Epoxy resin, curable resin composition, and cured product of curable resin composition
By preparing epoxy resin and hardened resin compositions with specific structures, the problem of taking into account the heat resistance and leakage marking characteristics is solved, and high heat resistance and leakage marking characteristics are achieved in high temperature environments. It is suitable for in complex electrical and electronic materials.
Patent Information
- Application Number
- CN202280022791.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-18
- Filing Date
- 2022-06-17
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-06-17
AI Technical Summary
When the conventional resin composition improves heat resistance, it is easy to cause a decrease in leakage marking characteristics, making it difficult to take into account both high heat resistance and high flame retardancy, especially in high temperature environments, the requirements of heat resistance and leakage marking characteristics are difficult to take into account.
By preparing an epoxy resin of a specific structure, the epoxy equivalent is divided by an epoxy resin having a value of 2.0 or more and less than 2.2, and the content of the inorganic filler in the hardening resin composition is 74% by weight or more and 95% by weight or less, a hardened product with excellent heat resistance and leakage trace resistance is formed by combining the reaction of an appropriate phenol resin with epihalohydrin.
It realizes the high heat resistance and leakage trace resistance of hardened substances under high temperature environments, and is suitable for electrical and electronic parts and composite materials, improving the reliability and performance of the material.
Smart Images

Figure CN117043215B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an epoxy resin having a specific structure, a curable resin composition, and a cured product of the curable resin composition. Background Art
[0002] Epoxy resins are widely used in electrical / electronic fields such as cast products, laminated boards, integrated circuit (IC) sealing materials, structural materials, adhesives, coatings, etc. due to their excellent electrical properties (dielectric constant / dielectric loss tangent, insulation), mechanical properties, adhesion, and thermal properties (heat resistance, etc.).
[0003] In recent years, in the electrical / electronic field, it is required that the flame retardancy, moisture resistance, adhesion, dielectric properties and other properties of the resin composition be improved, highly purified, low viscosity for highly filling fillers (inorganic fillers or organic fillers), reactivity for shortening the molding cycle and other properties be further improved (Patent Document 1). In addition, as a structural material, in aerospace materials, leisure / sports equipment applications, etc., a material with light weight and excellent mechanical properties is required.
[0004] In the field of semiconductor sealing and substrates (the substrate itself or its peripheral materials), as the semiconductors change, they become more complex due to thinning, stacking, systematization, and three-dimensionalization, requiring very high levels of heat resistance or high fluidity and other required characteristics. In particular, with the expansion of plastic packaging to automotive applications, the requirements for improved heat resistance have become more stringent. Specifically, as the driving temperature of semiconductors rises, very high heat resistance is required. In recent years, there has also been a trend towards high-bandgap semiconductors, and it is also necessary to cope with driving temperatures of 175°C or even above 200°C. For the driving temperature, the peripheral components are required to have sufficient heat resistance (glass transition temperature (Tg), especially Tg in thermomechanical properties (thermomechanical analysis (TMA))). Specifically, a temperature about 10% higher than the driving temperature is required (in the case of 200°C, a Tg of 220°C or above is required, for example, 225°C), and the requirements are increasing year by year (Non-patent document 1).
[0005] Moreover, in recent years, the demand for high-voltage power devices has increased dramatically in the demand for electric vehicles, etc., and the tracking resistance has been emphasized. In addition, the tracking resistance has also been emphasized in applications such as solar power generation, wind power generation, and electric vehicles (EVs), and in particular, in strict applications, the Comparative Tracking Index (CTI) is required to exceed 600.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2019-001841
[0009] Non-patent literature
[0010] Non-patent document 1: Fuji Electric Technical Report, Vol. 89, No. 4, 2016, pp. 247-250 (2016vol.89No.4247-250) Summary of the invention
[0011] Problems to be solved by the invention
[0012] Generally speaking, for the purpose of improving the heat resistance of resin composition, aromatic crosslinking units are sometimes introduced, but in the case described, since the main skeleton is aromatic, it is easy to carbonize, and the anti-tracking characteristic decreases. In addition, in the case of improving heat resistance by high molecular weight, since the molecular weight becomes large, the thermal decomposition temperature rises, and the anti-tracking characteristic decreases. That is, there is a trade-off relationship between heat resistance and tracking characteristic, so it is very difficult to remove the tracking characteristic while maintaining heat resistance. And then, in the case of a resin containing a polysaccharide compound in order to impart characteristics such as flame retardancy, the anti-tracking characteristic is easily deteriorated, and it is difficult to take into account high anti-tracking characteristic and flame retardancy.
[0013] Generally speaking, the material performance level category (PLC) is set according to the CTI value. By assigning the PLC to a smaller category, the design size (creeping distance) of the device can be reduced, so the PLC is preferably 3 or less, and particularly preferably 1 or less.
[0014] Furthermore, PLC and CTI have the following relationship.
[0015] PLC1: CTI above 600, PLC2: CTI above 400 and less than 600, PLC3: above 250 and less than 400, PLC4: above 100 and less than 175, PLC5: less than 100.
[0016] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an epoxy resin and a curable resin composition whose cured product has excellent heat resistance and anti-tracking properties.
[0017] Technical means of solving problems
[0018] The present inventors have made intensive research to solve the above problems and have completed the present invention. That is, the present invention relates to the following [1] to [3]. In the present application, "(numerical value 1) to (numerical value 2)" means including upper and lower limits. [1]
[0020] An epoxy resin represented by the following formula (1), wherein the value obtained by dividing the epoxy equivalent (g / eq.) by the softening point (° C.) is 2.0 or more and less than 2.2.
[0021] [Chemistry 1]
[0022]
[0023] (In formula (1), a plurality of Rs exist independently and represent a methyl group or a hydrogen atom, and n is an average value of the number of repetitions and is a real number of 1 to 10) [2]
[0025] A curable resin composition comprising the epoxy resin according to the above item [1]. [3]
[0027] The curable resin composition according to the above item [2], wherein the content of the inorganic filler is 74% by weight or more and 95% by weight or less based on the total amount of the curable resin composition. [4]
[0029] A cured product obtained by curing the curable resin composition according to the above item [2] or [3].
[0030] Effects of the Invention
[0031] The present invention relates to an epoxy resin having a specific structure, a curable resin composition and a cured product thereof, wherein the cured product has excellent heat resistance and anti-tracking properties.
[0032] Therefore, the present invention is effectively used in insulating materials for electrical and electronic parts (high reliability semiconductor sealing materials, etc.) and laminated boards (printed wiring boards, build-up substrates, etc.) or various composite materials, adhesives, coatings, etc. represented by carbon fiber reinforced plastics (CFRP). BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The gel permeation chromatography (GPC) chart of Synthesis Example 1 is shown.
[0034] Figure 2 The GPC chart of Synthesis Example 2 is shown.
