Multi-band SWIR photodetector devices, their fabrication methods, and imaging systems
By combining a Si-based detector with a core-shell-shell structured NaYF4 upconversion nanomaterial, the technical gap of InGaAs focal plane array detectors in SWIR band detection has been overcome, enabling multi-band SWIR imaging, reducing costs and improving detection sensitivity and stability.
Patent Information
- Application Number
- CN202310929858.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-27
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-07-27
AI Technical Summary
Existing InGaAs focal plane array detectors lag significantly behind foreign technologies in terms of array size, detection sensitivity, reliability, and product cost, making it difficult to achieve selective detection in the SWIR band. Furthermore, the application of Si detectors in the SWIR band is limited.
By combining a Si-based detector with a core-shell-shell structured NaYF4 upconversion nanomaterial doped with rare earth elements, various upconversion nanoparticles were synthesized via a solvothermal method and spin-coated onto a Si-based detector. This enabled the conversion of light excitation in the 1150nm, 1208nm, 1500nm, and 2300nm bands into VIS-NIR light. Combined with a high-definition NIR industrial camera, multi-band SWIR imaging was achieved.
It enables narrowband photoelectric detection and nighttime visualization imaging in the SWIR band, reduces device costs, improves detection sensitivity and stability, is suitable for mass production, and broadens the application range of SWIR imaging.
Smart Images

Figure CN116960195B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photoelectric detection technology, specifically a multi-band SWIR photoelectric detection device, its fabrication method, and imaging system. Background Technology
[0002] The 1.5-2.0 micrometer short-wave infrared light is a wavelength safe for the human eye, a band suitable for optical communication, and an atmospheric transmission window. Therefore, designing a photodetector that can selectively detect near-infrared-short-wave infrared light (NIR-SWIR) and realizing a highly sensitive multi-band selective photodetector for near-infrared-short-wave infrared light is of great significance in fields such as optical communication, environmental monitoring, lidar, laser medicine, and military applications.
[0003] Currently, InGaAs focal plane array detectors are widely used. These are hybrid SWIR imaging devices, consisting of an InGaAs detector array and a CMOS readout circuit interconnected via flip-chip bonding. However, focal plane array technology encompasses both optoelectronics and microelectronics, resulting in complex structures and significant technical challenges, requiring high levels of expertise in design, manufacturing processes, and commercialization. Major foreign manufacturers have imposed strict embargoes on InGaAs focal plane array detectors. Compared to foreign technologies, domestic InGaAs focal plane array detectors lag significantly in terms of array size, detection sensitivity, reliability, and cost. Further improvements in product technology are needed to advance their application in the civilian market. Under these circumstances, the widespread use of short-wave infrared InGaAs focal plane array detectors in the domestic civilian market is severely limited.
[0004] Commercial silicon (Si) photodetectors are crucial components of optoelectronic devices, serving as primary detectors in the visible light (VIS) and NIR bands. They exhibit high sensitivity at room temperature and demonstrate excellent long-term stability after packaging. Furthermore, Si detectors can be combined with accessories such as filters (long-wavelength and bandpass filters), preamplifiers, and fiber optic connectors, enabling their application in industrial control systems, gas analysis, thermal sensors, and fiber optic testing equipment, showing broad application prospects. However, the operating wavelength of typical Si detectors is between 0.3 and 1.0 micrometers, making selective detection of SWIR difficult. Rare-earth-doped upconversion nanocrystals (UCNCs), due to their 4f electron configuration, possess narrow-band NIR-SWIR absorption characteristics, enabling them to perform NIR-SWIR photon conversion, such as converting photons at 1150, 1208, 1500, and 2300 nm into VIS-NIR photons via an anti-Stokes process. Currently, narrowband NIR PDs (with a full width at half maximum of approximately 30-50 nm) based on UCNPs have been achieved, with a specific detectivity D* = ~10 8-11Jones. Therefore, UCNPs are considered suitable photoactive materials for the fabrication of narrowband NIRPDs. However, to date, no UCNC-based visualization imaging SWIR narrowband photodetector devices have been reported, especially for the 1550nm and 2300nm bands, which are crucial for optical communications, military applications, environmental monitoring, lidar, and industrial imaging. Summary of the Invention
[0005] The purpose of this invention is to provide a multi-band SWIR photodetector to solve the problems mentioned in the background art.
[0006] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions:
[0007] A multi-band SWIR photodetector includes a detector, wherein the detector is provided with a first upconversion nanoparticle, a second upconversion nanoparticle, a third upconversion nanoparticle, and a fourth upconversion nanoparticle that can be excited by light of 1150nm, 1208nm, 1500nm and 2300nm to generate VIS-NIR light respectively.
