A method for removing impurities and modifying lithium mica slag
By using ultrasonic treatment and calcium salt reaction to remove soluble fluoride salts in lepidolite slag, the problem of prolonged cement setting time caused by high content of fluorine salts in lepidolite slag was solved, impurity removal modification of lepidolite slag was achieved, and the cost of cement production was reduced. cost, and increase the dosage of lepidolite slag in cement.
Patent Information
- Application Number
- CN202310978050.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-04
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-08-04
AI Technical Summary
The high content of soluble fluoride salts in lepidolite slag results in a longer cement setting time, which limits the absorption capacity of lepidolite slag in the cement industry. The existing defluoridation method consumes high energy and has a low defluoridation rate.
Adopt pretreatment and impurity removal modification steps, including rough crushing treatment, adding water and impurity remover, high-frequency and low-frequency ultrasonic treatment, to promote the reaction of soluble calcium salt and soluble fluoride salt to form calcium fluoride precipitation, remove soluble fluorine, and pass Solid-liquid separation and drying obtain impurity-removed modified lepidolite slag.
It effectively reduces the soluble fluorine content in lepidolite slag to less than 10 ppm, improves the setting time of cement, and increases the amount of lepidolite slag in cement. The process is easy to operate, has low energy consumption, and has stable cement performance.
Smart Images

Figure BDA0004378107630000071 
Figure BDA0004378107630000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of industrial waste residue treatment, and in particular relates to a method for removing impurities and modifying lithium mica residue. Background Art
[0002] Lepidolite slag is the waste residue after lithium carbonate is extracted from lepidolite and auxiliary materials after high-temperature roasting. For every ton of lithium carbonate produced, about 20 tons of waste residue are generated. With the rapid development of the lithium carbonate industry, more than 20 million tons of lepidolite waste residue are produced in Yichun, Jiangxi alone every year. In order to digest the huge amount of lepidolite slag produced and solve the environmental pressure, most lithium carbonate plants cooperate with cement plants to use lepidolite slag as a mixed material admixture in the cement industry.
[0003] Large-scale production practice has proved that since lithium mica slag contains more soluble fluoride salts, when the lithium mica slag is used as a cement admixture exceeding 10%, the soluble fluorine will cause the cement setting time to be seriously prolonged. Therefore, the presence of higher soluble fluoride salts in lithium mica slag restricts the cement industry's ability to absorb lithium mica slag.
[0004] The source of fluorine in lithium mica slag is mainly the lithium mica ore itself. At present, lithium carbonate factories add lithium mica ore powder to the defluorination activator and mix it. The resulting mixture is roasted at high temperature to destroy the original stable structure of lithium mica and effectively remove fluorine. However, this method has high energy consumption, the roasting temperature reaches 950-1000℃, and the defluorination rate is not high. The fluorine content in the slag is still 2.8%-4.5%, of which the soluble fluorine content is 0.5%-0.9%. Therefore, it is necessary to develop a new method for removing impurities from lithium mica slag. Summary of the invention
[0005] The invention aims to provide a method for removing impurities and modifying lithium mica slag. The treatment process has low energy consumption, simple operation and convenient implementation. The soluble fluorine content in the treated lithium mica slag is lower than 10 ppm, and the slag can be used as a cement admixture. The produced cement has stable performance.
[0006] In order to solve the above technical problems of the present invention, the present invention provides the following technical solutions:
[0007] The object of the present invention is to provide a method for removing impurities and modifying lepidolite slag, comprising the steps of:
[0008] S1. Pretreatment: The lithium mica slag is roughly crushed to control the particle size of the material after the rough crushing to be ≤5cm;
[0009] S2, impurity removal and modification: add 3-4 times the volume of water to the coarsely broken lithium mica slag, stir and mix, then add impurity remover, and perform high-frequency ultrasonic treatment for 20-30 minutes to obtain a mixed slurry, put the mixed slurry into a grinder for 15-30 minutes, perform low-frequency ultrasonic treatment for 20-30 minutes, separate the solid and liquid, and dry the slag to obtain impurity-removed and modified lithium mica slag.
[0010] Furthermore, in S1, the coarse crushing machine is at least one of a jaw crusher, a cone crusher and a hammer crusher.
[0011] Furthermore, in S2, the impurity remover is at least one of calcium nitrate, calcium nitrite and calcium formate.