[0035] Figure 3 The GPC chart of Synthesis Example 3 is shown.
[0036] Figure 4 The GPC chart of Example 1 is shown.
[0037] Figure 5 The GPC chart of Example 2 is shown.
[0038] Figure 6 The GPC chart of Example 3 is shown.
[0039] Figure 7 The GPC chart of Comparative Synthesis Example 1 is shown.
[0040] Figure 8 The GPC chart of Comparative Synthesis Example 2 is shown.
[0041] Fig. 9 This figure shows the GPC chart of FAE-2500.
[0042] Fig.10 The TMA charts of Example 4, Example 5, Comparative Example 1, and Comparative Example 2 are shown.
[0043] Fig.11 The GPC chart of Synthesis Example 4 is shown.
[0044] Fig.12 The GPC chart of Example 7 is shown.
[0045] Fig.13 The CTI measurement results of Examples 10 to 13 and Comparative Examples 5 to 8 are shown. DETAILED DESCRIPTION
[0046] The epoxy resin of the present invention is represented by the following formula (1), and the value obtained by dividing the epoxy equivalent (g / eq.) by the softening point (° C.) is 2.0 or more and less than 2.2.
[0047] [Chemistry 2]
[0048]
[0049] (In formula (1), a plurality of Rs exist independently and represent a methyl group or a hydrogen atom, and n is an average value of the number of repetitions and is a real number of 1 to 10).
[0050] In the above formula (1), n can be calculated from the number average molecular weight determined by gel permeation chromatography (GPC, detector: UV (ultraviolet) 254 nm) or the area ratio of each separated peak. n is more preferably a real number of 1 to 5, and particularly preferably a real number of 2 to 4.
[0051] When n=1 in the formula (1), it is preferably less than 50 area%, and more preferably less than 45 area%. In addition, the lower limit is 25 area%. When it is less than 25 area%, the fluidity of the resin is poor, and when it is used as a sealing material, the productivity is deteriorated. As an indicator of fluidity, the melt viscosity in the resin is used as an indicator. When the viscosity is measured by the cone and plate method at 150°C (ICI melt viscosity), the viscosity is preferably less than 2Pa·s. In addition, if the viscosity is too low, there is a possibility of air being drawn in during molding and forming voids, and sometimes adhesion occurs during the preparation (or modification) of liquid resins, etc., so it is preferably 0.4Pa·s or more. In addition, considering the balance between heat resistance and thermal decomposition characteristics, it is more preferably 0.45Pa·s or more, and particularly preferably 0.5Pa·s or more.
[0052] In addition, the compound of formula (1) wherein n is less than 1 is preferably contained in a ratio of 0.5 area % to 10 area %, more preferably 0.5 area % to 5 area %, and particularly preferably 0.5 area % to 2.5 area %. The compound wherein n is less than 1 is a compound having a structure with less than 3 functional groups or an epoxy resin of tert-butylmethylphenol. Therefore, when the compound wherein n is less than 1 exceeds 10 area %, not only is it suggested that the heat resistance is reduced, but there is also a concern about odor during handling or adverse effects on the human body. On the other hand, when the compound wherein n is less than 1 is less than 0.5 area %, there is a concern that the network becomes too dense, the weight loss caused by thermal decomposition becomes large, and the thermal decomposition characteristics are adversely affected (and it is further speculated that the tracking characteristics are adversely affected).
[0053] The epoxy resin of the present invention is generally a solid resin at room temperature, and its softening point is preferably above 90°C, and more preferably above 95°C. In addition, its upper limit is 150°C. When the softening point is higher than 150°C, the solvent is likely to remain when the resin is taken out, and voids are likely to form when hardening. In addition, foaming is likely to occur when the solvent is distilled off, and there are also large production issues. On the other hand, when the softening point is below 90°C, it has an adverse effect on heat resistance or thermal decomposition resistance. In addition, its epoxy equivalent is preferably 200g / eq. to 300g / eq., and more preferably 205g / eq. to 250g / eq. When the epoxy equivalent is lower than 200g / eq., epichlorohydrin will remain, or a large amount of epoxides will remain as impurities, and there is a possibility of deterioration of characteristics. In addition, when it exceeds 300g / eq., the reduction of heat resistance becomes a problem.
[0054] In the present invention, the epoxy equivalent is measured by a method based on Japanese Industrial Standards (JIS) K-7236. The softening point is measured using a softening point measuring instrument FP90 manufactured by METTLER TOLEDO.
[0055] The epoxy resin of the present invention is preferably an epoxy resin with a high softening point and a large number of functional groups per unit molecular weight. The softening point tends to become higher as the molecular weight increases. This means that the softening point is the temperature at which the fluidity of the resin when heated is observed, and the larger the molecular weight, the more difficult it is for the molecule to move, that is, the softening point increases. On the other hand, it is generally believed that if the softening point becomes larger, the heat resistance will increase, but for the increase in the heat resistance, it is more effective to increase the number of functional groups per unit weight, and the epoxy equivalent becomes a value related to the number of functional groups.
[0056] When the softening point is low and the epoxy equivalent is large, it is suggested that there are few functional groups per molecule, and conversely, when the softening point is high and the epoxy equivalent is small, there are many functional groups per molecule. Therefore, a compound with a high softening point and a small epoxy equivalent is preferred.
[0057] In the present invention, the value obtained by dividing the epoxy equivalent (g / eq.) by the softening point (°C) is defined as parameter A, and parameter A is preferably 2.0 or more and less than 2.2. When parameter A is less than 2.0, it is considered that some impurities remain because the epoxy equivalent is too small, and conversely, when it is 2.2 or more, it means that the epoxy equivalent is large, and the softening point is low relative to the value of the epoxy equivalent, and it is not possible to achieve both heat resistance and thermal decomposition characteristics.
[0058] Here, the thermal decomposition characteristics are considered to be a parameter that affects the tracking resistance. In the tracking test, the lower the thermal decomposition temperature, the more difficult it is to conduct between electrodes, so it is considered that it can withstand high voltage. Generally, if the molecular weight is increased, the thermal decomposition temperature tends to rise, but in the present invention, even if the molecular weight is increased, there is no significant difference in the thermal decomposition temperature, and it is considered that the high tracking resistance can be maintained.
[0059] The method for producing the epoxy resin of the present invention is not particularly limited, and the epoxy resin can be obtained, for example, by subjecting a phenol resin represented by the following formula (2) to an addition reaction or a ring-closure reaction with an epihalohydrin in the presence of a solvent and a catalyst.
[0060] [Chemistry 3]
[0061]
[0062] (In formula (2), a plurality of Rs exist independently and represent a methyl group or a hydrogen atom, and n is an average value of the number of repetitions and is a real number of 1 to 10).
[0063] In the above formula (2), n can be calculated from the number average molecular weight determined by gel permeation chromatography (GPC, detector: UV 254 nm) or the area ratio of each separated peak.