[0008] The first upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Ho and Yb; the second upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Tm and Yb; the third upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Er and Yb; and the fourth upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Ho and Yb.
[0009] Preferably, the first upconversion nanoparticles include NaYF4 doped with Ho, NaYF4 doped with Yb, and NaYF4; wherein the doping amount of Ho is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction.
[0010] Preferably, the second upconversion nanoparticles include NaYF4 doped with Tm, NaYF4 doped with Yb, and NaYF4; wherein the doping amount of Tm is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction.
[0011] Preferably, the third upconversion nanoparticles include Er-doped NaYF4, Yb-doped NaYF4, and NaYF4; wherein the doping amount of Er is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction.
[0012] Preferably, the fourth upconversion nanoparticles include NaYF4 doped with Ho, NaYF4 doped with Yb, and NaYF4; wherein the doping amount of Ho is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction.
[0013] Preferably, the detector is a Si-based detector.
[0014] Another objective of this invention is to provide a method for fabricating the above-mentioned multi-band SWIR photodetector, which includes the following steps:
[0015] The first, second, third, and fourth upconversion nanoparticles were synthesized by a solvothermal method.
[0016] The first, second, third, and fourth upconversion nanoparticles were dissolved in cyclohexane and then spin-coated onto the detector to obtain the multi-band SWIR photodetector.
[0017] Another objective of this invention is to provide a multi-band SWIR photodetector device prepared using the above-described method.
[0018] Another objective of this invention is to provide an imaging system, including an industrial camera and the aforementioned multi-band SWIR photodetector.
[0019] The multi-band SWIR photodetector provided by this invention can be used to detect SWIR at 1150nm, 1208nm, 1500nm, and 2300nm, and to achieve nighttime visualization imaging of multi-band SWIR. Specifically, the first, second, third, and fourth upconversion nanoparticles can convert excitation light into VIS-NIR light through an anti-Stokes process under laser irradiation at 1150nm, 1208nm, 1500nm, and 2300nm, respectively, which is then effectively captured by Si-based detectors to achieve narrowband detection. Compared to ordinary Si-based detectors, this invention, by combining the detector with the first, second, third, and fourth upconversion nanoparticles, can broaden its response band to the short-wave infrared region, achieving narrowband light detection of SWIR. Furthermore, the multi-band SWIR photodetector provided by this invention, when combined with a 2MP high-definition near-infrared 700-1000nm narrowband industrial camera, can be used for nighttime short-wave infrared visualization imaging.
[0020] Compared to commonly used InGaAs focal plane array detectors, the multi-band SWIR photodetector provided by this invention has a simpler design structure, lower cost, better stability, and the advantage of large-scale production. Utilizing the narrow-band absorption and anti-Stokes luminescence properties of upconversion nanomaterials, narrow-band detection of SWIR can be innovatively achieved, which is more conducive to the widespread application of the device in manufacturing, military, and other fields. Attached Figure Description
[0021] Figure 1 This is a flowchart illustrating the fabrication process of a multi-band SWIR photodetector and imaging system provided in an embodiment of the present invention.
[0022] Figure 2 A physical diagram of the imaging system provided in an embodiment of the present invention.
[0023] Figure 3 This is a TEM image of the first upconversion nanoparticles prepared in Example 1.
[0024] Figure 4 The photocurrent response diagrams of the SWIR photodetector device prepared in Example 1 under illumination at 1150nm, 1208nm, 1500nm and 2300nm are shown.
[0025] Figure 5 This is an actual imaging effect diagram of the imaging system obtained in Example 1. Detailed Implementation
[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] Existing SWIR imaging devices are generally based on InGaAs focal plane array detectors, which are formed by flip-chip interconnection of InGaAs detector arrays and CMOS readout circuits. The fabrication of such detectors involves focal plane array technology, which has very high requirements for design, manufacturing processes, and commercialization. The device structure is complex, and the optical system design is challenging. Major foreign manufacturers have imposed strict embargoes on InGaAs focal plane array detectors. Compared with foreign technology, domestic InGaAs focal plane detectors still lag significantly behind in terms of array size, detection sensitivity, reliability, and product cost, becoming a true "bottleneck" technology.
[0028] To address the aforementioned challenges, this invention aims to design a Si-based detector / upconversion nanomaterial composite structure, combined with a high-definition NIR (700-1000nm) narrowband industrial camera, to achieve multi-band narrowband photoelectric detection of SWIR and a nighttime shortwave infrared visualization imaging system. Compared to InGaAs focal plane array detectors, Si-based detectors are less expensive, require less advanced manufacturing technology, have a relatively mature market, and are easy to mass-produce. Meanwhile, upconversion nanomaterials possess narrowband absorption spectral characteristics, with absorption peaks covering the NIR-SWIR range. Furthermore, the absorption and emission peak positions can be tuned by different rare-earth doping ions. This material exhibits low toxicity and no background fluorescence, making it a high-performance narrowband photoelectric material for combination with Si-based detectors.
