A high-resistance and high-magnetic property hexagonal ferrite material and preparation method

By introducing dopants such as PTCC and Co2O3 into hexagonal ferrite, and performing positive pressure sintering in an oxygen atmosphere, the problem of low resistivity in the existing technology is solved, and hexagonal iron with high resistivity and high magnetic properties is achieved. Oxygen material significantly improves the stability and service life of the material.

CN116969751BActive Publication Date: 2024-10-29UNIV OF ELECTRONICS SCI & TECH OF CHINA +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311070026.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-24
Publication Date
2024-10-29
Estimated Expiration
2043-08-24

AI Technical Summary

Technical Problem

The existing technology cannot increase the resistivity while maintaining the high magnetic properties of hexagonal ferrite, which causes the micro motor to easily generate eddy currents in the alternating electric field, causing the magnet to heat up and shorten its service life.

Method used

Using dopants such as PTCC, CaCO3, SiO2, H3BO3 and Co2O3, the grain boundary/grain characteristics and microstructure of the hexagonal ferrite are controlled through ball milling, pre-sintering, sintering and other processes to increase the resistivity and improve the resistivity temperature characteristics. , while performing positive pressure sintering in an oxygen atmosphere to improve magnetic moment orientation and magnetic properties.

Benefits of technology

It achieves the high resistivity (≥220Ω·m) and high magnetic properties of hexagonal ferrite (residual magnetic induction intensity Br≥4.3kG, magnetic coercive force Hcb≥4.1kOe, intrinsic coercive force Hcj≥4.8kOe), Significantly improves the stability and service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116969751B_ABST
    Figure CN116969751B_ABST
Patent Text Reader

Abstract

The invention discloses a high-resistance and high-magnetic property hexagonal ferrite material and a preparation method, which belongs to the technical field of ferrite material preparation. It solves the following key technical problems in the fields of permanent magnet motor development and so on: first, the resistivity of hexagonal ferrite is greatly improved, and the resistance-temperature characteristics are improved; second, the intrinsic coercive force and magnetic induction coercive force are greatly increased, so that the stability of the micro motor during operation is enhanced. In the present invention, while the resistivity of the material is greatly improved, the coercive force is also improved by about 7%; in the report of J.European Ceram Soc.2023,43:5521‑5529, the resistivity of the material is increased by 47.5% compared with that before doping, and the resistivity of the material in the present invention is increased by 325% compared with that before doping, showing significant advantages in magnetic properties and electrical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present technology belongs to the technical field of ferrite material preparation, and particularly relates to hexagonal ferrite material and a preparation method thereof. Background Art

[0002] With the rapid development of emerging industries such as new energy vehicles, high-end equipment, and smart homes, the market demand for micro motors is also increasing, which has promoted the rapid development of hexagonal ferrite materials. Hexagonal ferrite materials are an important type of basic functional materials. With their advantages such as wide raw material sources, low prices, and excellent magnetic properties, they occupy an important position in the development of magnetic materials. However, with the expansion of application fields and the high-endization of products, in order to break through the bottleneck of existing products, the market has higher and higher performance requirements for hexagonal ferrites. In addition to magnetic properties, electrical properties are also beginning to be gradually concerned by people. Due to the low resistivity of hexagonal ferrites, eddy currents are easily generated in alternating electric fields, causing the magnets to heat up. Excessive temperature will reduce the magnetic properties of hexagonal ferrites, and even demagnetize, which will seriously shorten the service life of micro motors and even cause safety problems. Therefore, if the resistivity of hexagonal ferrites can be improved, it can not only greatly improve the service life of micro motors, but also help improve the performance of hexagonal ferrites, break through the existing bottlenecks of products, and realize the high-end application of hexagonal ferrites, which is of great significance to the development of micro motors.

