange reactions.
[0005] To this end, this patent selects the green synthesis route of direct dehydrogenation of mixed alcohols to prepare mixed esters, studies various aspects of the catalyst for the dehydrogenation reaction of mixed alcohols, uses low-cost mixed alcohols to prepare higher value-added ester products, and mixes them with diesel as an alternative fuel for diesel engines. This patent is expected to fundamentally solve the problem of the poor miscibility of alcohols and diesel, and deeply explore its practical application value. Summary of the invention
[0006] This patent invents a method for preparing a zinc-modified copper-supported silica catalyst for dehydrogenation of mixed alcohols. The specific technical solution of the invention is:
[0007] (1) Synthesis of copper-ammine complex
[0008] Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, and calculate the Cu loading amount of 20wt% to 40wt% based on the mass of the carrier, wherein the mass ratio of copper to zinc is 5 to 20:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; dissolve Ce(NO3)3 and La(NO3)3 as auxiliary agents into the above solution, and the added amount is calculated based on the content of Ce and La each accounting for 1% of the catalyst; slowly add ammonia water under stirring to generate a copper-ammine complex, and control the pH value to 8 to 9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1% to 10%;
[0009] (2) Preparation of catalytic precursor
[0010] After the copper-ammonia complex is generated, a certain amount of inclusion agent β-cyclodextrin and a certain amount of silica sol are weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the amount of β-cyclodextrin added is 1 to 3 times the sum of the amounts of copper and zinc substances, and the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6 to 7, and after filtering, washing, drying, roasting, and sieving, a catalyst precursor of 20 to 40 mesh is obtained;
[0011] (3) Preparation of zinc-modified copper-supported silica catalyst
[0012] The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350°C, and cooled under nitrogen protection to finally obtain a zinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
[0013] 2. The catalyst according to claim 1, characterized in that it is used for mixed alcohol dehydrogenation reaction, the reaction conditions are that the raw materials are alcohol A and alcohol B mixed in a ratio of 20:1 to 5:1, the reaction temperature is 240°C to 280°C, the reaction pressure is 0.2MPa to 0.5MPa, and the reaction space velocity is 1h -1 ~4h -1 The gas used is nitrogen, and the feed flow rate is 0.065-0.103 ml / min, wherein the above-mentioned alcohol A is methanol or ethanol, and the alcohol B is propanol or n-butanol.
[0014] Compared with the prior art, the present invention has the following innovations:
[0015] (1) The bimetallic rare earth ions Ce and La are doped as additives. The addition of rare earth metals can enhance the interaction between copper and the carrier, improve its dispersion, and reduce the size of copper particles. The addition of La and Ce rare earth elements can reduce the grain size of CuO in the calcined Cu / SiO2 catalyst, thereby reducing the grain size of CuO in the reduced catalyst, improving the activity of catalytic conversion, and having a better catalytic effect.
[0016] (2) β-cyclodextrin has a hydrophobic inner cavity and a hydrophilic surface. It can form a host-guest inclusion complex with organic, inorganic and other guest molecules or form a coordination modifier on its surface. Since β-cyclodextrin and its modifications have good reaction substrate selectivity and catalytic performance in a suitable liquid phase reaction system, the products formed usually have higher yields and selectivities compared with traditional organic synthesis methods. This patent selects β-cyclodextrin to include copper ammonia complex to form a catalyst precursor, which can significantly improve the selectivity and conversion rate of zinc-modified copper-loaded silica catalysts.
[0017] In addition, the raw materials used in the present invention are widely available and low in cost, and other materials used are conventional materials, so the catalyst has low cost, is conducive to industrial application, has good catalytic effect, and has good application prospects. DETAILED DESCRIPTION
[0018] The present invention is described in detail below in conjunction with embodiments:
[0019] Embodiment 1:
[0020] (1) Synthesis of copper-ammine complex
[0021] Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, and calculate the Cu loading amount as 30wt% based on the mass of the carrier, wherein the mass ratio of copper to zinc is 10:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; dissolve Ce(NO3)3 and La(NO3)3 as auxiliary agents into the above solution, and the added amount is calculated according to the content of Ce and La each accounting for 1% of the catalyst; slowly add ammonia water under stirring to form a copper-ammine complex, and control the pH value to 8-9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1%-10%;
[0022] (2) Preparation of catalytic precursor
[0023] After the copper-ammonia complex is generated, a certain amount of inclusion agent β-cyclodextrin and a certain amount of silica sol are weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the amount of β-cyclodextrin added is 1 to 3 times the sum of the amounts of copper and zinc substances, and the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6 to 7, and after filtering, washing, drying, roasting, and sieving, a catalyst precursor of 20 to 40 mesh is obtained;
[0024] (3) Preparation of zinc-modified copper-supported silica catalyst
[0025] The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350°C, and cooled under nitrogen protection to finally obtain a zinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
[0026] Embodiment 2:
[0027] (1) Synthesis of copper-ammine complex
[0028] Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, and calculate the Cu loading amount to be 20wt% based on the mass of the carrier, wherein the mass ratio of copper to zinc is 10:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; dissolve Ce(NO3)3 and La(NO3)3 as auxiliary agents into the above solution, and the added amount is calculated based on the content of Ce and La each accounting for 1% of the catalyst; slowly add ammonia water under stirring to form a copper-ammine complex, and control the pH value to be 8-9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1%-10%;
[0029] (2) Preparation of catalytic precursor
[0030] After the copper-ammonia complex is generated, a certain amount of inclusion agent β-cyclodextrin and a certain amount of silica sol are weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the amount of β-cyclodextrin added is 1 to 3 times the sum of the amounts of copper and zinc substances, and the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6 to 7, and after filtering, washing, drying, roasting, and sieving, a catalyst precursor of 20 to 40 mesh is obtained;