[0029] Specifically, in one embodiment of the present invention, a multi-band SWIR photodetector includes a detector, wherein the detector is provided with a first upconversion nanoparticle, a second upconversion nanoparticle, a third upconversion nanoparticle, and a fourth upconversion nanoparticle that can be excited by light of 1150nm, 1208nm, 1500nm and 2300nm to generate VIS-NIR light respectively.
[0030] The first upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Ho and Yb; the second upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Tm and Yb; the third upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Er and Yb; and the fourth upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Ho and Yb.
[0031] Furthermore, the first upconversion nanoparticles include NaYF4 doped with Ho, NaYF4 doped with Yb, and NaYF4, denoted as Ho@Yb@Y; wherein the doping amount of Ho is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction. The first upconversion nanoparticles can have structures such as NaYF4:5%-80%Ho@NaYF4:5%-80%Yb@NaYF4 (abbreviated as 5%-80%Ho@5%-80%Yb@Y), NaYF4:5%-80%Yb@NaYF4:5%-80%Ho@NaYF4 (abbreviated as 5%-80%Yb@5%-80%Ho@Y), and NaYF4:5%-80%Yb@NaYF4@NaYF4:5%-80%Ho (abbreviated as 5%-80%Yb@Y@5%-80%Ho) according to the core-shell-shell structure, but are not limited to these.
[0032] Furthermore, the second upconversion nanoparticles include NaYF4 doped with Tm, NaYF4 doped with Yb, and NaYF4, denoted as Tm@Yb@Y; wherein the doping amount of Tm is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction. The second upconversion nanoparticles can have structures such as NaYF4:5%-80%Tm@NaYF4:5%-80%Yb@NaYF4 (abbreviated as 5%-80%Tm@5%-80%Yb@Y), NaYF4:5%-80%Yb@NaYF4:5%-80%Tm@NaYF4 (abbreviated as 5%-80%Yb@5%-80%Tm@Y), and NaYF4:5%-80%Yb@NaYF4@NaYF4:5%-80%Tm (abbreviated as 5%-80%Yb@Y@5%-80%Tm) according to the core-shell-shell structure, but are not limited to these.
[0033] Furthermore, the third upconversion nanoparticles include Er-doped NaYF4, Yb-doped NaYF4, and NaYF4, denoted as Yb@Er@Y; wherein the doping amount of Er is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction. The third upconversion nanoparticles can have structures such as NaYF4:5%-80%Yb@NaYF4:5%-80%Er@NaYF4 (abbreviated as 5%-80%Yb@5%-80%Er@Y), NaYF4:5%-80%Er@NaYF4:5%-80%Yb@NaYF4 (abbreviated as 5%-80%Er@5%-80%Yb@Y), and NaYF4:5%-80%Yb@NaYF4@NaYF4:5%-80%Er (abbreviated as 5%-80%Yb@Y@5%-80%Er) according to the core-shell-shell structure, but are not limited to these.
[0034] Furthermore, the fourth upconversion nanoparticles include NaYF4 doped with Ho, NaYF4 doped with Yb, and NaYF4, denoted as Ho@Yb@Y-2; wherein the doping amount of Ho is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction. The fourth upconversion nanoparticles can have structures such as NaYF4:5%-80%Ho@NaYF4:5%-80%Yb@NaYF4 (abbreviated as 5%-80%Ho@5%-80%Yb@Y), NaYF4:5%-80%Yb@NaYF4:5%-80%Ho@NaYF4 (abbreviated as 5%-80%Yb@5%-80%Ho@Y), and NaYF4:5%-80%Yb@NaYF4@NaYF4:5%-80%Ho (abbreviated as 5%-80%Yb@Y@5%-80%Ho) according to the core-shell-shell structure, but are not limited to these.
[0035] Furthermore, the detector is a Si-based detector.
[0036] As attached Figure 1 As shown, in another embodiment of the present invention, a method for fabricating the above-mentioned multi-band SWIR photodetector and imaging system is also provided, which includes the following steps:
[0037] S1. The first upconversion nanoparticle, the second upconversion nanoparticle, the third upconversion nanoparticle, and the fourth upconversion nanoparticle were synthesized by a solvothermal method.
[0038] S2. The first, second, third, and fourth upconversion nanoparticles were dissolved in cyclohexane to obtain a cyclohexane solution of upconversion nanoparticles with a molar concentration of 0.01-0.8 mol / L. This solution was then spin-coated onto a commercial Si-based detector to obtain a multi-band SWIR photodetector. The spin-coating parameters were set as follows: low speed 200-1000 rpm, held for 2-10 s; high speed 2000-8000 rpm, held for 20-100 s.