[0064] The hydroxyl equivalent of the phenol resin of formula (2) is preferably 140 g / eq. to 180 g / eq., more preferably 140 g / eq. to 165 g / eq. In addition, the amount of the compound with n=1 is preferably 30 area % to 60 area %, more preferably 40 area % to 60 area %. In addition, the total amount of the compound with n being 2 or more is preferably 25 area % to 40 area %.
[0065] Here, a method for producing the phenol resin represented by the above formula (2) will be described.
[0066] The method for preparing the phenol resin represented by the formula (2) is not particularly limited. Specifically, alkylphenols (3-methyl-6-tert-butylphenol and 4-methyl-2-tert-butylphenol) and p-hydroxybenzaldehyde are polycondensed under acidic conditions to form a novolac. Preferably, the alkylphenols (3-methyl-6-tert-butylphenol and 4-methyl-2-tert-butylphenol) and p-hydroxybenzaldehyde are reacted in a ratio of 3:2 to 2:1. Regarding the ratio of 3-methyl-6-tert-butylphenol to 4-methyl-2-tert-butylphenol, it is preferred that 90% by weight or more of the alkylphenol is 3-methyl-6-tert-butylphenol, and the ratio is adjusted by the amount of alkylphenol prepared when the phenol resin is produced. Specifically, the alkylphenol as a raw material is added according to the target alkylphenol introduction ratio.
[0067] The hydroxyl equivalent of the obtained phenol resin is preferably 140 g / eq. to 170 g / eq., more preferably 145 g / eq. to 165 g / eq., and particularly preferably 150 g / eq. to 160 g / eq.
[0068] The acidic catalyst used when synthesizing the phenol resin represented by the formula (2) can be exemplified by hydrochloric acid, phosphoric acid, sulfuric acid, formic acid, zinc chloride, ferric chloride, aluminum chloride, p-toluenesulfonic acid, methanesulfonic acid, activated clay, ion exchange resin, etc. These can be used alone or in combination of two or more. The amount of the catalyst used is 0.1% to 50% by weight, preferably 1% to 30% by weight, relative to the phenolic hydroxyl group used. If too much, waste increases, and if too little, the reaction proceeds slowly.
[0069] The reaction can be carried out using an organic solvent as required, or can be carried out without a solvent. Wherein, by subjecting the water to be purified during the reaction to azeotropic dehydration, the reaction can be carried out more efficiently, so it is preferred to utilize a solvent that can azeotrope with water. In the present invention, it is particularly preferred to use a hydrocarbon organic solvent such as toluene or xylene.
[0070] Thereafter, washing or neutralization is performed, and the resin is taken out after distilling off the solvent, or the resin can be taken out by reprecipitation or recrystallization. Since the softening point of the phenol resin represented by the formula (2) is very high, it is preferably taken out by reprecipitation or recrystallization, for example, by replacing the solvent with a poor solvent to precipitate it.
[0071] The phenol resin represented by the formula (2) is a crystal or a resin solid, and the ratio of n=1 in the GPC is preferably less than 60%. In particular, it is less than 55 area%, and further less than 50 area%. The total amount of the residual raw material monomer is preferably less than 5 area%, and each peak is preferably less than 1.5 area%. The amount of this monomer affects the residual amount of low molecular weight of the epoxy resin, and the amount affects heat resistance, etc.
[0072] Next, the method for producing the epoxy resin of the present invention will be described.
[0073] As described above, the method for producing the epoxy resin of the present invention is not particularly limited, and the epoxy resin can be obtained, for example, by subjecting the phenol resin represented by the formula (2) to an addition reaction or a ring-closure reaction with an epihalohydrin in the presence of a solvent and a catalyst.
[0074] The amount of epihalohydrin used is usually 1.0 mol to 20.0 mol, preferably 1.5 mol to 10.0 mol, based on 1 mol of the phenolic hydroxyl groups of the phenol resin.
[0075] As the alkali metal hydroxide that can be used in the epoxidation reaction, sodium hydroxide, potassium hydroxide, etc. can be listed. The alkali metal hydroxide can be a solid substance, and its aqueous solution can also be used. In the case of using an aqueous solution, it can be the following method: the aqueous solution of the alkali metal hydroxide is continuously added to the reaction system, and water and epihalohydrin are continuously distilled out under reduced pressure or under normal pressure, and then liquid separation is carried out to remove water, so that epihalohydrin is continuously returned to the reaction system. Relative to 1 mole of phenolic hydroxyl groups of phenol resin, the usage amount of alkali metal hydroxide is generally 0.9 mole to 2.5 moles, preferably 0.95 mole to 1.5 moles. If the usage amount of alkali metal hydroxide is small, the reaction will not be fully carried out. On the other hand, the situation of excessively using more than 2.5 moles of alkali metal hydroxide relative to 1 mole of phenolic hydroxyl groups of phenol resin can cause unnecessary waste to be generated by the side.
[0076] In order to promote the reaction, quaternary ammonium salts such as tetramethylammonium chloride, tetramethylammonium bromide, trimethylbenzylammonium chloride, etc. may also be added as catalysts. The usage amount of the quaternary ammonium salt is usually 0.1 g to 15 g, preferably 0.2 g to 10 g, relative to 1 mol of the phenolic hydroxyl group of the phenol resin. If the usage amount is too small, sufficient reaction promotion effect cannot be obtained. If the usage amount is too large, the amount of the quaternary ammonium salt remaining in the epoxy resin increases, so it is also possible to become the cause of deterioration of electrical reliability.
[0077] During epoxidation, in terms of reaction, it is preferred to add aprotic polar solvents such as alcohols such as methanol, ethanol, isopropanol, dimethyl sulfone, dimethyl sulfoxide, tetrahydrofuran, dioxane, etc. to react. When using alcohols, its usage is generally 2% by weight to 50% by weight relative to the usage of epihalohydrin, preferably 4% by weight to 20% by weight. In addition, when using aprotic polar solvents, its usage is generally 5% by weight to 100% by weight relative to the usage of epihalohydrin, preferably 10% by weight to 80% by weight. The reaction temperature is generally 30°C to 90°C, preferably 35°C to 80°C. The reaction time is generally 0.5 hours to 100 hours, preferably 1 hour to 30 hours.
[0078] After the reaction is completed, the epihalohydrin or solvent is removed after washing the reactant or without washing under heating and reduced pressure. In addition, in order to make an epoxy resin with less hydrolyzable halogen, the recovered epoxy resin can also be dissolved in solvents such as toluene and methyl isobutyl ketone, and an aqueous solution of alkali metal hydroxides such as sodium hydroxide and potassium hydroxide is added to react, so that the closed loop is reliable. In this case, the amount of alkali metal hydroxide used is generally 0.01 mol to 0.3 mol, preferably 0.05 mol to 0.2 mol, relative to 1 mol of phenolic hydroxyl groups of the phenol resin used in glycidylation. The reaction temperature is generally 50°C to 120°C, and the reaction time is generally 0.5 hours to 24 hours. After the reaction is completed, the generated salt is removed by filtration, washing, etc., and then the solvent is distilled off under heating and reduced pressure to obtain the epoxy resin of the present invention.
