A method for preparing fiber-reinforced silicon carbide ceramic valve parts by reaction sintering and pressing
By using short-cut carbon fiber unbundling process and vacuum sintering technology, the problem of poor toughness in silicon carbide ceramic valve parts has been solved, achieving low-cost and high-efficiency toughening effect, which is suitable for industrial production.
Patent Information
- Application Number
- CN202310902371.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-07-21
AI Technical Summary
Existing silicon carbide ceramic valve components have poor toughness and are prone to cracking under high-speed particle impact, resulting in low service reliability. Furthermore, existing toughening processes are costly and complex, making them unsuitable for products with low economic added value.
A short-cut carbon fiber unbundling process is used to coat the unbundled carbon fibers onto the surface of silicon carbide granulated powder through ball milling and spray granulation. Combined with vacuum sintering and post-processing, fiber-toughened silicon carbide ceramic valves are prepared.
It achieves low-cost and high-efficiency toughening, improves the density and service reliability of silicon carbide ceramic valves, and is suitable for industrial production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of silicon carbide ceramic valve components, and in particular to a method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing. Background Art
[0002] Silicon carbide ceramics have excellent properties such as high hardness, high strength, high temperature resistance, oxidation resistance, corrosion resistance, wear resistance, thermal shock resistance, and good chemical stability, making it an ideal material for preparing high-performance valves. Ceramic valves made using the excellent properties of silicon carbide ceramics have better performance than traditional metal valves and plastic valves, and are particularly suitable for harsh industrial and mining environments with strong corrosion, severe wear and erosion, and high temperatures, such as mining, thermal power, petroleum, chemical industry, papermaking, polysilicon, metallurgy, and other fields. At present, silicon carbide ceramics have been used to make valve plates, valve balls, gate discs, valve seats and other valve parts.
[0003] However, compared with metals and plastics, silicon carbide ceramics have poor toughness and are particularly impact-resistant. When the fluid contains high-speed particles, the impact of the particles may cause impact cracks in the valve parts, which may lead to damage to the valve parts. The service reliability of the valve parts is low, and the excellent performance of silicon carbide ceramics cannot be fully utilized.
[0004] Reaction sintering is a commonly used method for preparing silicon carbide ceramics. Silicon carbide is generated by infiltrating molten silicon into the green body and reacting with the existing carbon in the green body in situ, and the silicon carbide powder in the green body is combined to prepare dense silicon carbide ceramics, which has been widely used in industrial production. Chinese patent CN202210133196.6 discloses a technical solution of this technical team, including preparing granulation powder, adding toughening fiber, pre-setting carbon fiber braid, impregnation, and then pressing, ramming, sintering and other steps. This solution does have a good toughening effect, but its cost is relatively high and the process is relatively complicated, which is suitable for products with high economic added value. For products with relatively small economic added value, this process is not conducive to improving the market competitiveness of the product.
[0005] Therefore, there is an urgent need to further study and optimize the toughening process of reaction-sintered silicon carbide ceramics, so that the toughening of reaction-sintered silicon carbide ceramic valve parts can be achieved in a more economical and simple way, which is of great significance for promoting the technological progress of the silicon carbide ceramic valve parts industry. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a method for preparing fiber-reinforced silicon carbide ceramic valve parts by reaction sintering and pressing to address the deficiencies of the prior art, thereby achieving the purpose of toughening silicon carbide ceramic valve parts in an economical and simple way.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing fiber-reinforced silicon carbide ceramic valve parts by reaction sintering and pressing, wherein the raw materials for preparing the ceramic valve parts include silicon carbide ceramic matrix material and toughening material; the matrix material includes 100 parts of silicon carbide micropowder, 5-20 parts of carbon powder, 5-15 parts of adhesive, 0.5-3 parts of surfactant and 0.5-2 parts of dispersant by weight; the toughening material is chopped carbon fiber, and the addition amount of the chopped carbon fiber is 0.1-15% of the total amount of the matrix material;