[0039] S3. The above-mentioned multi-band SWIR photodetector (i.e., Si-based detector / upconversion nanoparticle composite structure) is combined with a commercially available high-definition NIR narrowband (700-1000nm) industrial camera to form a multi-band SWIR visualization imaging system. Its physical image is shown below. Figure 2 As shown.
[0040] The multi-band SWIR photodetector provided in this invention has a simple design structure, simple manufacturing technology, low cost, good stability, and can be mass-produced and manufactured, making it highly practical. It solves the problems of complex device structure, high optical system design difficulty, low detection sensitivity, and high product cost of current SWIR imaging devices, and can realize multi-band narrowband photodetection of SWIR and visualization imaging under dark conditions.
[0041] The following embodiments are some specific implementation examples of the present invention in practical applications, but are not limited thereto.
[0042] Example 1
[0043] This embodiment provides a method for fabricating the above-mentioned multi-band SWIR photodetector and imaging system, which includes the following steps:
[0044] S1. First upconversion nanoparticles (20% Ho@15% Yb@Y), second upconversion nanoparticles (20% Tm@15% Yb@Y), third upconversion nanoparticles (15% Yb@20% Er@Y), and fourth upconversion nanoparticles (60% Ho@15% Yb@Y) were synthesized by the classic solvothermal method. They can be excited by light at 1150 nm, 1208 nm, 1500 nm, and 2300 nm, respectively, to generate VIS-NIR light, which can then be effectively captured by a Si-based detector to achieve narrowband detection.
[0045] Specifically, the synthesis method of the first upconversion nanoparticles (20% Ho@15% Yb@Y) is as follows:
[0046] Step 1: Take 0.076g of holmium chloride hexahydrate powder and 0.243g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0047] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0048] Step 3: Aliquot the mixed solution B obtained in Step 2 into centrifuge tubes. Add 15 mL of ethanol solution to each tube, centrifuge at 10000 rpm for 20 min, then discard the supernatant. Add 16 mL of cyclohexane solution, sonicate to dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:20%Ho precipitate. Its TEM image is shown below. Figure 3 As shown in a.
[0049] Step 4: Core-shell structured upconversion nanoparticles were prepared using a homogeneous encapsulation method. Specifically, 0.06 g of ytterbium chloride hexahydrate powder and 0.26 g of yttrium chloride hexahydrate powder were placed in a three-necked flask, along with the NaYF4:20%Ho precipitate obtained in Step 3. Then, 6 mL of oleic acid and 15 mL of octadecene solution were added. The mixture was fixed in an oil bath and stirred at 700 rpm at 160°C under nitrogen protection until the reagents in the three-necked flask were completely dissolved. The mixture was then cooled to 30°C. Steps 2-3 were repeated to obtain the NaYF4:20%Ho@NaYF4:15%Yb precipitate, and its TEM image is shown below. Figure 3 As shown in b.
[0050] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 20% Ho@15% Yb@Y first upconversion nanoparticles with a core-shell-shell structure. The TEM image is shown below. Figure 3 As shown in c.
[0051] Specifically, the synthesis method of the second upconversion nanoparticles (20% Tm@15% Yb@Y) is as follows:
[0052] Step 1: Take 0.077g of thulium chloride hexahydrate powder and 0.243g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0053] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0054] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:20%Tm precipitate.
[0055] Step 4: Core-shell structured upconversion nanoparticles were prepared using a homogeneous encapsulation method. Specifically, 0.06 g of yttrium chloride hexahydrate powder and 0.26 g of yttrium chloride hexahydrate powder were placed in a three-necked flask, along with the NaYF4:20%Tm precipitate obtained in Step 3. Then, 6 mL of oleic acid and 15 mL of octadecene solution were added. The mixture was fixed in an oil bath and stirred at 700 rpm under nitrogen protection at 160°C until the reagents in the three-necked flask were completely dissolved. The mixture was then cooled to 30°C. Steps 2-3 were repeated to obtain the NaYF4:20%Tm@NaYF4:15%Yb precipitate.
[0056] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 20% Tm@15% Yb@Y second upconversion nanoparticles with a core-shell-shell structure.
[0057] Specifically, the synthesis method of the third upconversion nanoparticles (15% Yb@20% Er@Y) is as follows:
[0058] Step 1: Take 0.058g of ytterbium chloride hexahydrate powder and 0.258g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0059] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0060] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:15%Yb precipitate.