[0079] Hereinafter, the curable resin composition of the present invention will be described.
[0080] Regarding the epoxy resin used in the curable resin composition of the present invention, the epoxy resin represented by the formula (1) can be used alone or in combination with other epoxy resins. When used in combination, the proportion of the epoxy resin represented by the formula (1) in all epoxy resins is preferably 10% to 98% by weight, more preferably 30% to 95% by weight, and even more preferably 60% to 95% by weight. By setting the addition amount of the epoxy resin represented by the formula (1) to 10% or more, an improvement in elastic modulus and low water absorption can be achieved.
[0081] Specific examples of other epoxy resins that can be used in combination with the epoxy resin represented by the formula (1) include: polycondensates of bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.) or phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, o-phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.); polycondensates of the phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinyl norbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.); ) polymers; polycondensates of the phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.); polycondensates of the phenols and aromatic dimethanols (benzenedimethanol, biphenyl dimethanol, etc.); polycondensates of the phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethyl biphenyl, etc.); polycondensates of the phenols and aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethylbiphenyl, bisphenoxymethylbiphenyl, etc.); polycondensates of the bisphenols and various aldehydes or glycidyl ether epoxy resins, alicyclic epoxy resins, glycidylamine epoxy resins, glycidyl ester epoxy resins, etc. obtained by glycidylating alcohols, etc., are not limited to these as long as they are commonly used epoxy resins. These may be used alone or in combination of two or more.
[0082] Examples of the curing agent that can be used in the curable resin composition of the present invention include amine curing agents, acid anhydride curing agents, amide curing agents, and phenol curing agents. Specific examples of the curing agent that can be used include o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,2'-diaminodiphenyl sulfone, diethyltoluenediamine, dimethylthiotoluenediamine, diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 4,4 '-Diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetramethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetraethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetraisopropyldiphenylmethane, 4,4'-methylenebis(N-methylaniline), bis(aminophenyl)fluorene, 3,4'-diaminodiphenyl ether, 4,4'-diamino Diphenyl ether, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)biphenyl, 4,4'-(1,3-phenylenediisopropylidene)dianiline, 4,4'-(1,4-phenylenediisopropylidene)dianiline, naphthalene diamine, benzidine, dimethylbenzidine, international Aromatic amine compounds such as those described in Synthesis Example 1 and Synthesis Example 2 of Publication No. 2017 / 170551; aliphatic amines such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), norbornanediamine, ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, dimer diamine, triethylenetetramine, etc., but are not limited thereto and can be used appropriately according to the properties to be imparted to the composition. In order to ensure the pot life, it is preferred to use aromatic amines, and in the case of imparting instant curability, it is preferred to use aliphatic amines. By using an amine compound containing a difunctional component as a main component as a curing agent, a highly linear network can be constructed during the curing reaction, thereby exhibiting particularly excellent toughness.In addition, amide compounds such as dicyandiamide, polyamide resin synthesized from dimer of linolenic acid and ethylenediamine; anhydride compounds such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride; bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol , bisphenol AD, etc.) or condensation products of phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, o-phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), or condensation products of the phenols and various diene compounds (dicyclopentadiene, terpenes, etc.) Polymers of the phenols described herein (including but not limited to phenolic compounds such as vinylcyclohexene, vinyl cyclohexene, norbornadiene, vinyl norbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.), or polycondensates of the phenols described herein with ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.), or polycondensates of the phenols described herein with aromatic dimethanols (benzenedimethanol, biphenyl dimethanol, etc.), or polycondensates of the phenols described herein with aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.), or polycondensates of the phenols described herein with aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethylbiphenyl, bisphenoxymethylbiphenyl, etc.), or polycondensates of the bisphenols described herein with various aldehydes, and modified products thereof; imidazole, trifluoroborane-amine complex, guanidine derivatives, etc., but are not limited to these.
[0083] In the curable resin composition of the present invention, the amount of the curing agent used is preferably 0.5 to 1.5 equivalents, particularly preferably 0.6 to 1.2 equivalents, per 1 equivalent of epoxy groups of the epoxy resin. By setting the amount to 0.5 to 1.5 equivalents, good curing properties can be obtained.
[0084] When the curing reaction is carried out using the curing agent, a curing accelerator may also be used in combination. Examples of the curing accelerator include: imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole; tertiary amines such as 2-(dimethylaminomethyl)phenol, triethylenediamine, triethanolamine, and 1,8-diazabicyclo(5,4,0)undecene-7; organic phosphines such as triphenylphosphine, diphenylphosphine, and tributylphosphine; metal compounds such as tin octoate; tetraphenylphosphonium-tetraphenylborate, tetraphenylphosphonium-ethyltriphenylborate, and other tetrasubstituted phosphonium-tetrasubstituted borates; tetraphenylboron salts such as 2-ethyl-4-methylimidazole-tetraphenylborate and N-methylmorpholine-tetraphenylborate; carboxylic acid compounds such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthoic acid, and salicylic acid. From the viewpoint of promoting the curing reaction between the amine compound and the epoxy resin, a carboxylic acid compound such as salicylic acid is preferred. The curing accelerator may be used in an amount of 0.01 to 15 parts by weight based on 100 parts by weight of the epoxy resin as required.
[0085] Furthermore, in the curable resin composition of the present invention, an inorganic filler may be added as needed. As inorganic fillers, crystalline silica, fused silica, alumina, zircon, calcium silicate, calcium carbonate, silicon carbide, silicon nitride, boron nitride, zirconium oxide, forsterite, steatite, spinel, titanium dioxide, talc, etc., or beads formed by spheroidizing these, etc., can be cited, but are not limited to these. These can be used alone or in combination. The amount of these inorganic fillers used varies depending on the purpose, but for example, in the case of a sealant for semiconductors, in terms of heat resistance, moisture resistance, mechanical properties, flame retardancy, etc. of the cured product of the curable resin composition, it is preferably used in a proportion of 20% by weight or more in the curable resin composition, more preferably 30% by weight or more, especially in order to increase the linear expansion coefficient relative to the lead frame, and then preferably in a proportion of 70% by weight to 95% by weight.
[0086] Furthermore, in the present invention, the content of the inorganic filler is important, especially in terms of improving the tracking resistance. In consideration of the tracking resistance, the preferred content of the inorganic filler in the total amount of the curable resin composition of the present invention is 74% by weight or more and 95% by weight or less, and particularly preferably 78% by weight or more and 95% by weight or less. In the case of the epoxy resin structure of the present invention, it can be confirmed that if it is 74% by weight or more, the tracking resistance is greatly improved, and in the case of less than 74% by weight, for example, in the case of less than 70% by weight, the tracking performance is less superior to other epoxy resins.