[0003] The Chinese patent publication number CN115784733A discloses a high-performance calcium lanthanum cobalt ferrite material and its preparation method, which has the following atomic formula: Ca 1-x-y Sr y La x Fe 2n-z Co z , 0.4≤x≤0.6, 0.05≤y≤0.3, 0.25≤z≤0.5, 4.7≤n≤5.3. Magnetic performance indicators are: residual magnetic induction intensity B r =4400Gs, magnetic coercivity H cb =4046Oe, intrinsic coercivity H cj=4812Oe. The patent publication number CN111439995B discloses a high-performance Co-free hexagonal permanent ferrite material and its preparation method, and its main components include: 1.38-4.46mol% CaCO3, 2.15-6.15mol% La2O3, 1.38-5.38mol% SrCO3, 73.5-82.2mol% Fe2O3, 1.15-5.77mol% Al2O3, 1.92-6.54mol% ZnO, 1.69-7.31mol% CuO. The additives include: 0.01-0.08wt% La2O3, 0.03-0.09wt% Al2O3, 0.08-0.18wt% H3BO3, 0.08-0.38wt% CaCO3, 0.18-0.38wt% SiO2, 0.12-0.72wt% Ca(C6H 11 O7)2, 0.12~0.72wt%HO(CH2CH2O) n H. Magnetic performance indicators are: residual magnetic induction intensity B r ≥460mT; Intrinsic coercivity H cj ≥370kA / m; Magnetic coercivity H cb ≥330kA / m; Maximum magnetic energy product (BH) max ≥41kJ / m 3 The patent publication number is CN113087513A, which discloses a high coercive force ferrite and its preparation method. The composition is A 1-x-y Ca x La y (Fe 12-u-v Co u ) 19 , where A represents at least one of Sr and Ba, x, y, u, and v are molar ratios, 0.01≤x≤0.3, 0.1≤y≤0.5, 0.1≤u≤0.3, 0.1≤v≤0.5. The magnetic property indicators are: intrinsic coercivity H cj ≥430kA / m, residual magnetism B r ≥460mT, maximum magnetic energy product (BH) max ≥41kJ / m 3 , magnetic coercivity H cb Although the above materials have excellent magnetic properties, their resistivity values ​​have not been published.

[0004] Regarding the research on the resistivity of hexagonal ferrite, the University of Electronic Science and Technology of my country has announced a method to improve the resistivity of hexagonal ferrite (Zhong L, Lan ZW, et al. Synergetic effect of site-controlled two-step Ca doping on magnetic and electrical properties of M-type strontiumhexaferrites. J. European Ceram Soc. 2023, 43: 5521-5529). It uses regional regulation of two-step doping to increase the resistivity of the prepared hexagonal ferrite from 50Ω·m to 110Ω·m, but its magnetic coercivity H cb and intrinsic coercivity H cj They decreased from 3.5kOe and 4.5kOe to 2.8kOe and 3.1kOe respectively. The School of Physics and Materials Science of Sholini University in India announced a method to increase the resistivity of hexagonal ferrite (R. Jasrotia, VP Singh, B. Sharma, et al. Sol-gel synthesized Ba-Nd-Cd-In nanohexaferrites for high frequency and microwave devices applications, J. Alloy. Compd. 830 (2020) 1-6). The resistivity of the prepared hexagonal ferrite was increased from 360Ω·m to 531Ω·m by co-doping with Nd-Cd-In, which is 47.5% higher than that of undoped nanoferrite. However, the magnetic properties were not disclosed.

[0005] Based on the above, in the existing patents and research, it is still impossible to improve the resistivity while maintaining the high magnetic properties of hexagonal ferrite. Therefore, the present invention provides a high-resistance and high-magnetic property hexagonal ferrite material and a preparation method, which improves the resistivity temperature characteristics on the basis of ensuring high magnetic properties, and effectively reduces the damage caused by eddy currents during the use of hexagonal ferrite. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a high-resistance and high-magnetic property hexagonal ferrite material and a preparation method thereof.

[0007] The technical problem to be solved by the present invention is to provide a method for preparing a high resistivity hexagonal ferrite material. The material has a high residual magnetic induction intensity B r ≥4.3kG, high magnetic coercivity H cb ≥4.1kOe, high intrinsic coercivity Hcj ≥4.8kOe, maximum magnetic energy product (BH) max ≥4.5MG·Oe; high resistivity ρ≥220Ω·m.

[0008] The technical solution adopted by the present invention to solve the technical problem is a high-resistance and high-magnetic property hexagonal ferrite material, the components of which include: 4.6-11.4wt% SrCO3, 82.8-90.1wt% Fe2O3, 0.5-0.8wt% CaCO3, 0.3-0.5wt% La2O3, and 1.4-2.3wt% Co2O3.