[0061] Step 4: Prepare core-shell structured upconversion nanoparticles using a homogeneous encapsulation method. Specifically, take 0.076 g of erbium chloride hexahydrate powder and 0.243 g of yttrium chloride hexahydrate powder in a three-necked flask, and simultaneously add the NaYF4:15%Yb precipitate obtained in Step 3. Then add 6 mL of oleic acid and 15 mL of octadecene solution, fix the flask in an oil bath, and stir at 700 rpm under nitrogen protection at 160 °C until the reagents in the three-necked flask are completely dissolved. Then cool to 30 °C. Repeat steps 2-3 to obtain NaYF4:15%Yb@NaYF4:20%Er precipitate.
[0062] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 15% Yb@20% Er@Y third upconversion nanoparticles with a core-shell-shell structure.
[0063] Specifically, the synthesis method of the fourth upconversion nanoparticles (60% Ho@15% Yb@Y) is as follows:
[0064] Step 1: Take 0.228g of holmium chloride hexahydrate powder and 0.121g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0065] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0066] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:60%Ho precipitate.
[0067] Step 4: Prepare core-shell structured upconversion nanoparticles using a homogeneous encapsulation method. Specifically, take 0.06 g of ytterbium chloride hexahydrate powder and 0.26 g of yttrium chloride hexahydrate powder in a three-necked flask, add the NaYF4:60%Ho precipitate obtained in Step 3, then add 6 mL of oleic acid and 15 mL of octadecene solution. Fix the flask in an oil bath and stir at 700 rpm under nitrogen protection at 160°C until the reagents in the three-necked flask are completely dissolved. Then cool to 30°C. Repeat steps 2-3 to obtain NaYF4:60%Ho@NaYF4:15%Yb precipitate.
[0068] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 60% Ho@15% Yb@Y fourth upconversion nanoparticles with a core-shell-shell structure.
[0069] S2. Dissolve the precipitates of each of the synthesized upconversion nanoparticles in cyclohexane to obtain a cyclohexane solution of upconversion nanoparticles with a molar concentration of 0.5 mol / L.
[0070] S3. Using a spin coater, the cyclohexane solution of the upconversion nanoparticles was spin-coated onto a commercial Si-based detector to obtain a Si-based detector / upconversion nanoparticle composite structure, which is the multi-band SWIR photodetector device. The spin coater parameters were set as follows: low speed 1000 rpm, hold for 10 s; high speed 4000 rpm, hold for 20 s. This multi-band SWIR photodetector device exhibits significant photocurrent responses to light at 1150 nm, 1208 nm, 1500 nm, and 2300 nm, as detailed below. Figure 4 As shown.
[0071] S4. Combine the above-mentioned multi-band SWIR photodetector with a commercially available NIR narrowband (700-1000nm) industrial camera to form a multi-band SWIR visualization imaging system. This system can be used to detect light at 1150nm, 1208nm, 1500nm, and 2300nm in dark conditions. The actual imaging effect is shown in the image below. Figure 5 As shown.
[0072] Example 2
[0073] This embodiment provides a method for fabricating the above-mentioned multi-band SWIR photodetector and imaging system, which includes the following steps:
[0074] S1. First upconversion nanoparticles (40% Ho@25% Yb@Y), second upconversion nanoparticles (40% Tm@25% Yb@Y), third upconversion nanoparticles (40% Yb@25% Er@Y), and fourth upconversion nanoparticles (50% Ho@25% Yb@Y) were synthesized by the classic solvothermal method. They can be excited by light at 1150 nm, 1208 nm, 1500 nm, and 2300 nm, respectively, to generate VIS-NIR light, which can then be effectively captured by a Si-based detector to achieve narrowband detection.
[0075] Specifically, the synthesis method of the first upconversion nanoparticles (40% Ho@25% Yb@Y) is as follows:
[0076] Step 1: Take 0.152g of holmium chloride hexahydrate powder and 0.182g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0077] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0078] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:40%Ho precipitate.
[0079] Step 4: Prepare core-shell structured upconversion nanoparticles using a homogeneous encapsulation method. Specifically, take 0.097 g of ytterbium chloride hexahydrate powder and 0.228 g of yttrium chloride hexahydrate powder in a three-necked flask, add the NaYF4:40%Ho precipitate obtained in Step 3, then add 6 mL of oleic acid and 15 mL of octadecene solution. Fix the flask in an oil bath and stir at 700 rpm under nitrogen protection at 160 °C until the reagents in the three-necked flask are completely dissolved. Then cool to 30 °C. Repeat steps 2-3 to obtain NaYF4:40%Ho@NaYF4:25%Yb precipitate.
[0080] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 40% Ho@25% Yb@Y first upconversion nanoparticles with a core-shell-shell structure.