[0009] The preparation method specifically comprises the following steps:
[0010] (1) Preparation of granulated powder
[0011] Weigh the above matrix materials according to the ratio, add deionized water, the amount of deionized water is 0.9-1.5 times the mass of silicon carbide micropowder, and then ball mill for 8-20 hours to obtain silicon carbide ceramic slurry; then spray granulate the silicon carbide ceramic slurry to obtain granulated powder, sieve, take granulated powder between 10-100 mesh, and set aside, wherein the moisture content of the granulated powder is 0.5-1.2%, and the mass ratio of the particle size of 60-180 mesh in the granulated powder is greater than 90%;
[0012] (2) Pretreatment of chopped carbon fiber
[0013] Weigh the chopped carbon fiber and add it to a ball mill with a polyurethane liner, then add polyurethane balls to the ball mill, and perform roller milling for 1-5 hours to make the chopped carbon fiber bundle fluffy; then add deionized water to the ball mill, and continue roller milling for 1-8 hours to initially debundle the chopped carbon fiber bundle; then filter the treated chopped carbon fiber bundle, add it to a polyurethane ball mill, add anhydrous ethanol and polyurethane balls to the mill, and perform roller milling for 1-8 hours to further debundle the chopped carbon fiber bundle, then filter and dry to obtain debundled chopped carbon fiber for standby use;
[0014] (3) Debundled chopped carbon fiber coated granulated powder
[0015] The chopped carbon fibers prepared in step (2) are added to a coating machine, the coating machine is started, and the debundled chopped carbon fibers begin to rotate with the coating machine, and the chopped carbon fibers are sprayed with an alcohol solution containing phenolic resin and carbon black to humidify and thicken them, and then the granulation powder in step (1) is added, and the alcohol solution containing phenolic resin and carbon black is continuously sprayed, so that the debundled chopped carbon fibers adhere to the granulation powder during the rotation of the coating machine, thereby obtaining silicon carbide granulation powder coated with carbon fiber bundles;
[0016] The carbon fiber coated granulated powder is then dried at a temperature not higher than 70° C. to make its moisture content within the range of 0.5-1.2%.
[0017] (4) Silicon carbide granulated powder mixing
[0018] The coated granulated powder obtained in step (3) and the other granulated powders except 10-100 mesh in step (1) are mixed uniformly in a sugar coating machine;
[0019] (5) Valve molding
[0020] The granulated powder obtained in step (4) is pressed and molded to obtain a valve body green body, wherein the density of the valve body green body is 1.80-2.10 g / cm 3 ;
[0021] (6) Valve parts sintering
[0022] The processed valve green body is placed in a vacuum sintering furnace, and metal silicon particles are laid on the bottom and side of the valve green body, and then kept at 1450-1800°C for 1-8 hours to obtain a silicon carbide ceramic valve sintered body;
[0023] (7) Post-processing of valve parts
[0024] The silicon carbide ceramic valve component sintered body is subjected to post-processing treatments such as grinding and polishing to obtain silicon carbide ceramic valve components of required specifications, shapes and sizes.
[0025] Preferably, the silicon carbide powder is made of D 50 3-10μm silicon carbide powder, D 50 15-30μm silicon carbide powder and D 50 The silicon carbide powder with a size of 40-60 μm is mixed in a mass ratio of (3-8):(2-4):1.
[0026] Preferably, the binder is phenolic resin, polyvinyl alcohol or carboxymethyl cellulose; the surfactant is stearic acid or fatty acid glyceride; and the dispersant is tetramethylammonium hydroxide or polyacrylic acid.
[0027] Preferably, the carbon powder has a D 50 Less than 200nm.
[0028] Preferably, the chopped carbon fiber is a high-strength carbon fiber, and its tensile strength is not less than 3500 MPa;
[0029] The length of the chopped carbon fiber is less than 5 mm, and the diameter of the filament bundle is less than 500 μm.
[0030] Preferably, the diameter of the polyurethane ball in step (2) is 10-50 mm.
[0031] Preferably, the mass ratio of polyurethane balls to chopped carbon fibers in step (2) is (0.6-1.5):1; the mass ratio of deionized water to chopped carbon fibers is (0.8-2):1; the mass ratio of anhydrous ethanol to chopped carbon fibers is (0.8-1.5):1; and the drying temperature in step (2) is 50-80°C.
[0032] Preferably, the mass fraction of the phenolic resin in step (3) is 1-10%; the carbon black is nano-carbon powder, D 50 Not larger than 50nm, and its mass fraction is 1-15%.