[0012] The soluble fluoride salt in the lithium mica slag exists in the form of sodium fluoride and potassium fluoride. The present invention utilizes the soluble calcium salt and the soluble fluoride salt to react chemically under solution conditions to generate calcium fluoride precipitation that does not affect the setting time of cement. Its ion equation is:
[0013] Ca 2+ +F-=CaF2↓
[0014] The soluble calcium salt selected by the present invention has a promoting effect on the hydration of cement and is an inorganic early strength agent for cement. Therefore, if there is unreacted calcium salt left in the slag, it will not have a negative effect on the cement. The inventor also found that when the soluble calcium salt and the soluble fluoride salt react chemically, the mechanical vibration and cavitation of the ultrasonic wave can accelerate the vibration and diffusion of the molecules, making the reaction more sufficient, wherein, after adding water and impurity remover to the coarsely broken lithium mica slag, high-frequency ultrasonic treatment is selected, mainly using high-energy vibration to destroy the structure of the lithium mica slag, accelerating the dissolution of the soluble fluoride salt, so that the impurity remover can fully react with the soluble fluoride salt, and then grinding the reacted slurry to further destroy the structure of the lithium mica slag, so that the soluble fluoride salt inside the lithium mica slag can be smoothly dissolved, and combined with low-frequency ultrasonic treatment, the soluble fluoride salt and the soluble calcium salt react fully.
[0015] Furthermore, in S2, the amount of the impurity remover calculated as calcium ions is 0.6-1.0 times the molar amount of soluble fluorine in the lithium mica slag.
[0016] Furthermore, in S2, the frequency of the high-frequency ultrasound is 60-80 kHz, and the frequency of the low-frequency ultrasound is 30-40 kHz.
[0017] Furthermore, in S2, the solid-liquid separation is at least one of centrifugation, sedimentation, and filtration.
[0018] The liquid obtained by solid-liquid separation can be recycled as mixing water for coarsely crushed lithium mica slag after potassium and sodium ions are extracted.
[0019] Furthermore, in S2, the drying is performed at 80-100°C for 0.5-1h.
[0020] Beneficial effects of the present invention:
[0021] 1. The present invention utilizes soluble calcium salt to react chemically with soluble fluoride salt in lithium mica slag under solution conditions to generate calcium fluoride precipitate which does not affect cement setting time, so as to remove soluble fluoride salt in lithium mica slag, and simultaneously removes soluble potassium and sodium ions harmful to cement performance contained in the lithium mica slag through solid-liquid separation, thereby achieving the purpose of modifying and removing impurities from the lithium mica slag. The inventor also found that when the soluble calcium salt and the soluble fluoride salt react chemically, the ultrasonic treatment of high frequency followed by low frequency is combined, and the mechanical vibration and cavitation of the ultrasonic wave can accelerate the vibration and diffusion of the molecules, so that the reaction is more complete. After water and impurity remover are added to the coarsely broken lithium mica slag, high-frequency ultrasonic treatment is selected, mainly using high-energy vibration to destroy the structure of the lithium mica slag, accelerate the dissolution of the soluble fluoride salt, so that the impurity remover can fully react with the soluble fluoride salt, and then the slurry of the reaction is ground to further destroy the structure of the lithium mica slag, so that the soluble fluoride salt inside the lithium mica slag can be smoothly dissolved, and combined with low-frequency ultrasonic treatment, the soluble fluoride salt and the soluble calcium salt react fully. The method of the present invention is simple to operate and easy to implement. The soluble fluorine content in the treated lithium mica slag is less than 10ppm, and the modified lithium mica slag has no effect on the setting time of cement, and the amount of cement in the cement can reach more than 30%.
[0022] 2. The modified impurity-free lithium mica slag is used as a cement admixture to produce cement. The cement produced has stable performance and reduces the production cost of cement. The solid waste lithium mica slag is utilized as a resource, with good economic benefits. According to the annual output of 2 million tons of cement mixed with 15% of modified impurity-free lithium mica slag, 300,000 tons of lithium mica slag can be consumed, which greatly saves the land resources occupied by stacking or landfilling lithium mica slag and is environmentally friendly. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0024] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0025] Embodiment 1:
[0026] S1. Pretreatment: The lithium mica slag is roughly crushed to control the particle size of the material after the rough crushing to be ≤5cm;
[0027] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.65%, and the soluble fluorine in the lithium mica slag was calculated to be 0.38 mol), and 37g of calcium nitrate was added after stirring and mixing, and a high-frequency ultrasonic treatment was performed at 70kHz for 25min to obtain a mixed slurry, and the mixed slurry was put into a mill for pulverization for 20min, and a low-frequency ultrasonic treatment was performed at 35kHz for 25min, and the solid-liquid separation was performed, wherein the slag was treated at 90°C for 45min and dried to obtain the lithium mica slag for impurity removal and modification.