[0081] Specifically, the synthesis method of the second upconversion nanoparticles (40% Tm@25% Yb@Y) is as follows:
[0082] Step 1: Take 0.153g of thulium chloride hexahydrate powder and 0.182g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0083] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0084] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:40%Tm precipitate.
[0085] Step 4: Core-shell structured upconversion nanoparticles were prepared using a homogeneous encapsulation method. Specifically, 0.097 g of ytterbium chloride hexahydrate powder and 0.228 g of yttrium chloride hexahydrate powder were placed in a three-necked flask, along with the NaYF4:40%Tm precipitate obtained in Step 3. Then, 6 mL of oleic acid and 15 mL of octadecene solution were added. The mixture was fixed in an oil bath and stirred at 700 rpm at 160°C under nitrogen protection until the reagents in the three-necked flask were completely dissolved. The mixture was then cooled to 30°C. Steps 2-3 were repeated to obtain the NaYF4:40%Tm@NaYF4:25%Yb precipitate.
[0086] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 40% Tm@25% Yb@Y second upconversion nanoparticles with a core-shell-shell structure.
[0087] Specifically, the synthesis method of the third upconversion nanoparticles (40% Yb@25% Er@Y) is as follows:
[0088] Step 1: Take 0.155g of ytterbium chloride hexahydrate powder and 0.182g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0089] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0090] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:40%Yb precipitate.
[0091] Step 4: Core-shell structured upconversion nanoparticles were prepared using a homogeneous encapsulation method. Specifically, 0.095 g of erbium chloride hexahydrate powder and 0.243 g of yttrium chloride hexahydrate powder were placed in a three-necked flask, along with the NaYF4:40%Yb precipitate obtained in Step 3. Then, 6 mL of oleic acid and 15 mL of octadecene solution were added. The mixture was fixed in an oil bath and stirred at 700 rpm under nitrogen protection at 160°C until the reagents in the three-necked flask were completely dissolved. The mixture was then cooled to 30°C. Steps 2-3 were repeated to obtain the NaYF4:40%Yb@NaYF4:25%Er precipitate.
[0092] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 40% Yb@25% Er@Y third upconversion nanoparticles with a core-shell-shell structure.
[0093] Specifically, the synthesis method of the fourth upconversion nanoparticles (50% Ho@25% Yb@Y) is as follows:
[0094] Step 1: Take 0.190g of holmium chloride hexahydrate powder and 0.152g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0095] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0096] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:50%Ho precipitate.
[0097] Step 4: Prepare core-shell structured upconversion nanoparticles using a homogeneous encapsulation method. Specifically, take 0.097 g of ytterbium chloride hexahydrate powder and 0.228 g of yttrium chloride hexahydrate powder in a three-necked flask, add the NaYF4:50%Ho precipitate obtained in Step 3, then add 6 mL of oleic acid and 15 mL of octadecene solution. Fix the flask in an oil bath and stir at 700 rpm under nitrogen protection at 160 °C until the reagents in the three-necked flask are completely dissolved. Then cool to 30 °C. Repeat steps 2-3 to obtain NaYF4:50%Ho@NaYF4:25%Yb precipitate.
[0098] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 50% Ho@25% Yb@Y fourth upconversion nanoparticles with a core-shell-shell structure.
[0099] S2. Dissolve the precipitates of each of the synthesized upconversion nanoparticles in cyclohexane to obtain a cyclohexane solution of upconversion nanoparticles with a molar concentration of 0.8 mol / L.
[0100] S3. Using a spin coater, the cyclohexane solution of the upconversion nanoparticles was spin-coated onto a commercial Si-based detector to obtain a Si-based detector / upconversion nanoparticle composite structure, which is a multi-band SWIR photodetector. The spin coater parameters were set as follows: low speed 200 rpm, held for 2 seconds; high speed 2000 rpm, held for 40 seconds. This multi-band SWIR photodetector exhibits significant photocurrent responses to light at 1150 nm, 1208 nm, 1500 nm, and 2300 nm.
[0101] S4. Combine the above-mentioned multi-band SWIR photodetector with a commercial NIR narrowband (700-1000nm) industrial camera to form a multi-band SWIR visualization imaging system, which can be used to detect light at 1150nm, 1208nm, 1500nm and 2300nm in dark conditions.
[0102] Example 3
[0103] This embodiment provides a method for fabricating the above-mentioned multi-band SWIR photodetector and imaging system, which includes the following steps:
[0104] S1. First upconversion nanoparticles (80% Ho@55% Yb@Y), second upconversion nanoparticles (80% Tm@55% Yb@Y), third upconversion nanoparticles (80% Yb@55% Er@Y), and fourth upconversion nanoparticles (70% Ho@55% Yb@Y) were synthesized by the classic solvothermal method. They can be excited by light at 1150 nm, 1208 nm, 1500 nm, and 2300 nm, respectively, to generate VIS-NIR light, which can then be effectively captured by a Si-based detector to achieve narrowband detection.