[0033] The beneficial effects of the present invention are:
[0034] Compared with the toughening process using a preset two-dimensional or three-dimensional carbon fiber reinforcement, the technical solution of the present invention is simpler, the manufacturing cost is lower, and it still has a good toughening effect, and is particularly suitable for industrial production.
[0035] Compared with the toughening process of directly mixing chopped carbon fiber bundles with granulated powder, the technical solution of the present invention can improve the dispersion uniformity of carbon fibers, thereby improving the uniformity and consistency of the prepared products and increasing the service reliability of the products.
[0036] The carbon fiber debundling process adopted in the present invention is relatively mild and will not cause a significant reduction in the strength of the carbon fiber precursor, thereby being able to better exert the reinforcing and toughening effects of the carbon fiber.
[0037] After the carbon fiber is unbundled, the diameter of the toughened carbon fiber bundle is smaller, and the inhibitory effect on the densification of reaction-sintered silicon carbide ceramics is weakened, so a higher density can be obtained, thereby improving the hardness and wear resistance of the product.
[0038] After the carbon fiber is unbundled, it is coated on the surface of silicon carbide granulated powder. After pressing and forming, the unbundled carbon fiber bundles can be overlapped to form a three-dimensional spatial network, which has a similar effect of toughening a preset three-dimensional braided body, and the technical solution of the present invention is relatively simple.
[0039] The present invention sprays resin and carbon black on the debundled chopped carbon fiber filaments, which can preferentially react with silicon in the siliconizing process to generate silicon carbide, forming a protective layer for the carbon fiber filaments, thereby avoiding reduction in carbon fiber performance during subsequent siliconizing treatment.
[0040] Compared with the existing carbon fiber toughened silicon carbide ceramic process, the process of the present invention is simple, low in production cost, high in production efficiency, and has a better toughening effect. It has obvious comprehensive advantages in cost and performance and is particularly suitable for industrial pressing and molding to prepare high-performance silicon carbide ceramic valve parts. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the embodiments.
[0042] Example 1
[0043] A method for preparing a fiber-reinforced silicon carbide ceramic valve component by reaction sintering and pressing, comprising the following steps:
[0044] (1) Preparation of granulated powder
[0045] Weigh the matrix material according to the ratio: D 50 50 parts of 3μm silicon carbide powder, D 50 35 parts of 15μm silicon carbide powder, D 50 15 parts of 40μm silicon carbide powder, 8 parts of carbon powder, 10 parts of phenolic resin, 0.5 parts of stearic acid, and 0.5 parts of tetramethylammonium hydroxide.
[0046] Then, the weighed matrix material was added into 100 parts of deionized water and ball-milled in a drum ball mill for 8 hours to prepare silicon carbide ceramic slurry.
[0047] The silicon carbide ceramic slurry is then sprayed and granulated using a centrifugal spray tower to obtain granulated powder; the moisture content of the granulated powder is measured to be 0.8%, and the mass ratio of the particle size of 60-180 mesh in the granulated powder is 91.5%.
[0048] The above granulated powder was sieved, and the granulated powder with mesh size between 10 and 100 was taken out, and the weight was 14.5 parts, and the granulated powder was set aside.
[0049] (2) Pretreatment of chopped carbon fiber
[0050] Weigh 100 parts of 3.0 mm long chopped carbon fibers, add them into a ball mill with a polyurethane liner, weigh 30 parts of 15 mm diameter polyurethane balls, and 60 parts of 40 mm diameter polyurethane balls, and roll ball mill for 3 hours to make the chopped carbon fiber bundles fluffy.
[0051] Then, 120 parts of deionized water were added to the ball mill, and the ball mill was performed for 5 hours to initially debundle the chopped carbon fiber bundles.
[0052] The above-mentioned initially debonded chopped carbon fiber bundle is filtered and then added to a polyurethane ball mill. 90 parts of anhydrous ethanol, 30 parts of polyurethane balls with a diameter of 15 mm and 60 parts of polyurethane balls with a diameter of 40 mm are added to the ball mill. Roller ball milling is performed for 6 hours to further debond the chopped carbon fiber bundle. The chopped carbon fiber bundle is then filtered and dried at 60°C to obtain debonded chopped carbon fiber for later use.