[0009] The doping agent is calculated as oxides according to the weight percentage of the main formula: 0.5-1.5wt% CaCO3, 0.2-0.4wt% SiO2, 0.1-0.5wt% H3BO3, 0.8-2.0wt% Co2O3, 0.1-0.6wt% PTCC;

[0010] A method for preparing a high-resistance and high-magnetic property hexagonal ferrite material, wherein the main formula of the hexagonal ferrite material is 4.6-11.4wt% SrCO3, 82.8-90.1wt% Fe2O3, 0.5-0.8wt% CaCO3, 0.3-0.5wt% La2O3, and 1.4-2.3wt% Co2O3;

[0011] Step 1: ball milling once;

[0012] Mix the main formula powder evenly in a planetary ball mill for 12 to 21 hours;

[0013] Step 2: Pre-burning;

[0014] The ball mill obtained in step 1 is dried, sintered in air, heated to 1150-1350° C., kept warm for 1-3 hours, and then cooled naturally;

[0015] Step 3: doping;

[0016] Add the following dopants according to weight ratio to the powder obtained in step 2: 0.5-1.5wt% CaCO3, 0.2-0.4wt% SiO2, 0.1-0.5wt% H3BO3, 0.8-2.0wt% Co2O3, 0.2-0.4wt% PTCC;

[0017] Step 4: secondary ball milling;

[0018] The powder obtained in step 3 is ball-milled in a drum ball mill, and the final powder particle size is between 0.5 and 0.8 μm;

[0019] Step 5: Dehydration;

[0020] The ball-milled slurry obtained in step 4 is dehydrated through gauze, and the water content of the slurry is controlled between 17% and 33%;

[0021] Step 6: Molding;

[0022] The dehydrated slurry obtained in step 5 is pressed and molded in a magnetic field molding machine, the molding magnetic field strength is 0.8-1.6T, and the molding pressure is 80-120MPa;

[0023] Step 7: Sintering;

[0024] Place the blank obtained in step 6 in a sintering furnace in an oxygen atmosphere and sinter it at 800-950°C for 0.25-0.5 hours, raise the temperature to 1100-1250°C in 0.5 hours, maintain the oxygen pressure in the furnace at 0.11-0.16 MPa, and keep it for 1-3 hours.

[0025] Step 8: Test;

[0026] The sample obtained in step 7 is subjected to magnetic property test.

[0027] The residual magnetic induction intensity B of the material was tested using the AMT-4A permanent magnetic property automatic measuring instrument. r , magnetic coercivity H cb , intrinsic coercivity H cj 、Maximum magnetic energy product (BH) max ; Use TongHui2826 LCR digital bridge to test the room temperature resistivity ρ of the material, and use an oven to measure the change of resistivity with temperature.

[0028] The final technical indicators of the hexagonal ferrite material prepared by the present invention are as follows:

[0029] Residual magnetic induction intensity B r : ≥4.3kGs;

[0030] Magnetic coercivity H cb :≥4.1kOe;

[0031] Intrinsic coercivity H cj :≥4.8kOe;

[0032] Maximum magnetic energy product (BH) max :≥4.5MG·Oe;

[0033] Resistivity ρ: ≥220Ω·m (25~60℃).