[0087] In the curable resin composition of the present invention, a release agent may be formulated to facilitate demolding from a mold during molding. As a release agent, any of the known ones may be used, for example, ester waxes such as carnauba wax and montan wax; fatty acids such as stearic acid and palmitic acid and their metal salts; polyolefin waxes such as oxidized polyethylene and non-oxidized polyethylene, etc. These may be used alone or in combination of two or more. The amount of these release agents formulated is preferably 0.5 wt% to 3 wt% relative to all organic components. If it is less than this, demolding from the mold will deteriorate, and if it is more than this, adhesion to the lead frame, etc. will deteriorate.
[0088] In the curable resin composition of the present invention, a coupling agent may be adjusted to improve the adhesion between the inorganic filler and the resin component. As a coupling agent, any of the existing known ones can be used, for example, various alkoxysilane compounds such as vinyl alkoxysilane, epoxy alkoxysilane, styryl alkoxysilane, methacryloxy alkoxysilane, acryloxy alkoxysilane, amino alkoxysilane, mercapto alkoxysilane, isocyanate alkoxysilane, alkoxy titanium compounds, aluminum chelates, etc. These can be used alone or in combination of two or more. Regarding the method of adding the coupling agent, the inorganic filler surface can be treated with the coupling agent in advance and then mixed with the resin, or the inorganic filler can be mixed with the coupling agent after mixing the resin.
[0089] Furthermore, the curable resin composition of the present invention may be formulated with known additives as needed. Specific examples of usable additives include polybutadiene and modified products thereof, modified products of acrylonitrile copolymers, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, maleimide compounds, cyanate compounds, silicone gel, silicone oil, and colorants such as carbon black, phthalocyanine blue, and phthalocyanine green.
[0090] The curable resin composition of the present invention is obtained by uniformly mixing the above-mentioned components. The curable resin composition of the present invention can be easily made into a cured product by the same method as the conventionally known method. For example, the curable resin composition of the present invention is obtained by fully mixing the epoxy resin and the curing agent, and the curing accelerator, inorganic filler, release agent, silane coupling agent and additives as required using an extruder, a kneader, a roller, etc. until they are uniform, and then the curable resin composition is molded by melt casting, transfer molding, injection molding, compression molding, etc., and then heated at 80°C to 200°C for 2 hours to 10 hours to obtain a cured product.
[0091] In addition, the curable resin composition of the present invention may also contain a solvent as needed. The curable resin composition (epoxy resin varnish) containing a solvent is impregnated into a fibrous material (substrate) such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, paper, etc. and heated and dried to obtain a prepreg, and the obtained prepreg is hot-pressed to form a cured product of the curable resin composition of the present invention. The solvent content of the curable resin composition is generally 10% to 70% by weight, preferably about 15% to 70% by weight, as an internal ratio. As the solvent, for example, γ-butyrolactones; amide solvents such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-dimethylimidazolidinone; sulfones such as tetramethylene sulfone; ether solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and propylene glycol monobutyl ether, preferably mono- or di-lower (carbon number 1-3) alkyl ethers of lower (carbon number 1-3) alkanediols; ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, more preferably di-lower (carbon number 1-3) alkyl ketones in which two alkyl groups may be the same or different; aromatic solvents such as toluene and xylene, etc. These may be used alone or as a mixed solvent of two or more.
[0092] In addition, by applying the epoxy resin varnish onto a release film and removing the solvent under heating to perform B-stage, a sheet-like adhesive can be obtained. The sheet-like adhesive can be used as an interlayer insulating layer in a multilayer substrate or the like.
[0093] The cured product obtained in the present invention can be used for various purposes. Specifically, general uses of thermosetting resins such as epoxy resins can be listed, for example, adhesives, coatings, coating agents, forming materials (including sheets, films, FRP, etc.), insulating materials (including printed circuit boards, wire coatings, etc.), sealants, and additives to other resins, etc.
[0094] Examples of adhesives include adhesives for civil engineering, construction, automobiles, general business, medical use, and adhesives for electronic materials. Among these, adhesives for electronic materials include adhesives for semiconductors such as interlayer adhesives for multilayer substrates such as build-up substrates, die bonding agents, and bottom fillers; bottom fillers for ball grid array (BGA) enhancement, anisotropic conductive film (ACF), anisotropic conductive paste (ACP) and other mounting adhesives.
[0095] Examples of the sealant include potting seals, immersion seals, and transfer mold seals for capacitors, transistors, diodes, light-emitting diodes, ICs, large scale integration circuits (LSIs), and the like; potting seals for ICs and LSIs such as chip on board (COB), chip on film (COF), and tape automated bonding (TAB); bottom fillers for flip chips; and sealing (including reinforcement bottom fillers) during installation of IC packages such as quad flat packages (QFPs), ball grid arrays (BGAs), and chip size packages (CSPs).
[0096] Example
[0097] Next, the present invention will be described in more detail by way of examples, and parts are parts by weight unless otherwise specified. The present invention is not limited to these examples.
[0098] Epoxy equivalent
[0099] The measurement was carried out according to the method based on JIS K-7236.
[0100] Softening point
[0101] The softening point was measured using a softening point tester FP90 manufactured by METTLER TOLEDO.
[0102] Hydroxyl equivalent
[0103] The sample was acetylated using acetic anhydride in a pyridine solution. After the acetylation was completed, the remaining anhydride was decomposed with water and titrated using a 0.5N KOH ethanol solution with a potentiometric titrator to measure the amount of free acetic acid. The hydroxyl equivalent was calculated based on the result.