[0053] (3) Debundled chopped carbon fiber coated granulated powder
[0054] Weigh 5 parts of the debundled chopped carbon fibers prepared in step (2), add them into a coating machine, start the coating machine, make the debundled chopped carbon fibers start to rotate with the coating machine, spray humidify and viscosity-enhance the chopped carbon fibers with an alcohol solution containing 2% by mass of phenolic resin and 3% by mass of carbon black, then continuously add the 10-100 mesh silicon carbide granulated powder prepared in step (1), and continuously spray the alcohol solution containing phenolic resin and carbon black, so that the debundled chopped carbon fibers adhere to the granulated powder during the rotation of the coating machine, to obtain silicon carbide granulated powder coated with chopped carbon fibers, until all the silicon carbide granulated powder is added.
[0055] The granulated powder coated with the chopped carbon fiber is then dried at 50° C. to make its moisture content 0.7%.
[0056] (4) Silicon carbide granulated powder mixing
[0057] The coated granulated powder obtained in step (3) and the other granulated powders except 10-100 mesh in step (1) are rotated in a sugar coating machine and mixed evenly.
[0058] (5) Valve molding
[0059] The granulated powder obtained in step (4) was placed in a steel mold, vibrated, flattened, and molded into a disk with a diameter of 102 mm and a thickness of 21 mm. The green density was measured to be 1.92 g / cm 3 The disc is then dried at 65°C for 10 hours to obtain a valve green body for later use.
[0060] (6) Valve parts sintering
[0061] The dried valve green body is placed in a vacuum sintering furnace, and metal silicon particles are laid on the bottom and sides of the valve plate green body, with the silicon dosage being 1.2 times the mass of the valve green body. It is then sintered at 1450°C for 6 hours to obtain a silicon carbide ceramic valve sintered body.
[0062] (7) Post-processing of valve parts
[0063] The residual silicon on the surface of the valve component sintered body is removed, and the surface is surface-ground to obtain a silicon carbide ceramic valve plate with a diameter of 100 mm, a thickness of 20 mm, and a surface roughness of 5 microns.
[0064] After testing, the relative density of the obtained silicon carbide ceramic valve plate is 99.1%, the Vickers microhardness is 24.6GPa, the three-point bending strength is 572.9MPa, and the fracture toughness is 7.2MPa·m 1 / 2 .
[0065] Example 2
[0066] A method for preparing a fiber-reinforced silicon carbide ceramic valve component by reaction sintering and pressing, comprising the following steps:
[0067] (1) Preparation of granulated powder
[0068] Weigh the matrix material according to the ratio: D 50 45 parts of 5μm silicon carbide powder, D 50 40 parts of 25μm silicon carbide powder, D 50 15 parts of 50μm silicon carbide powder, 5 parts of carbon powder, 5 parts of phenolic resin, 1.6 parts of stearic acid, and 0.7 parts of tetramethylammonium hydroxide.
[0069] Then, the weighed matrix material was added into 110 parts of deionized water and ball-milled in a drum ball mill for 12 hours to prepare silicon carbide ceramic slurry.
[0070] The silicon carbide ceramic slurry is then sprayed and granulated using a centrifugal spray tower to obtain granulated powder; the moisture content of the granulated powder is measured to be 0.8%, and the mass ratio of the granular particles of 60-180 mesh in the granulated powder is 92.1%.
[0071] The above granulated powder was sieved, and the granulated powder with mesh size between 10 and 100 was taken out, and the weight was 13.6 parts, and it was set aside.
[0072] (2) Pretreatment of chopped carbon fiber
[0073] Weigh 100 parts of 3.5 mm long chopped carbon fibers, add them into a ball mill with a polyurethane liner, weigh 35 parts of 15 mm diameter polyurethane balls, and 70 parts of 40 mm diameter polyurethane balls, and roll mill for 4 hours to make the chopped carbon fiber bundles fluffy.
[0074] Then, 130 parts of deionized water were added to the ball mill, and the ball mill was performed for 6 hours to initially debundle the chopped carbon fiber bundles.