[0034] The core idea of ​​the present invention is that due to the presence of defects such as interstitial atoms and dislocations, the grain boundaries of hexagonal ferrites usually show higher resistance than grains. Therefore, the improvement of the resistivity of hexagonal ferrites requires the control of the grain boundary / grain characteristics of the material, while the microstructure of the hexagonal ferrite needs to be regulated to maintain the magnetic properties. First, PTCC has high resistivity and high melting point. It is enriched at the grain boundaries during the sintering process, which can significantly increase the grain boundary resistance, thereby increasing the resistivity of hexagonal ferrites. At the same time, the positive temperature coefficient effect of PTCC can improve the resistivity-temperature characteristics of hexagonal ferrites to a certain extent. In addition, the coercive force is affected by the irreversible magnetization process, including irreversible magnetic domain rotation and irreversible domain wall displacement. Factors such as the anisotropy, porosity, stress and impurities of the material will lead to an increase in the resistance to the irreversible magnetization process. During the sintering process, PTCC will undergo ion diffusion and form a concentration gradient at the grain boundaries, resulting in a strong pinning effect, which hinders the domain wall displacement during the re-magnetization process, thereby greatly improving the coercive force. Secondly, since the pre-sintering temperature is high and the melting point of Co2O3 is low, about 890°C, Co2O3 will partially volatilize during the pre-sintering process, resulting in lattice defects. The introduction of Co2O3 during the second grinding process can, on the one hand, repair the lattice defects caused by the volatilization of Co during the pre-sintering process and increase the saturation magnetic induction intensity. On the other hand, it forms a crystal promoting / crystal inhibiting composite additive with CaCO3, SiO2, H3BO3 and the aforementioned high-melting-point PTCC to regulate the grain / grain boundary characteristics of the ferrite and achieve the single-domain densification growth of hexagonal ferrite. Third, an oxygen atmosphere is used for positive pressure sintering during the sintering process. Maintaining a high pressure in the furnace through oxygen can promote the consistent arrangement of magnetic moments and improve the orientation of hexagonal ferrite. At the same time, the oxygen atmosphere can reduce Fe 2+ The generation of impurity ions can be inhibited from entering the crystal lattice, thereby increasing the saturation magnetic induction intensity and thus increasing the residual magnetic induction intensity and coercive force of the material.

[0035] The present invention provides a high-resistance and high-magnetic property hexagonal ferrite material and a preparation method, which solves the following key technical problems in the field of permanent magnet motor development: first, the resistivity of the hexagonal ferrite is greatly improved, and the resistance-temperature characteristic is improved; second, the intrinsic coercive force and the magnetic induction coercive force are greatly increased, so that the stability of the micro motor during operation is enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Shown is the change in resistivity of the PTCC used in the present invention with temperature.

[0037] Figure 2 The figure shows the change of resistivity of the hexagonal ferrite material of Example 1 with temperature.

[0038] Figure 3 Shown is the change in resistivity of the hexagonal ferrite material of Example 2 with temperature.

[0039] Figure 4 Shown is a scanning electron microscope photograph of the hexagonal ferrite material of Example 1.

[0040] Figure 5 Shown is a scanning electron microscope photograph of the hexagonal ferrite material of Example 2. DETAILED DESCRIPTION

[0041] In view of the current blank in improving the resistivity of hexagonal ferrite at home and abroad, the present invention provides a high-resistance and high-magnetic property hexagonal ferrite material and preparation method, and its guiding ideology is: ion occupation mechanism, grain boundary theory, steric hindrance mechanism, magnetic moment orientation theory. First, by adopting PTCC doping, the resistivity of hexagonal ferrite can be greatly improved by regulating the grain boundary resistance; the Co2O3 additive is introduced in the secondary ball milling process, on the one hand, to repair the lattice defects caused by the loss of Co during the pre-sintering process, on the other hand, it forms a crystal promoting / crystal blocking composite additive with H3BO3, CaCO3, SiO2 additives and the aforementioned high melting point PTCC to regulate the grain / grain boundary characteristics of the ferrite. Secondly, oxygen is introduced during the sintering process to maintain a high pressure in the sintering furnace, thereby forcing the magnetic moment to be uniformly oriented under pressure, improving the orientation degree of the hexagonal ferrite, and at the same time ensuring that the metal ions are oxidized to a suitable valence state.

[0042] The main component of the hexagonal ferrite material of the present invention is calculated as oxide by mole percentage, and the dopant component is calculated as oxide by weight percentage. The hexagonal ferrite material of the present invention and the preparation method thereof include the following steps:

[0043] 1. Formulation

[0044] Using 4.6-11.4wt% SrCO3, 82.8-90.1wt% Fe2O3, 0.5-0.8wt% CaCO3, 0.3-0.5wt% La2O3, 1.4-2.3wt% Co2O3;

[0045] 2. One-time ball milling

[0046] Mix the above powders evenly in a planetary ball mill for 12 to 21 hours;

[0047] 3. Pre-burning

[0048] The ball mill obtained in step 2 is dried, heated to 1150-1350° C. in air atmosphere, kept at this temperature for 1-3 hours, and then cooled naturally;