[0105] Specifically, the synthesis method of the first upconversion nanoparticles (80% Ho@55% Yb@Y) is as follows:
[0106] Step 1: Take 0.304g of holmium chloride hexahydrate powder and 0.061g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0107] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0108] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:80%Ho precipitate.
[0109] Step 4: Prepare core-shell structured upconversion nanoparticles using a homogeneous encapsulation method. Specifically, take 0.213 g of ytterbium chloride hexahydrate powder and 0.137 g of yttrium chloride hexahydrate powder in a three-necked flask, add the NaYF4:80%Ho precipitate obtained in Step 3, then add 6 mL of oleic acid and 15 mL of octadecene solution. Fix the flask in an oil bath and stir at 700 rpm under nitrogen protection at 160°C until the reagents in the three-necked flask are completely dissolved. Then cool to 30°C. Repeat steps 2-3 to obtain NaYF4:80%Ho@NaYF4:55%Yb precipitate.
[0110] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 80% Ho@55% Yb@Y first upconversion nanoparticles with a core-shell-shell structure.
[0111] Specifically, the synthesis method of the second upconversion nanoparticles (80% Tm@55% Yb@Y) is as follows:
[0112] Step 1: Take 0.307g of thulium chloride hexahydrate powder and 0.061g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0113] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0114] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:80%Tm precipitate.
[0115] Step 4: Core-shell structured upconversion nanoparticles were prepared using a homogeneous encapsulation method. Specifically, 0.213 g of yttrium chloride hexahydrate powder and 0.137 g of yttrium chloride hexahydrate powder were placed in a three-necked flask, along with the NaYF4:80%Tm precipitate obtained in Step 3. Then, 6 mL of oleic acid and 15 mL of octadecene solution were added. The mixture was fixed in an oil bath and stirred at 700 rpm at 160°C under nitrogen protection until the reagents in the three-necked flask were completely dissolved. The mixture was then cooled to 30°C. Steps 2-3 were repeated to obtain the NaYF4:80%Tm@NaYF4:55%Yb precipitate.
[0116] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 80% Tm@55% Yb@Y second upconversion nanoparticles with a core-shell-shell structure.
[0117] Specifically, the synthesis method of the third upconversion nanoparticles (80% Yb@55% Er@Y) is as follows:
[0118] Step 1: Take 0.310g of ytterbium chloride hexahydrate powder and 0.061g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0119] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0120] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:80%Yb precipitate.
[0121] Step 4: Prepare core-shell structured upconversion nanoparticles using a homogeneous encapsulation method. Specifically, take 0.210 g of erbium chloride hexahydrate powder and 0.137 g of yttrium chloride hexahydrate powder in a three-necked flask, and simultaneously add the NaYF4:80%Yb precipitate obtained in Step 3. Then add 6 mL of oleic acid and 15 mL of octadecene solution, fix the flask in an oil bath, and stir at 700 rpm under nitrogen protection at 160 °C until the reagents in the three-necked flask are completely dissolved. Then cool to 30 °C. Repeat steps 2-3 to obtain NaYF4:80%Yb@NaYF4:55%Er precipitate.
[0122] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 80% Yb@55% Er@Y third upconversion nanoparticles with a core-shell-shell structure.
[0123] Specifically, the synthesis method of the fourth upconversion nanoparticles (70% Ho@55% Yb@Y) is as follows:
[0124] Step 1: Take 0.266g of holmium chloride hexahydrate powder and 0.091g of yttrium chloride hexahydrate powder into a three-necked flask, add 6mL of oleic acid and 15mL of octadecene solution, fix it in an oil bath, and stir at 700rpm under nitrogen protection at 160℃ until the drugs in the three-necked flask are completely dissolved. Then cool to 30℃ to obtain mixed solution A.
[0125] Step 2: Dissolve 0.1g sodium hydroxide and 0.148g ammonium fluoride powder in 6mL methanol solution. Slowly add the methanol solution to the mixed solution A obtained in Step 1 above. After stirring thoroughly for 1 hour, raise the temperature from room temperature to 125℃. During the heating process, bubbles continuously emerge in the three-necked flask. After the bubbles disappear from the three-necked flask, connect the condenser and slowly raise the temperature of the solution in the three-necked flask to 300℃. Stir thoroughly for 2 hours, then stop heating and lower the temperature to 30℃ to obtain mixed solution B.