[0028] Embodiment 2:
[0029] S1. Pretreatment: The lithium mica slag is roughly crushed to control the particle size of the material after the rough crushing to be ≤5cm;
[0030] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.85%, and the soluble fluorine in the lithium mica slag was calculated to be 0.5 mol), and 66g of calcium nitrate was added after stirring and mixing, and the mixture was subjected to high-frequency ultrasonic treatment at 60kHz for 30min to obtain a mixed slurry, which was put into a mill and ground for 20min, and subjected to low-frequency ultrasonic treatment at 30kHz for 30min, and solid-liquid separation was performed, wherein the slag was treated at 100°C for 0.5h and dried to obtain impurity-removing and modified lithium mica slag.
[0031] Embodiment 3:
[0032] S1. Pretreatment: The lithium mica slag is roughly crushed to control the particle size of the material after the rough crushing to be ≤5cm;
[0033] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.65%, and the soluble fluorine in the lithium mica slag was calculated to be 0.38 mol), and 34g of calcium nitrite was added after stirring and mixing, and the mixture was subjected to high-frequency ultrasonic treatment at 80kHz for 20min to obtain a mixed slurry, which was put into a mill and ground for 30min, and subjected to low-frequency ultrasonic treatment at 40kHz for 20min, and solid-liquid separation was performed, wherein the slag was treated at 80°C for 1h and dried to obtain the lithium mica slag subjected to impurity removal and modification.
[0034] Embodiment 4:
[0035] S1. Pretreatment: The lithium mica slag is roughly crushed to control the particle size of the material after the rough crushing to be ≤5cm;
[0036] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.85%, and the soluble fluorine in the lithium mica slag was calculated to be 0.5 mol), and 60g of calcium nitrate was added after stirring and mixing, and the mixture was subjected to high-frequency ultrasonic treatment at 70kHz for 25min to obtain a mixed slurry, which was put into a mill and ground for 20min, and subjected to low-frequency ultrasonic treatment at 35kHz for 25min, and solid-liquid separation was performed, wherein the slag was treated at 90°C for 0.5h and dried to obtain impurity-removing and modified lithium mica slag.
[0037] Embodiment 5:
[0038] S1. Pretreatment: coarsely crush the lithium mica slag to control the particle size of the coarsely crushed material to be ≤5cm;
[0039] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.65%, and the soluble fluorine in the lithium mica slag was calculated to be 0.38 mol), and 30g of calcium formate was added after stirring and mixing, and a high-frequency ultrasonic treatment was performed at 70kHz for 25min to obtain a mixed slurry, and the mixed slurry was put into a mill for pulverization for 20min, and a low-frequency ultrasonic treatment was performed at 35kHz for 25min, and the solid-liquid separation was performed, wherein the slag was treated at 90°C for 45min and dried to obtain the lithium mica slag for impurity removal and modification.
[0040] Embodiment 6:
[0041] S1. Pretreatment: coarsely crush the lithium mica slag to control the particle size of the coarsely crushed material to be ≤5cm;
[0042] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.85%, and the soluble fluorine in the lithium mica slag was calculated to be 0.5 mol), and 52g of calcium formate was added after stirring and mixing, and a high-frequency ultrasonic treatment was performed at 70kHz for 25min to obtain a mixed slurry, and the mixed slurry was put into a mill for pulverization for 20min, and a low-frequency ultrasonic treatment was performed at 35kHz for 25min, and the solid-liquid separation was performed, wherein the slag was treated at 90°C for 45min and dried to obtain the lithium mica slag for impurity removal and modification.
[0043] Comparative Example 1:
[0044] S1. Pretreatment: coarsely crush the lithium mica slag to control the particle size of the coarsely crushed material to be ≤5cm;
[0045] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.85%, and the soluble fluorine in the lithium mica slag was calculated to be 0.5 mol), and 60g of calcium nitrate was added after stirring and mixing to obtain a mixed slurry. The mixed slurry was put into a mill and ground for 20min, and the solid-liquid separation was performed. The slag was treated at 90°C for 0.5h and dried to obtain impurity-removed lithium mica slag.