[0049] 4. Doping

[0050] Add the following dopants according to weight ratio to the powder obtained in step 3: 0.5-1.5wt% CaCO3, 0.2-0.4wt% SiO2, 0.1-0.5wt% H3BO3, 0.8-2.0wt% Co2O3, 0.2-0.4wt% PTCC;

[0051] 5. Secondary ball milling

[0052] The powder obtained in step 4 is ball-milled in a drum ball mill for 12 to 24 hours, and the particle size of the powder is controlled between 0.5 and 0.8 μm;

[0053] 6. Dehydration

[0054] The ball-milled slurry obtained in step 5 is dehydrated through gauze, and the water content of the slurry is controlled between 17% and 33%;

[0055] 7. Molding

[0056] The dehydrated slurry obtained in step 6 is pressed and molded in a magnetic field molding machine, the molding magnetic field strength is 0.8-1.6T, and the molding pressure is 80-120MPa;

[0057] 8. Sintering

[0058] The blank obtained in step 7 is placed in a sintering furnace in an oxygen atmosphere for sintering at 800-950° C. for 0.25-0.5 hours, and then the temperature is rapidly raised to 1100-1250° C., the oxygen pressure in the furnace is maintained at 0.11-0.16 MPa, and the temperature is maintained for 1-3 hours;

[0059] 9. Testing

[0060] The sample obtained in step 8 is subjected to magnetic property test.

[0061] The residual magnetic induction intensity B of the material was tested using the AMT-4A permanent magnetic property automatic measuring instrument. r , magnetic coercivity H cb , intrinsic coercivity H cj 、Maximum magnetic energy product (BH) max ; The resistivity ρ of the material was tested using the TongHui TH2826 LCR digital bridge, and the change of resistivity with temperature was measured in conjunction with a drying oven6+.

[0062] In order to verify the core idea of ​​the present invention, 4 groups of comparative examples are set, and the implementation schemes of comparative examples 1 to 4 are as follows:

[0063] Comparative Example PTCC <![CDATA[Co2O3 additive]]> Positive oxygen pressure 1 none none none 2 have have none 3 have none have 4 none have have

[0064] Specific examples 1-2, comparative examples 1-4:

[0065] Examples 1-2, Comparative Examples 1-4: A high resistivity hexagonal ferrite material and a preparation method thereof, comprising the following steps:

[0066] 1. Formulation

[0067] Using 10.2wt% SrCO3, 86.9wt% Fe2O3, 0.7wt% CaCO3, 0.5wt% La2O3, 1.7wt% Co2O3;

[0068] 2. One-time ball milling

[0069] Mix Examples 1, 2, and Comparative Examples 1 to 4 uniformly in a planetary ball mill for 12 to 21 hours;

[0070] 3. Pre-burning

[0071] The ball mill obtained in step 2 is dried, heated to 1150-1350° C. in air atmosphere, kept at this temperature for 1-3 hours, and then cooled naturally;

[0072] 4. Doping

[0073] The following dopants were added to the powders of Examples 1 and 2 obtained in step 3 according to weight ratio:

[0074]

[0075] The powders of Comparative Examples 1 to 4 obtained in step 3 are added with the following dopants by weight:

[0076]

[0077] 5. Secondary ball milling

[0078] The powder obtained in step 4 was ball-milled in a drum ball mill for 18 hours, and the powder particle size was controlled between 0.5 and 0.8 μm;

[0079] 6. Dehydration

[0080] The ball-milled slurry obtained in step 5 is dehydrated through gauze, and the water content of the slurry is controlled between 17% and 33%;

[0081] 7. Molding

[0082] The dehydrated slurry obtained in step 6 is pressed and molded in a magnetic field molding machine, the molding magnetic field strength is 1.2T, and the molding pressure is 100MPa;

[0083] 8. Sintering

[0084] The blanks of Examples 1 and 2 obtained in step 7 were placed in a sintering furnace for oxygen atmosphere sintering. The pressure in the furnace was controlled to be 0.12 MPa. The temperature was kept at 850° C. for 0.5 hour, and then the temperature was rapidly increased to 1140° C. and kept at this temperature for 3 hours.