[0075] The above-mentioned initially de-bundled chopped carbon fiber bundle is filtered and then added to a polyurethane ball mill. 100 parts of anhydrous ethanol, 30 parts of polyurethane balls with a diameter of 15 mm and 60 parts of polyurethane balls with a diameter of 40 mm are added to the ball mill. Roller ball milling is performed for 6 hours to further de-bundle the chopped carbon fiber bundle. The chopped carbon fiber bundle is then filtered and dried at 65°C to obtain de-bundled chopped carbon fiber for later use.
[0076] (3) Debundled chopped carbon fiber coated granulated powder
[0077] Weigh 6 parts of the debundled chopped carbon fibers prepared in step (2), add them into a coating machine, start the coating machine, make the debundled chopped carbon fibers start to rotate with the coating machine, spray humidify and viscosity-enhance the chopped carbon fibers with an alcohol solution containing 3% by mass of phenolic resin and 5% by mass of carbon black, then continuously add the 10-100 mesh silicon carbide granulated powder prepared in step (1), and continuously spray the alcohol solution containing phenolic resin and carbon black, so that the debundled chopped carbon fibers adhere to the granulated powder during the rotation of the coating machine, to obtain silicon carbide granulated powder coated with chopped carbon fibers, until all the silicon carbide granulated powder is added.
[0078] The granulated powder coated with the chopped carbon fiber is then dried at 60° C. to make its moisture content 0.8%.
[0079] (4) Silicon carbide granulated powder mixing
[0080] The coated granulated powder obtained in step (3) and the other granulated powders except 10-100 mesh in step (1) are rotated in a sugar coating machine and mixed evenly.
[0081] (5) Valve molding
[0082] The granulated powder obtained in step (4) was loaded into a spherical rubber mold, compacted, cold isostatically pressed, and turned to obtain a sphere with a diameter of 71 mm. The green density was measured to be 1.94 g / cm 3 The ball is then dried at 60°C for 12 hours to obtain a valve ball green body for later use.
[0083] (6) Valve parts sintering
[0084] The dried valve ball green body is placed in a vacuum sintering furnace, and metal silicon particles are laid on the bottom and sides of the valve ball green body. The silicon dosage is 1.3 times the mass of the valve body. It is then sintered at 1480°C for 5 hours to obtain a silicon carbide ceramic valve ball sintered body.
[0085] (7) Post-processing of valve parts
[0086] The residual silicon on the surface of the valve ball sintered body is removed, and the surface of the valve ball is ground to obtain a silicon carbide ceramic valve ball with a diameter of 70 mm and a surface roughness of 1 micron.
[0087] After testing, the relative density of the obtained silicon carbide ceramic valve ball is 98.9%, the Vickers microhardness is 24.3GPa, the three-point bending strength is 617.4MPa, and the fracture toughness is 7.8MPa·m 1 / 2 .
[0088] Example 3
[0089] A method for preparing a fiber-reinforced silicon carbide ceramic valve component by reaction sintering and pressing, comprising the following steps:
[0090] (1) Preparation of granulated powder
[0091] Weigh the matrix material according to the ratio: D 50 53 parts of 10 μm silicon carbide powder, D 50 32 parts of 30μm silicon carbide powder, D 50 15 parts of 60μm silicon carbide powder, 20 parts of carbon powder, 15 parts of phenolic resin, 3 parts of fatty acid glyceride, and 2 parts of polyacrylic acid.
[0092] Then, the weighed matrix material was added into 130 parts of deionized water and ball-milled in a drum ball mill for 15 hours to prepare silicon carbide ceramic slurry.
[0093] The silicon carbide ceramic slurry is then sprayed and granulated using a centrifugal spray tower to obtain granulated powder; the moisture content of the granulated powder is measured to be 0.9%, and the mass ratio of the granular powder with a particle size of 60-180 mesh is 91%.
[0094] The above granulated powder is sieved, and the granulated powder with mesh size between 10 and 100 is taken out, and the weight is 15 parts, and it is set aside.
[0095] (2) Pretreatment of chopped carbon fiber
[0096] Weigh 100 parts of 4 mm long chopped carbon fibers, add them into a ball mill with a polyurethane liner, weigh 30 parts of 20 mm diameter polyurethane balls, and 60 parts of 50 mm diameter polyurethane balls, and roll mill for 4 hours to make the chopped carbon fiber bundles fluffy.