[0126] Step 3: Dispense the mixed solution B obtained in Step 2 into centrifuge tubes, add 15 mL of ethanol solution to the centrifuge tubes, centrifuge at 10000 rpm for 20 min, pour off the supernatant, add 16 mL of cyclohexane solution, sonicate and dissolve the precipitate, then add 20 mL of ethanol solution and centrifuge again. Repeat this step twice to obtain NaYF4:70%Ho precipitate.
[0127] Step 4: Prepare core-shell structured upconversion nanoparticles using a homogeneous encapsulation method. Specifically, take 0.213 g of ytterbium chloride hexahydrate powder and 0.137 g of yttrium chloride hexahydrate powder in a three-necked flask, add the NaYF4:70%Ho precipitate obtained in Step 3, then add 6 mL of oleic acid and 15 mL of octadecene solution. Fix the flask in an oil bath and stir at 700 rpm under nitrogen protection at 160°C until the reagents in the three-necked flask are completely dissolved. Then cool to 30°C. Repeat steps 2-3 to obtain NaYF4:70%Ho@NaYF4:55%Yb precipitate.
[0128] Step 5: Take 0.26g of yttrium chloride hexahydrate powder into a three-necked flask, and repeat steps 2-4 to obtain a precipitate of 70% Ho@55% Yb@Y fourth upconversion nanoparticles with a core-shell-shell structure.
[0129] S2. Dissolve the precipitates of each of the synthesized upconversion nanoparticles in cyclohexane to obtain a cyclohexane solution of upconversion nanoparticles with a molar concentration of 0.02 mol / L.
[0130] S3. Using a spin coater, the cyclohexane solution of the above-mentioned upconversion nanoparticles was spin-coated onto a commercial Si-based detector to obtain a Si-based detector / upconversion nanoparticle composite structure, which is a multi-band SWIR photodetector. The spin coater parameters were set as follows: low speed 500 rpm, held for 5 s; high speed 8000 rpm, held for 100 s. This multi-band SWIR photodetector exhibits significant photocurrent responses to light at 1150 nm, 1208 nm, 1500 nm, and 2300 nm.
[0131] S4. Combine the above-mentioned multi-band SWIR photodetector with a commercial NIR narrowband (700-1000nm) industrial camera to form a multi-band SWIR visualization imaging system, which can be used to detect light at 1150nm, 1208nm, 1500nm and 2300nm in dark conditions.
[0132] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification.
Claims
1. A multi-band SWIR photodetector, comprising a detector, characterized in that, The detector is equipped with a first upconversion nanoparticle, a second upconversion nanoparticle, a third upconversion nanoparticle, and a fourth upconversion nanoparticle, which can be excited by light of 1150nm, 1208nm, 1500nm and 2300nm to generate VIS-NIR light respectively. Wherein, the first upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Ho and Yb; the second upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Tm and Yb; the third upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Er and Yb; and the fourth upconversion nanoparticle is a NaYF4 upconversion nanomaterial with a core-shell-shell structure doped with Ho and Yb. The first upconversion nanoparticles include NaYF4 doped with Ho, NaYF4 doped with Yb, and NaYF4; wherein the doping amount of Ho is 5%-80% by mole fraction, and the doping amount of Yb is 5%-80% by mole fraction. The second upconversion nanoparticles include NaYF4 doped with Tm, NaYF4 doped with Yb, and NaYF4; wherein the doping amount of Tm is 5%-80% by mole fraction, and the doping amount of Yb is 5%-80% by mole fraction. The third upconversion nanoparticles include Er-doped NaYF4, Yb-doped NaYF4, and NaYF4; wherein the Er doping amount is 5%-80% by mole fraction, and the Yb doping amount is 5%-80% by mole fraction. The fourth upconversion nanoparticles include NaYF4 doped with Ho, NaYF4 doped with Yb, and NaYF4; wherein the doping amount of Ho is 5%-80% in mole fraction and the doping amount of Yb is 5%-80% in mole fraction.
2. The multi-band SWIR photodetector device according to claim 1, characterized in that, The detector is a Si-based detector.
3. A method for fabricating a multi-band SWIR photodetector as described in any one of claims 1-2, characterized in that, Includes the following steps: The first, second, third, and fourth upconversion nanoparticles were synthesized by a solvothermal method. The first, second, third, and fourth upconversion nanoparticles were dissolved in cyclohexane and then spin-coated onto the detector to obtain the multi-band SWIR photodetector.
4. A multi-band SWIR photodetector device prepared by the preparation method described in claim 3.
5. An imaging system comprising an industrial camera, characterized in that, It also includes the multi-band SWIR photodetector device according to any one of claims 1-2 and 4.
Citation Information
Patent Citations
Nanocomposite particle and uses thereof
US20220257524A1
Multi-color up-conversion nanoprobe, preparation method therefor, and application thereof
WO2021031321A1