[0085] The comparative examples 1 and 2 blanks obtained in step 7 were placed in a sintering furnace for air sintering, kept at 850° C. for 0.5 hour, and then rapidly heated to 1140° C. and kept at this temperature for 3 hours.

[0086] The comparative example 3 blank obtained in step 7 is placed in a sintering furnace for oxygen atmosphere sintering. The pressure in the furnace is controlled to be 0.12 MPa. The temperature is kept at 850° C. for 0.5 hour, and the temperature is quickly raised to 1140° C. and kept for 3 hours.

[0087] The comparative example 4 blank obtained in step 7 is placed in a sintering furnace for oxygen atmosphere sintering. The pressure in the furnace is controlled to be 0.14 MPa. The temperature is kept at 850° C. for 0.5 hour, and the temperature is quickly raised to 1140° C. and kept for 3 hours.

[0088] The hexagonal ferrite material was prepared by the above process. The performance parameters of Examples 1 and 2 are as follows:

[0089]

[0090] The performance parameters of Comparative Examples 1 to 4 are as follows:

[0091]

[0092] In the report of Journal of the European Ceramic Society.2023,43:5521-5529, the resistivity of the material was improved but the coercive force decreased significantly, while in the present invention, the coercive force was also improved by about 7% while the resistivity of the material was greatly improved; in the report of J.European Ceram Soc.2023,43:5521-5529, the resistivity of the material was increased by 47.5% compared with before doping, while the resistivity of the material in the present invention was increased by 325% compared with before doping, showing significant advantages in magnetic properties and electrical properties.

Claims

1. A high-resistance and high-magnetic property hexagonal ferrite material, the main formula of the hexagonal ferrite material is: 10.2wt% SrCO3, 86.9wt% Fe2O3, 0.7wt% CaCO3, 0.5wt% La2O3, 1.7wt% Co2O3; The doping agent is calculated as oxides according to the weight percentage of the main formula: 0.5-1.5wt% CaCO3, 0.2-0.4wt% SiO2, 0.1-0.5wt% H3BO3, 0.8-2.0wt% Co2O3, 0.1-0.6wt% PTCC; The method for preparing the high-resistance and high-magnetic-property hexagonal ferrite material comprises the following steps: Step 1: ball milling once; Mix the main formula powder evenly in a planetary ball mill for 12 to 21 hours; Step 2: Pre-burning; The ball mill obtained in step 1 is dried, sintered in air, heated to 1150-1350° C., kept warm for 1-3 hours, and then cooled naturally; Step 3: doping; Add the following dopants according to weight ratio to the powder obtained in step 2: 0.5-1.5wt% CaCO3, 0.2-0.4wt% SiO2, 0.1-0.5wt% H3BO3, 0.8-2.0wt% Co2O3, 0.2-0.4wt% PTCC; Step 4: secondary ball milling; The powder obtained in step 3 is ball-milled in a drum ball mill, and the final powder particle size is between 0.5 and 0.8 μm; Step 5: Dehydration; The ball-milled slurry obtained in step 4 is dehydrated through gauze, and the water content of the slurry is controlled between 17% and 33%; Step 6: Molding; The dehydrated slurry obtained in step 5 is pressed and molded in a magnetic field molding machine, the molding magnetic field strength is 0.8-1.6T, and the molding pressure is 80-120MPa; Step 7: Sintering; Place the blank obtained in step 6 in a sintering furnace in an oxygen atmosphere and sinter it at 800-950°C for 0.25-0.5 hours, raise the temperature to 1100-1250°C in 0.5 hours, maintain the oxygen pressure in the furnace at 0.11-0.16 MPa, and keep it for 1-3 hours.

Citation Information

Patent Citations

  • A high-performance Co-free hexagonal permanent magnet ferrite material and its preparation method

    CN111439995B

  • High-coercivity ferrite and preparation method thereof

    CN113087513A

  • High-performance calcium lanthanum cobalt ferrite material and preparation method thereof

    CN115784733A

  • SrM microwave ferrite material with high remanence ratio and high anisotropic field, and preparation method thereof

    CN113860864A

  • Two-phase composite ferrite material for X-band self-biased device and preparation method of two-phase composite ferrite material

    CN115579203A