[0097] Then, 130 parts of deionized water were added to the ball mill, and the ball mill was performed for 4 hours to initially debundle the chopped carbon fiber bundles.
[0098] The above-mentioned initially debonded chopped carbon fiber bundle is filtered and then added to a polyurethane ball mill. 105 parts of anhydrous ethanol, 30 parts of polyurethane balls with a diameter of 15 mm and 60 parts of polyurethane balls with a diameter of 40 mm are added to the ball mill. Roller ball milling is performed for 5 hours to further debond the chopped carbon fiber bundle. The chopped carbon fiber bundle is then filtered and dried at 60°C to obtain debonded chopped carbon fiber for later use.
[0099] (3) Debundled chopped carbon fiber coated granulated powder
[0100] Weigh 5 parts of the debundled chopped carbon fibers prepared in step (2), add them into a coating machine, start the coating machine, make the debundled chopped carbon fibers start to rotate with the coating machine, spray humidify and viscosity-enhance the chopped carbon fibers with an alcohol solution containing 4% by mass of phenolic resin and 6% by mass of carbon black, then continuously add the 10-100 mesh silicon carbide granulated powder prepared in step (1), and continuously spray the alcohol solution containing phenolic resin and carbon black, so that the debundled chopped carbon fibers adhere to the granulated powder during the rotation of the coating machine, to obtain silicon carbide granulated powder coated with chopped carbon fibers, until all the silicon carbide granulated powder is added.
[0101] The granulated powder coated with the chopped carbon fiber is then dried at 50° C. to make its moisture content 0.8%.
[0102] (4) Silicon carbide granulated powder mixing
[0103] The coated granulated powder obtained in step (3) and the other granulated powders except 10-100 mesh in step (1) are rotated in a sugar coating machine and mixed evenly.
[0104] (5) Valve molding
[0105] The granulated powder obtained in step (4) was loaded into a rubber mold, compacted, isostatically pressed, and turned to obtain a valve sleeve with an outer diameter of 81 mm, an inner diameter of 61 mm, and a height of 71 mm. The green density was measured to be 1.82 g / cm 3 The disc is then dried at 60°C for 15 hours to obtain a valve green body for later use.
[0106] (6) Valve parts sintering
[0107] The dried valve sleeve green body is placed in a vacuum sintering furnace, and metal silicon particles are laid on the bottom and sides of the valve sleeve green body, with the silicon dosage being 1.5 times the mass of the valve body. It is then sintered at 1500°C for 54 hours to obtain a silicon carbide ceramic valve sleeve sintered body.
[0108] (7) Post-processing of valve parts
[0109] The inner and outer surfaces of the valve sleeve were surface ground to obtain a valve sleeve with an outer diameter of 80 mm, an inner diameter of 60 mm, a height of 70 mm, and a surface roughness of 5 microns.
[0110] After testing, the relative density of the obtained silicon carbide ceramic valve sleeve is 99%, the Vickers microhardness is 24.2GPa, the three-point bending strength is 590.2MPa, and the fracture toughness is 7.9MPa·m 1 / 2 .
[0111] Comparative Example 1:
[0112] A method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing, the steps are as follows:
[0113] The technical solution refers to Example 1.
[0114] The difference is that no chopped carbon fiber is added for toughening.
[0115] The rest is the same as Example 1.
[0116] After testing, the relative density of the silicon carbide ceramic valve plate obtained is 99.2%, the Vickers microhardness is 25.3GPa, the three-point bending strength is 413.6MPa, and the fracture toughness is 4.2MPa·m 1 / 2 .
[0117] Comparative Example 2:
[0118] A method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing, the steps are as follows:
[0119] The technical solution refers to Example 1.
[0120] The difference is:
[0121] The pretreatment of the carbon fiber in step 2 is removed, the silicon carbide granulated powder is not coated with the carbon fiber, and the chopped carbon fiber and the granulated powder are simply mechanically mixed.
[0122] The rest is the same as Example 1.
[0123] After testing, the obtained silicon carbide ceramic valve plate has a relative density of 98.1%, a Vickers microhardness of 23.8GPa, a three-point bending strength of 503.6MPa, and a fracture toughness of 6.2MPa·m 1 / 2 .