[0104] ·GPC (Gel Permeation Chromatography)
[0105] (Measurement Condition 1)
[0106] Device: Waters e2695
[0107] Column: Showa Denko (SHODEX) GPC KF-401HQ, KF-402HQ, KF-403HQ, KF-404HQ, total 4
[0108] Flow rate: 0.3ml / min
[0109] Column temperature: 40℃
[0110] Solvent used: tetrahydrofuran (THF)
[0111] Detector: UV 254nm
[0112] (Measurement Condition 2)
[0113] Device: HLC-8220GPC of Tosoh Corporation
[0114] Column: 1 TSK gel G3000HXL, 2 TSK gel G2000HXL, 3 in total, from Tosoh Corporation
[0115] Flow rate: 1.065ml / min
[0116] Column temperature: 40℃
[0117] Solvent used: tetrahydrofuran (THF)
[0118] Detector: UV 254nm
[0119] (Measurement Condition 3)
[0120] Device: HLC-8420GPC of Tosoh Corporation
[0121] Column: 1 TSK gel G3000HXL, 2 TSK gel G2000HXL, 3 in total, from Tosoh Corporation
[0122] Flow rate: 1.065ml / min
[0123] Column temperature: 40℃
[0124] Solvent used: tetrahydrofuran (THF)
[0125] Detector: UV 254nm
[0126] Standard polystyrene (TOSOH Corporation)
[0127] PStQuickC, PStQuickD (add styrene as an internal standard for calibration during molecular weight measurement)
[0128] [Synthesis example 1]
[0129] While nitrogen was purged into a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 137.2 parts of 3-methyl-6-tert-butylphenol, 0.16 parts of 4-methyl-2-tert-butylphenol, 60 parts of p-hydroxybenzaldehyde, 142 parts of toluene, and 1.4 parts of p-toluenesulfonic acid were added, and the reaction was carried out at 110°C to 115°C for 8 hours. After the reaction was completed, 25% NaOH water was added, and toluene was removed by azeotropic dehydration distillation. Thereafter, 75% sulfuric acid was added to adjust the pH to 5 to 7, and the precipitated resin powder was filtered and dried at 60°C to obtain 186 parts of phenol resin (P1). The obtained phenol resin (P1) was in powder form, had a softening point of 150°C or more, a hydroxyl equivalent of 155 g / eq., and 48.8 area % when n=1 based on GPC. The GPC chart (measurement condition 1) is shown at Figure 1 .
[0130] [Synthesis example 2]
[0131] While nitrogen was purged into a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 153.1 parts of 3-methyl-6-tert-butylphenol, 0.17 parts of 4-methyl-2-tert-butylphenol, 60 parts of p-hydroxybenzaldehyde, 142 parts of toluene, and 0.6 parts of p-toluenesulfonic acid were added, and the reaction was carried out at 100°C to 105°C for 6 hours. After the reaction was completed, 25% NaOH water was added, and toluene was removed by azeotropic dehydration distillation. Thereafter, 75% sulfuric acid was added to adjust the pH to 5 to 7, and the precipitated resin powder was filtered and dried at 60°C to obtain 198 parts of phenol resin (P2). The obtained phenol resin (P2) was in powder form, had a softening point of 150°C or more, a hydroxyl equivalent of 144 g / eq., and based on GPC, when n=1, it was 51.7 area%. The GPC chart (measurement condition 1) is shown at Figure 2 .
[0132] [Synthesis example 3]
[0133] While nitrogen was purged into a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 137.2 parts of 3-methyl-6-tert-butylphenol, 0.16 parts of 4-methyl-2-tert-butylphenol, 60 parts of p-hydroxybenzaldehyde, 142 parts of toluene, and 1.4 parts of p-toluenesulfonic acid were added, and the reaction was carried out at 110°C to 115°C for 8 hours. After the reaction was completed, 25% NaOH water was added, and toluene was removed by azeotropic dehydration distillation. Thereafter, 75% sulfuric acid was added to adjust the pH to 5 to 7, and the precipitated resin powder was filtered and dried at 60°C to obtain 180 parts of phenol resin (P3). The obtained phenol resin (P3) was in powder form, had a softening point of 150°C or more, a hydroxyl equivalent of 153 g / eq., and based on GPC, when n=1, it was 47.6 area%. The GPC chart (measurement condition 1) is shown at Figure 3 .
[0134] [Example 1]
[0135] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 310 parts of the phenol resin (P1) obtained in Synthesis Example 1, 973 parts of epichlorohydrin, 274 parts of dimethyl sulfoxide, and 15 parts of water were added, and the internal temperature was raised to 45°C. After adding 16 parts of sodium hydroxide in batches over 1.5 hours, the mixture was reacted at 45°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 1040 parts of methyl isobutylketone (MIBK) were added, and the organic layer was washed once with 440 parts of water. The organic layer was returned to the reaction vessel, 20 parts of a 30 wt% sodium hydroxide aqueous solution were added, and the mixture was reacted at 70°C for 2 hours. After cooling, the organic layer was washed four times with 130 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 170 parts of epoxy resin (E1) as a solid resin. The epoxy equivalent is 214 g / eq., the ICI viscosity (150°C) is 0.57 Pa·s, the softening point is 100°C, and the parameter A is 2.14. The average repeating unit n estimated by GPC (detector UV 254 nm) is 2.4, 42.3 area% when n=1, and 1.57 area% when n is less than 1. The GPC chart (measurement condition 2) is shown at Figure 4 .
[0136] [Example 2]
[0137] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 310 parts of the phenol resin (P1) obtained in Synthesis Example 1, 584 parts of epichlorohydrin, 274 parts of dimethyl sulfoxide, and 15 parts of water were added, and the internal temperature was raised to 45°C. After adding 16 parts of sodium hydroxide in batches over 1.5 hours, the mixture was reacted at 45°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 1040 parts of MIBK were added, and the organic layer was washed once with 440 parts of water. The organic layer was returned to the reaction vessel, 20 parts of a 30wt% sodium hydroxide aqueous solution were added, and the mixture was reacted at 70°C for 2 hours. After cooling, the organic layer was washed four times with 130 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 141 parts of epoxy resin (E2) as a solid resin. The epoxy equivalent is 225 g / eq., the ICI viscosity (150°C) is 1.92 Pa·s, the softening point is 110°C, and the parameter A is 2.05. The average repeating unit n estimated by GPC (detector UV 254 nm) is 2.9, 31.1 area% when n=1, and 1.28 area% when n is less than 1. The GPC chart (measurement condition 2) is shown at Figure 5 .
[0138] [Example 3]
[0139] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 310 parts of the phenol resin (P3) obtained in Synthesis Example 3, 778 parts of epichlorohydrin, 274 parts of dimethyl sulfoxide, and 15 parts of water were added, and the internal temperature was raised to 45°C. After adding 16 parts of sodium hydroxide in batches over 1.5 hours, the reaction was carried out at 45°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 1040 parts of MIBK were added, and the organic layer was washed once with 440 parts of water. The organic layer was returned to the reaction vessel, 20 parts of a 30% by weight sodium hydroxide aqueous solution were added, and the reaction was carried out at 70°C for 2 hours. After cooling, the organic layer was washed four times with 130 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 303 parts of epoxy resin (E3) as a solid resin. The epoxy equivalent is 216 g / eq., the total chlorine is 440 ppm (based on ISO 21627-3), the inorganic chloride ion concentration is 0.3 ppm, the ICI viscosity (150°C) is 0.64 Pa·s, the softening point is 100°C, and the parameter A is 2.16. The Mn estimated by GPC (detector UV 254 nm) is 1059, the Mw is 2001 (polystyrene conversion), and the area ratio is 39.5% when n=1 and 1.95% when n is less than 1. The GPC chart (measurement condition 3) is shown in Figure 6 .