[0031] (3) Preparation of zinc-modified copper-supported silica catalyst
[0032] The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350°C, and cooled under nitrogen protection to finally obtain a zinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
[0033] Embodiment three:
[0034] (1) Synthesis of copper-ammine complex
[0035] Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, and calculate the Cu loading amount to be 40wt% based on the mass of the carrier, wherein the mass ratio of copper to zinc is 10:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; dissolve Ce(NO3)3 and La(NO3)3 as auxiliary agents into the above solution, and the added amount is calculated based on the content of Ce and La each accounting for 1% of the catalyst; slowly add ammonia water under stirring to form a copper-ammine complex, and control the pH value to be 8-9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1%-10%;
[0036] (2) Preparation of catalytic precursor
[0037] After the copper-ammonia complex is generated, a certain amount of inclusion agent β-cyclodextrin and a certain amount of silica sol are weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the amount of β-cyclodextrin added is 1 to 3 times the sum of the amounts of copper and zinc substances, and the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6 to 7, and after filtering, washing, drying, roasting, and sieving, a catalyst precursor of 20 to 40 mesh is obtained;
[0038] (3) Preparation of zinc-modified copper-supported silica catalyst
[0039] The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350°C, and cooled under nitrogen protection to finally obtain a zinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
[0040] Embodiment 4:
[0041] (1) Synthesis of copper-ammine complex
[0042] Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, and calculate the Cu loading amount to be 40wt% based on the mass of the carrier, wherein the mass ratio of copper to zinc is 15:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; dissolve Ce(NO3)3 and La(NO3)3 as auxiliary agents into the above solution, and the added amount is calculated based on the content of Ce and La each accounting for 1% of the catalyst; slowly add ammonia water under stirring to form a copper-ammine complex, and control the pH value to be 8-9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1%-10%;
[0043] (2) Preparation of catalytic precursor
[0044] After the copper-ammonia complex is generated, a certain amount of inclusion agent β-cyclodextrin and a certain amount of silica sol are weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the amount of β-cyclodextrin added is 1 to 3 times the sum of the amounts of copper and zinc substances, and the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6 to 7, and after filtering, washing, drying, roasting, and sieving, a catalyst precursor of 20 to 40 mesh is obtained;
[0045] (3) Preparation of zinc-modified copper-supported silica catalyst
[0046] The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350°C, and cooled under nitrogen protection to finally obtain a zinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
[0047] Comparative Example 1:
[0048] (1) Synthesis of copper-ammine complex
[0049] Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, calculate the Cu loading amount by the weight of the carrier to be 40wt%, wherein the weight ratio of copper to zinc is 15:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; slowly add ammonia water under stirring to form a copper-ammine complex, and control the pH value to be 8-9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1%-10%;
[0050] (2) Preparation of catalytic precursor
[0051] After the copper-ammonia complex is generated, a certain amount of inclusion agent β-cyclodextrin and a certain amount of silica sol are weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the amount of β-cyclodextrin added is 1 to 3 times the sum of the amounts of copper and zinc substances, and the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6 to 7, and after filtering, washing, drying, roasting, and sieving, a catalyst precursor of 20 to 40 mesh is obtained;
[0052] (3) Preparation of zinc-modified copper-supported silica catalyst
[0053] The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350° C., and cooled under nitrogen protection to finally obtain a comparative example 1 zinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
[0054] Comparative Example 2:
[0055] (1) Synthesis of copper-ammine complex
[0056] Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, and calculate the Cu loading amount to be 40wt% based on the mass of the carrier, wherein the mass ratio of copper to zinc is 15:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; dissolve Ce(NO3)3 and La(NO3)3 as auxiliary agents into the above solution, and the added amount is calculated based on the content of Ce and La each accounting for 1% of the catalyst; slowly add ammonia water under stirring to form a copper-ammine complex, and control the pH value to be 8-9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1%-10%;
[0057] (2) Preparation of catalytic precursor
[0058] After the copper-ammonia complex is generated, a certain amount of silica sol is weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6-7, and then filtered, washed, dried, calcined, and sieved to obtain a catalyst precursor of 20-40 mesh;
[0059] (3) Preparation of zinc-modified copper-supported silica catalyst
[0060] The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350° C., and cooled under nitrogen protection to finally obtain a comparative example dizinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
[0061] The catalysts of the application example and the comparative example are compared under the conditions of mixed alcohol dehydrogenation reaction: the raw materials of the reaction conditions are alcohol A and alcohol B, which are mixed in a ratio of 20:1 to 5:1, the reaction temperature is 240°C, the reaction pressure is 0.2MPa, and the reaction space velocity is 1h -1 The gas used is nitrogen, the feed flow rate is 0.065-0.103 ml / min, the alcohol A is methanol or ethanol, the alcohol B is propanol or n-butanol, and the catalyst performance evaluation is shown in the following table:
[0062]
[0063]
[0064] From the above results, it can be seen that the catalyst performance application example > comparative example 2 > comparative example 1, which indicates that the zinc-modified copper-loaded silica prepared for the dehydrogenation of mixed alcohols has a novel structure, and after the mixed alcohols are catalyzed by the catalyst, the conversion rate of methanol, the selectivity and the yield of mixed esters are improved.