[0046] Comparative Example 2:
[0047] S1. Pretreatment: coarsely crush the lithium mica slag to control the particle size of the coarsely crushed material to be ≤5cm;
[0048] S2, impurity removal and modification: 3L of water was added to 1000g of coarsely broken lithium mica slag (wherein the soluble fluorine content was 0.85%, and the soluble fluorine in the lithium mica slag was calculated to be 0.5 mol), and 60g of calcium nitrate was added after stirring and mixing, and low-frequency ultrasonic treatment was performed at 35kHz for 25min to obtain a mixed slurry, and the mixed slurry was put into a mill and ground for 20min, and high-frequency ultrasonic treatment was performed at 70kHz for 25min, and solid-liquid separation was performed, wherein the slag was treated at 90°C for 0.5h and dried to obtain impurity-removing and modified lithium mica slag.
[0049] The fluorine content of the lithium mica slag before and after impurity removal and modification of Examples 1-6 and Comparative Examples 1 and 2 was detected. The fluorine content detection method was referred to HJ 999-2018 "Determination of fluorine in solid waste by alkali fusion-ion selective electrode method", and the results are shown in Table 1.
[0050] Table 1
[0051] Soluble fluorine content before defluorination (%) Soluble fluorine content after defluorination (ppm) Example 1 0.65 9.9 Example 2 0.85 8.5 Example 3 0.65 9.0 Example 4 0.85 8.2 Example 5 0.65 9.8 Example 6 0.85 8.5 Comparative Example 1 0.85 12.8 Comparative Example 2 0.85 10.6
[0052] It can be seen from Table 1 that the use of an impurity remover combined with ultrasonic treatment in Examples 1-6 can effectively remove the soluble fluorine in the lepidolite slag. After the impurity removal, the soluble fluorine in the lepidolite slag is reduced to below 10 ppm.
[0053] Compared with Example 4, in Example 1, after no ultrasonic treatment was performed, the soluble fluorine content after fluorine removal was 12.8 ppm, which was much higher than 8.2 ppm in Example 4. In Example 2, after low-frequency and then high-frequency ultrasonic treatment was adopted, the soluble fluorine content after fluorine removal was 10.6 ppm, and the fluorine removal effect was worse than that in Example 4.
[0054] The impurity-removed and modified lepidolite slag obtained in Examples 1-6 was added to ordinary Portland cement in amounts of 15% and 30%, respectively. Ordinary Portland cement and unmodified lepidolite slag (soluble fluorine content of 0.65%) were used as control groups to observe the initial and final setting times of the cement. The results are shown in Table 2.
[0055] Table 2
[0056]
[0057]
[0058] It can be seen from Table 2 that before the lithium mica slag is modified by fluorine removal, when the content of the slag in cement is only 5%, the setting time of the cement is more than twice that of the control cement, which will seriously affect the construction progress of the cement. After the lithium mica slag is modified, when the content of the slag in cement reaches 30%, the setting time of the cement is basically the same as that of the control cement, and the maximum time difference is only about 10 minutes, which will not affect the construction progress of the cement at all.
[0059] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A method for removing impurities and modifying lepidolite slag, characterized in that: The steps include: S1. Pretreatment: coarsely crush the lithium mica slag to control the particle size of the coarsely crushed material to be ≤5cm; S2, impurity removal and modification: add 3-4 times the volume of water to the coarsely broken lithium mica slag, stir and mix, add impurity remover, and treat with high-frequency ultrasound for 20-30min to obtain a mixed slurry, put the mixed slurry into a mill for 15-30min, treat with low-frequency ultrasound for 20-30min, separate the solid and liquid, and dry the slag to obtain impurity-removed lithium mica slag; The impurity remover is at least one of calcium nitrate, calcium nitrite and calcium formate. The amount of the impurity remover is calculated based on calcium ions and is 0.6-1.0 times the molar amount of soluble fluorine in the lithium mica slag. The frequency of the high-frequency ultrasound is 60-80kHz, and the frequency of the low-frequency ultrasound is 30-40kHz.
2. The method for removing impurities and modifying lepidolite slag according to claim 1, wherein: In S1, the coarse crushing machine is at least one of a jaw crusher, a cone crusher and a hammer crusher.
3. The method for removing impurities and modifying lepidolite slag according to claim 1, wherein: In S2, the solid-liquid separation is at least one of centrifugation, sedimentation, and filtration.
4. The method for removing impurities and modifying lepidolite slag according to claim 1, wherein: In S2, the drying is carried out at 80-100°C for 0.5-1h.
Citation Information
Patent Citations
Modified mica and preparation method and application thereof
CN108329721A
Process method for preparing lithium carbonate by treating lepidolite by using sulfuric acid method
CN110526265A
Lithium salt-based composite mineral admixture and preparation method thereof
CN114988741A
Lithium MICA extraction
WO2023275346A2