[0124] Comparative Example 3:
[0125] A method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing, the steps are as follows:
[0126] The technical solution refers to Example 1.
[0127] The difference is that the chopped carbon fiber with a length of 3.0 mm is replaced with the chopped carbon fiber with a length of 30 mm.
[0128] The rest is the same as Example 1.
[0129] After testing, the relative density of silicon carbide ceramic valve plate is 98.4%, the Vickers microhardness is 24.1GPa, the three-point bending strength is 550.3MPa, and the fracture toughness is 6.6MPa.m 1 / 2 .
[0130] Comparative Example 4:
[0131] A method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing, the steps are as follows:
[0132] The technical solution refers to Example 1.
[0133] The difference is that when the silicon carbide granulated powder is coated with debonded carbon fibers, the sprayed alcohol solution does not contain nano carbon black but only contains resin.
[0134] The rest is the same as Example 1.
[0135] After testing, the relative density of silicon carbide ceramic valve plate is 99.2%, the Vickers microhardness is 25.6GPa, the three-point bending strength is 540.8MPa, and the fracture toughness is 6.5MPa.m 1 / 2 .
[0136] Result analysis:
[0137] 1. By comparing Example 1 with Comparative Examples 1-3, it can be seen that the technical solution of the present invention, by introducing chopped carbon fibers of suitable sizes, debundling the carbon fibers, and spraying an alcohol solution containing resin and carbon black on the debundled carbon fibers, can achieve a good toughening effect.
[0138] 2. By comparing Example 1 with Comparative Example 2, it can be seen that the technical solution of the present invention, by unbundling the chopped carbon fibers and coating the unbundled carbon fiber filaments on the surface of the silicon carbide granulated powder, can improve the density of the valve parts, improve the uniformity of fiber distribution, and achieve better strengthening and toughening effects. If the chopped carbon fibers are directly mixed with the granulated powder, the density will be reduced, and the strengthening and toughening effects will be worse.
[0139] 3. By comparing Example 1 with Comparative Example 3, it can be seen that the technical solution of the present invention uses a carbon fiber bundle of appropriate size, which can be better coated on the surface of the granulated powder after being unbundled. If the carbon fiber is too long, even after being unbundled, its length far exceeds the circumference of the granulated powder, making the carbon fiber bundle too long, resulting in poor coating effect, reduced density of the valve part, and poor strength and toughness.
[0140] 4. By comparing Example 1 with Comparative Example 4, it can be seen that the technical solution of the present invention, spraying an alcohol solution containing nanocarbon black on the debundled carbon fiber filaments, can preferentially react with silicon in the siliconization process to generate silicon carbide, forming a protective layer for the carbon fiber filaments, and avoiding the reduction of the carbon fiber performance during the subsequent siliconization treatment. While the comparative sample sprayed with an alcohol solution without nanocarbon black, although the density and hardness did not deteriorate, its strength and toughness were significantly reduced. This should be because silicon directly reacted with the carbon fiber filaments during the siliconization process, resulting in the deterioration of the performance of the carbon fiber filaments, thereby deteriorating the strengthening and toughening effects.