[0065] By comparison, it is found that the catalyst of the present invention is doped with bimetallic rare earth ions Ce and La as additives. The addition of rare earth metals can enhance the interaction between copper and the carrier, improve its dispersion, and reduce the copper particle size. The addition of La and Ce rare earth elements can reduce the grain size of CuO in the calcined Cu / SiO2 catalyst, thereby reducing the grain size of CuO in the catalyst after reduction, improving the activity of catalytic conversion, and having a better catalytic effect.
[0066] In addition, during the preparation process, β-cyclodextrin was creatively introduced as an auxiliary agent. By utilizing the hydrophobic inner cavity and hydrophilic surface of cyclodextrin, it can form host-guest inclusion complexes with organic, inorganic and other guest molecules or form coordination modifiers on its surface. Cyclodextrin can fully encapsulate copper ions, prevent copper ion aggregation, and form a polymer system; and the hydrophilic surface of cyclodextrin guides copper ions to diffuse to the carrier, adsorb on the carrier surface, which is conducive to the loading of copper ligands and anchoring on the carrier, fully promoting the preparation of highly dispersed copper catalysts, increasing the number of active sites of the catalyst, and ensuring the high catalytic activity. Therefore, β-cyclodextrin and its modified bodies have good reaction substrate selectivity and catalytic performance in a suitable liquid phase reaction system.
[0067] As described in the review, the products formed by the method generally have higher yield and selectivity compared with the traditional organic synthesis method. This patent selects β-cyclodextrin to include copper ammonia complex to form a catalyst precursor, which can significantly improve the selectivity and conversion rate of zinc-modified copper-supported silica catalyst.
[0068] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a zinc-modified copper-supported silica catalyst for dehydrogenation of mixed alcohols, characterized in that: The mixed alcohol is a mixture of alcohol A and alcohol B, wherein A is methanol or ethanol, and alcohol B is propanol or n-butanol. Alcohol A and alcohol B are mixed in a ratio of 20:1 to 5:
1. The preparation comprises the following steps: (1) Synthesis of copper-ammine complex Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O solids, and calculate the Cu loading amount of 20wt% to 40wt% based on the mass of the carrier, wherein the mass ratio of copper to zinc is 5 to 20:1, and dissolve them in deionized water containing EDTA, citric acid or tartaric acid; dissolve Ce(NO3)3 and La(NO3)3 as auxiliary agents into the above solution, and the added amount is calculated based on the content of Ce and La each accounting for 1% of the catalyst; slowly add ammonia water under stirring to generate a copper-ammine complex, and control the pH value to 8 to 9; wherein the content of EDTA, citric acid or tartaric acid in deionized water is 1% to 10%; (2) Preparation of catalytic precursor After the copper-ammonia complex is generated, a certain amount of inclusion agent β-cyclodextrin and a certain amount of silica sol are weighed and mixed evenly, and then added thereto and stirred at 30°C for 4 hours, wherein the amount of β-cyclodextrin added is 1 to 3 times the sum of the amounts of copper and zinc substances, and the silica sol is calculated according to the mass of the required carrier silica; then the mixture is transferred to a rotary evaporator to evaporate ammonia so that the final pH value is 6 to 7, and after filtering, washing, drying, roasting, and sieving, a catalyst precursor of 20 to 40 mesh is obtained; (3) Preparation of zinc-modified copper-supported silica catalyst The catalytic precursor was reduced in a hydrogen atmosphere for 4 hours at a reduction temperature of 350°C, and cooled under nitrogen protection to finally obtain a zinc-modified copper-loaded silica catalyst, which needed to be sealed and stored.
2. The catalyst prepared according to the method of claim 1, characterized in that For mixed alcohol dehydrogenation reaction, the reaction conditions are that the raw materials are alcohol A and alcohol B mixed in a ratio of 20:1 to 5:1, the reaction temperature is 240°C to 280°C, the reaction pressure is 0.2MPa to 0.5MPa, and the reaction space velocity is 1h -1 ~4h -1 The gas used is nitrogen, and the feed flow rate is 0.065-0.103 ml / min, wherein the above-mentioned alcohol A is methanol or ethanol, and the alcohol B is propanol or n-butanol.