[0140] [Comparative Synthesis Example 1]
[0141] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 288 parts of the phenol resin (P2) obtained in Synthesis Example 2, 584 parts of epichlorohydrin, 274 parts of dimethyl sulfoxide, and 15 parts of water were added, and the internal temperature was raised to 45°C. After adding 16 parts of sodium hydroxide in batches over 1.5 hours, the mixture was reacted at 45°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 1040 parts of MIBK were added, and the organic layer was washed once with 440 parts of water. The organic layer was returned to the reaction vessel, 20 parts of a 30% by weight sodium hydroxide aqueous solution were added, and the mixture was reacted at 70°C for 2 hours. After cooling, the organic layer was washed four times with 130 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 165 parts of epoxy resin (E4) as a solid resin. The epoxy equivalent is 223 g / eq., the ICI viscosity (150°C) is 0.60 Pa·s, the softening point is 99.7°C, and the parameter A is 2.24. The average repeating unit n estimated by GPC is 2.4, 43.9 area% when n=1, and 1.9 area% when n is less than 1. The GPC chart (measurement condition 2) is shown at Figure 7 .
[0142] [Comparative Synthesis Example 2]
[0143] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 288 parts of the phenol resin (P2) obtained in Synthesis Example 2, 487 parts of epichlorohydrin, 274 parts of dimethyl sulfoxide, and 15 parts of water were added, and the internal temperature was raised to 45°C. After adding 16 parts of sodium hydroxide in batches over 1.5 hours, the mixture was reacted at 45°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 1040 parts of MIBK were added, and the organic layer was washed once with 440 parts of water. The organic layer was returned to the reaction vessel, 20 parts of a 30% by weight sodium hydroxide aqueous solution were added, and the mixture was reacted at 70°C for 2 hours. After cooling, the organic layer was washed four times with 130 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 161 parts of epoxy resin (E5) as a solid resin. The epoxy equivalent is 224 g / eq., the ICI viscosity (150°C) is 0.66 Pa·s, the softening point is 100.9°C, and the parameter A is 2.22. The average repeating unit n estimated by GPC is 2.3, 43 area% when n=1, and 2.1 area% when n is less than 1. The GPC chart (measurement condition 2) is shown at Figure 8 .
[0144] [Example 4, Example 5, Comparative Example 1, Comparative Example 2]
[0145] Using FAE-2500 (manufactured by Nippon Kayaku, analysis results will be described later) of epoxy resins E1, E2, E4, and E6 obtained in the examples and synthesis examples, triphenylmethane-type phenol resin (KAYAHARD KTG-105 manufactured by Nippon Kayaku) as a curing agent, and triphenylphosphine as a catalyst, an equivalent amount of triphenylmethane-type phenol resin was formulated with respect to the epoxy resin, and 1 phr of triphenylphosphine was formulated with respect to the epoxy resin, and the mixture was uniformly mixed / kneaded using a mixing roller, and then demolded, and then hardened under the conditions of 160°C × 2 hours + 180°C × 6 hours to obtain a test piece for evaluation.
[0146] The epoxy equivalent of FAE-2500 is 213 g / eq., the ICI viscosity (150°C) is 0.30 Pa·s, the softening point is 93.5°C, and the parameter A is 2.28. The GPC chart (measurement condition 2) is shown in Fig. 9 .
[0147] The results of the evaluation test pieces measured under the following conditions are shown in Table 1. In addition, the thermomechanical analysis (TMA) chart is shown in Fig.10 .
[0148] <Dynamic Viscoelasticity Measurement (DMA)>
[0149] The glass transition temperature (temperature at which tan δ is maximum) and the value of tan δ at that time were measured using a dynamic viscoelasticity tester.
[0150] Dynamic viscoelasticity tester: DMA-2980 manufactured by TA-instruments
[0151] Heating rate: 2℃ / min
[0152] <Thermomechanical properties measurement (TMA)>
[0153] The glass transition temperature (Tg) and coefficient of thermal expansion (CTE) were evaluated using a thermomechanical property measuring device.
[0154] <Thermogravimetric-differentialthermal analysis (TG-DTA)>
[0155] The thermal decomposition temperature and the residual carbon content at 500°C were measured by TG-DTA.
[0156] Test sample: Powder (passing through 100 μm mesh and retained in 75 μm mesh) 5 mg to 10 mg
[0157] Measurement conditions: Heating rate 10℃ / min Air flow 200ml
[0158] [Table 1]
[0159]
[0160] [Example 6, Comparative Example 3]
[0161] An epoxy resin (E1), an epoxy resin (E6, FAE-2500 (manufactured by Nippon Kayaku), a XYLOK type phenol resin (MEHC-7800SS manufactured by Meiwa Chemical) as a hardener, triphenylphosphine (TPP, manufactured by Tokyo Chemical Industry Co., Ltd.) as a catalyst, silica gel (fused silica MSR-2212, manufactured by Ronson) as an inorganic filler, palm wax (Cera Rica, manufactured by Noda) as a release agent, and a silane coupling agent (trade name: KBM-303, manufactured by Shin-Etsu Chemical Co., Ltd.) as an additive were uniformly mixed and kneaded using a mixing roll to obtain a curable resin composition.
[0162] The curable resin composition was crushed and tableted using a tablet press. The tableted curable resin composition was transfer molded (175°C for 60 minutes to 150 minutes), and after demolding, it was cured under the conditions of 160°C for 2 hours + 180°C for 6 hours to obtain an evaluation test piece. The following evaluation was performed using this test piece. The measurement results are recorded in Table 2.
[0163] <Tracking resistance test>
[0164] Applicable standards IEC-Pub.60112-2003 (4th edition) and JIS-C2134-2007
[0165] Test voltage: 400V~600V
[0166] Test solution: 0.1% ammonium chloride aqueous solution
[0167] The number of drops is 50. If the test piece is broken due to less than 50 drops, it is judged as NG.
[0168] The temperature and humidity of the test room are 21℃~23℃40%RH~45%RH
[0169] Test equipment: YST-112 tracking tester manufactured by Yamayo Testing Machine Co., Ltd.
[0170] Test sample shape: diameter 50mm, thickness 3mm
[0171] 1 point per piece
[0172] [Table 2]
[0173]
[0174] The results in Table 1 show that the epoxy resin of the present invention has high heat resistance and dimensional stability (low linear expansion). In addition, the results in Table 2 show that the epoxy resin of the present invention has high tracking resistance.