[0141] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing fiber-reinforced silicon carbide ceramic valve parts by reaction sintering and pressing, characterized in that: The raw materials for preparing ceramic valve parts include silicon carbide ceramic matrix material and toughening material; the matrix material includes 100 parts of silicon carbide micropowder, 5-20 parts of carbon powder, 5-15 parts of adhesive, 0.5-3 parts of surfactant and 0.5-2 parts of dispersant by weight; the toughening material is chopped carbon fiber, the length of the chopped carbon fiber is less than 5mm, the diameter of the filament bundle is less than 500μm, and the addition amount of the chopped carbon fiber is 0.1-15% of the total amount of the matrix material; the preparation method specifically includes the following steps: (1) Preparation of granulated powder Weigh the above matrix materials according to the ratio, add deionized water, the amount of deionized water is 0.9-1.5 times the mass of silicon carbide micropowder, and then ball mill for 8-20 hours to obtain silicon carbide ceramic slurry; then spray granulate the silicon carbide ceramic slurry to obtain granulated powder, wherein the moisture content of the granulated powder is 0.5-1.2%, and the mass percentage of the particle size of 60-180 mesh in the granulated powder is greater than 90%, and then sieve the granulated powder to take the granulated powder between 10-100 mesh for standby use; (2) Pretreatment of chopped carbon fiber Weigh the chopped carbon fibers and add them to a ball mill with a polyurethane liner, then add polyurethane balls to the ball mill, and perform roller milling for 1-5 hours to make the chopped carbon fiber bundles fluffy; then add deionized water to the ball mill, and continue roller milling for 1-8 hours to preliminarily debundle the chopped carbon fiber bundles; then filter the treated chopped carbon fiber bundles, add them to the ball mill, add anhydrous ethanol and polyurethane balls to the ball mill, and perform roller milling for 1-8 hours to further debundle the chopped carbon fiber bundles, then filter and dry to obtain debundled chopped carbon fibers for standby use; (3) Debundled chopped carbon fiber coated granulated powder The chopped carbon fibers prepared in step (2) are added to a coating machine, the coating machine is started, the debundled chopped carbon fibers begin to rotate with the coating machine, the chopped carbon fibers are sprayed with an alcohol solution containing phenolic resin and carbon black to humidify and thicken them, and then the 10-100 mesh granulation powder prepared in step (1) is added, and the alcohol solution containing phenolic resin and carbon black is continuously sprayed, so that the debundled chopped carbon fibers adhere to the granulation powder during the rotation of the coating machine, thereby obtaining carbon fiber-coated silicon carbide granulation powder; and the carbon fiber-coated silicon carbide granulation powder is dried at a temperature not higher than 70° C. to have a moisture content of 0.5-1.2%; (4) Silicon carbide granulated powder mixing The carbon fiber-coated silicon carbide granulated powder obtained in step (3) and the other granulated powders except 10-100 mesh in step (1) are mixed uniformly in a sugar coating machine; (5) Valve molding The granulated powder obtained in step (4) is pressed and molded to obtain a valve green body, wherein the density of the valve green body is 1.80-2.10 g / cm 3 ; (6) Valve parts sintering The processed valve green body is placed in a vacuum sintering furnace, and metal silicon particles are laid on the bottom and side of the valve green body, and then kept at 1450-1800°C for 1-8 hours to obtain a silicon carbide ceramic valve sintered body; (7) Post-processing of valve parts The silicon carbide ceramic valve component sintered body is subjected to post-processing treatments such as grinding and polishing to obtain silicon carbide ceramic valve components of required specifications, shapes and sizes.
2. The method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing according to claim 1, characterized in that: The silicon carbide powder is made of D 50 3-10μm silicon carbide powder, D 50 15-30μm silicon carbide powder and D 50 The silicon carbide powder with a size of 40-60 μm is mixed in a mass ratio of (3-8):(2-4):
1.
3. The method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing according to claim 1, characterized in that: The adhesive is phenolic resin, polyvinyl alcohol or carboxymethyl cellulose; the surfactant is stearic acid or fatty acid glyceride; and the dispersant is tetramethylammonium hydroxide or polyacrylic acid.
4. The method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing according to claim 1, characterized in that: The toner D 50 Less than 200nm.
5. The method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing according to claim 1, characterized in that: The chopped carbon fiber is a high-strength carbon fiber with a tensile strength of not less than 3500 MPa.
6. The method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing according to claim 1, characterized in that: The diameter of the polyurethane ball in step (2) is 10-50 mm.
7. The method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing according to claim 1, characterized in that: The mass ratio of the polyurethane balls to the chopped carbon fibers in step (2) is (0.6-1.5):1; the mass ratio of the deionized water to the chopped carbon fibers is (0.8-2):1; The mass ratio of anhydrous ethanol to short-cut carbon fibers is (0.8-1.5):1; the drying temperature in step (2) is 50-80°C.
8. The method for preparing fiber-reinforced silicon carbide ceramic valve components by reaction sintering and pressing according to claim 1, characterized in that: The mass fraction of the phenolic resin in the alcohol solution in step (3) is 1-10%, the mass fraction of the carbon black is 1-15%, and the carbon black is nano carbon powder. 50 Not larger than 50nm.