[0175] [Synthesis Example 4]
[0176] While nitrogen was purged into a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 130.3 parts of 3-methyl-6-tert-butylphenol, 0.2 parts of 4-methyl-2-tert-butylphenol, 60 parts of p-hydroxybenzaldehyde, 142 parts of toluene, and 1.4 parts of p-toluenesulfonic acid were added, and the reaction was carried out at 110°C to 115°C for 8 hours. After the reaction was completed, 25% NaOH water was added, and toluene was removed by azeotropic dehydration distillation. Thereafter, 75% sulfuric acid was added to adjust the pH to 5 to 7, and the precipitated resin powder was filtered and dried at 60°C to obtain 186 parts of phenol resin (P4). The obtained phenol resin (P4) was in powder form, had a softening point of more than 200°C, a hydroxyl equivalent of 160 g / eq., and 37.0 area % when n=1 based on GPC. The GPC chart (measurement condition 1) is shown at Fig.11 .
[0177] [Example 7]
[0178] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 320 parts of the phenol resin (P4) obtained in Synthesis Example 4, 973 parts of epichlorohydrin, 274 parts of dimethyl sulfoxide, and 15 parts of water were added, and the internal temperature was raised to 45°C. After adding 16 parts of sodium hydroxide in batches over 1.5 hours, the reaction was carried out at 45°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 1040 parts of MIBK were added, and the organic layer was washed once with 440 parts of water. The organic layer was returned to the reaction vessel, 20 parts of a 30% by weight sodium hydroxide aqueous solution were added, and the reaction was carried out at 70°C for 2 hours. After cooling, the organic layer was washed four times with 130 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 107 parts of epoxy resin (E7) as a solid resin. The epoxy equivalent is 220 g / eq., the ICI viscosity (150°C) is 0.8 Pa·s or more, the softening point is 108.5°C, and the parameter A is 2.03. The average repeating unit n estimated by GPC (detector UV 254 nm) is 3.4, 24.9 area% when n=1, and 2.91 area% when n is less than 1. The GPC chart (measurement condition 3) is shown at Fig.12 In addition, the peak with a retention time of 35.619 minutes accounted for 1.75% by area, and the other peaks accounted for less than 1.5% by area.
[0179] [Example 8, Example 9]
[0180] The epoxy resin E3 and epoxy resin E7 obtained in the above examples, trisphenol methane type phenol resin (Kayahard KTG-105 manufactured by Nippon Kayaku, hydroxyl equivalent 102 g / eq.), biphenyl aralkyl type phenol resin (Kayahard GPH-65 manufactured by Nippon Kayaku, hydroxyl equivalent 200 g / eq.) as a curing agent, triphenylphosphine (TPP, manufactured by Tokyo Chemical Industry Co., Ltd.) as a catalyst, silica gel (fused silica MSR-2212, manufactured by Ronson) as an inorganic filler, palm wax (Cera Rica, manufactured by Noda) as a mold release agent, and silane coupling agent (trade name: KBM-303, manufactured by Shin-Etsu Chemical Co., Ltd.) as an additive were prepared according to the ratio (parts by weight) in Table 3, uniformly mixed and kneaded using a mixing roll, and then demolded and cured under the conditions of 160° C.×2 hours+180° C.×6 hours to obtain a test piece for evaluation. The test piece was used to carry out the tracking resistance test. The measurement results are shown in Table 3.
[0181] [Table 3]
[0182]
[0183] [Example 9, Comparative Example 4]
[0184] The epoxy resin E1 obtained in the above-mentioned example, a biphenyl aralkyl type epoxy resin (NC-3000 manufactured by Nippon Kayaku), a XYLOK type phenol resin (MEHC-7800SS manufactured by Meiwa Chemical Industry Co., Ltd.) as a hardener, triphenylphosphine (TPP, manufactured by Tokyo Chemical Industry Co., Ltd.) as a catalyst, silica gel (fused silica MSR-2212, manufactured by Ronson) as an inorganic filler, carnauba wax (Cera Rica, manufactured by Noda) as a release agent, and a silane coupling agent (trade name: KBM-303 manufactured by Shin-Etsu Chemical Industry Co., Ltd.) as an additive were used and uniformly mixed and kneaded using a mixing roll to obtain a curable resin composition.
[0185] The curable resin composition was crushed and tableted using a tablet press. The tableted curable resin composition was transfer molded (175°C for 60 minutes to 15 minutes), and then demolded and cured under the conditions of 160°C × 2 hours + 180°C × 6 hours to obtain an evaluation test piece. This test piece was used to conduct a tracking resistance test. The measurement results are recorded in Table 4.
[0186] [Table 4]
[0187]
[0188] [Example 10 to Example 13, Comparative Example 5 to Comparative Example 8]
[0189] The epoxy resin E1 obtained in the above example, a biphenyl aralkyl type epoxy resin (NC-3000 manufactured by Nippon Kayaku), a XYLOK type phenol resin (MEHC-7800SS manufactured by Meiwa Chemical) as a hardener, a biphenyl aralkyl type phenol resin (KAYAHARD GPH-65 manufactured by Nippon Kayaku), a catalyst triphenylphosphine (TPP, manufactured by Tokyo Chemical Industry Co., Ltd.), a silica gel (fused silica MSR-2212, manufactured by Ronson) as an inorganic filler, a carnauba wax (Cera Rica, manufactured by Noda) as a release agent, and a silane coupling agent (trade name: KBM-303, manufactured by Shin-Etsu Chemical Co., Ltd.) as an additive were uniformly mixed and kneaded using a mixing roll to obtain a curable resin composition.
[0190] After the curable resin composition is crushed, it is tableted using a tablet press. The tableted curable resin composition is transfer molded (175°C for 60 minutes to 15 minutes), and then after demolding, it is cured under the conditions of 160°C × 2 hours + 180°C × 6 hours to obtain an evaluation test piece. This test piece is used to carry out a leakage tracking resistance test. In particular, regarding CTI, it is measured using a measurement method based on IEC-Pub.60112-2003 (4th edition). The measurement results are recorded in Table 5. Fig.13 .
[0191] [Table 5]
[0192]
[0193] The above results show that the cured product using the epoxy resin of the present invention maintains a relatively high CTI, and in particular, the CTI increase rate is higher in a formulation where the inorganic filler content is 74 wt % or more, more preferably 78 wt % or more, than in other compositions.
[0194] Industrial Applicability
[0195] The epoxy resin of the present invention is effective for applications in vehicle-mounted materials, particularly power device peripheral materials, and is particularly effective for applications requiring heat resistance and a high comparative tracking index (CTI).
Claims
1. An epoxy resin represented by the following formula (1), wherein the value obtained by dividing the epoxy equivalent (g / eq.) by the softening point (° C.) is 2.0 or more and less than 2.2, In formula (1), a plurality of Rs independently represent a methyl group or a hydrogen atom; n is an average value of the number of repetitions and is a real number of 1 to 10.
2. A curable resin composition comprising the epoxy resin according to claim 1. 3 . The curable resin composition according to claim 2 , wherein the content of the inorganic filler is 74% by weight or more and 95% by weight or less in the total amount of the curable resin composition.
4. A cured product obtained by curing the curable resin composition according to claim 2 or 3.