A High-Entropy Activation Flotation Method for Low-Grade Scheelite
By combining activators and inhibitors, the flotation recovery rate of low-grade scheelite was improved, solving the problem of low tungsten resource recovery and achieving efficient recovery under low-temperature conditions.
Patent Information
- Application Number
- CN202311217802.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-20
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-20
AI Technical Summary
Low-grade scheelite is closely associated with calcium-bearing gangue minerals, resulting in low tungsten resource recovery rate and poor concentrate quality. Existing collectors have poor selectivity and high cost, and the consumption of reagents during flotation is large, making it difficult to achieve efficient recovery.
By combining a combination of activators (lead nitrate, manganese nitrate, and mercuric nitrate) with the inhibitor water glass, the surface activation entropy change of scheelite is increased. Combined with benzohydroxyxamic acid collector, efficient recovery by low-temperature flotation is achieved.
It significantly improved the recovery rate of scheelite, reduced the amount of reagents used, solved the problem of low reagent selectivity in traditional methods, and achieved a recovery rate of more than 70%.
Smart Images

Figure CN117160681B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a high-entropy activation flotation method for low-grade scheelite, belonging to the field of mineral processing technology. Background Technology
[0002] Tungsten is an important rare metal with high melting point, high density, high strength, high thermal conductivity, and corrosion resistance, playing a vital role in industries such as aerospace, military, electronics, energy, and chemicals. Due to its rarity and importance, the efficient recycling and utilization of this resource is of significant strategic importance.
[0003] Scheelite (CaWO4) is one of the most common tungsten-bearing minerals and a major tungsten resource. Major scheelite producing countries include China, Russia, the United States, Canada, and Australia. Although my country has abundant scheelite resources, it often occurs in close association with calcium-bearing gangue minerals such as fluorite (CaF2), calcite (CaCO3), and dolomite (CaMg(CO3)2), resulting in low tungsten grade and fine particle size, leading to low beneficiation recovery and significant tungsten resource loss. Both scheelite and calcium-bearing gangue minerals contain Ca atoms on their surfaces, resulting in poor adsorption selectivity of flotation reagents, ultimately leading to low flotation recovery and poor concentrate quality. Furthermore, a large amount of Ca is released during grinding and flotation. 2+ and Mg 2+ This results in problems such as high reagent consumption and difficulty in removing reagents from flotation concentrate.
[0004] Currently, the collectors commonly used in the flotation process of scheelite mainly include anionic collectors, cationic collectors, amphoteric collectors, and non-polar collectors. Among them, anionic collectors are the most widely used, mainly including fatty acid collectors, sulfonic acid collectors, phosphonic acid collectors, and chelating collectors.
[0005] Fatty acid collectors such as sodium oleate, talc oil, and oxidized paraffin soap can adsorb onto the surface of scheelite, causing the mineral to become hydrophobic and float. However, low-temperature conditions in the pulp significantly reduce the activity of these collectors, and they do not disperse well in the pulp. To maintain high beneficiation performance, the amount of collector used in industry is usually increased, which not only increases reagent costs but also creates difficulties for subsequent tailings treatment. Emulsification with oxidized paraffin soap can improve solubility and dispersion at low temperatures, maintaining good selectivity in the separation process and allowing scheelite flotation regardless of the season. However, oxidized paraffin soap has poor selectivity for most calcium-containing minerals, requiring the addition of inhibitors with strong selectivity for gangue minerals such as calcite during the flotation process to enhance its selectivity for scheelite.
[0006] Sulfonic acid and phosphonic acid collectors react with sulfonate and phosphonate ions on the surface of scheelite to form hydrophobic, insoluble salts. These hydrophobic substances adsorbed on the scheelite surface cause the scheelite to float. These two types of collectors exhibit excellent selectivity for scheelite; however, the beneficiation cost of using either of these collectors alone is too high. Furthermore, their collecting capacity is inferior to that of fatty acid collectors. Therefore, sulfonic acid and phosphonic acid collectors are generally used in combination with fatty acid collectors to reduce the amount of fatty acid collector required.
[0007] Chelating collectors, especially benzohydroxyxamic acid, have shown excellent selectivity and collecting performance in the flotation of scheelite, making its collection of scheelite a research hotspot. Benzohydroxyxamic acid forms a five-membered ring chelate by forming O-Ca-O bonds with the Ca atoms on the scheelite surface through the two oxygen atoms in its molecule. Simultaneously, the nonpolar groups of other benzohydroxyxamic acids are adsorbed onto the benzohydroxyxamic acid adsorption layer on the scheelite surface via hydrogen bonds, enabling a certain degree of separation between scheelite and calcium-containing gangue. However, benzohydroxyxamic acid is expensive, and when used alone as a collector, its bonding ability with calcium atoms is limited, and its hydrophobic groups are small, resulting in insufficient hydrophobicity of the mineral surface. A large dosage is needed to overcome this drawback. Therefore, in production practice, metal ions are added for activation. Lead nitrate has been the most successful activator for scheelite. Lead ions and their hydroxyl complexes adsorb onto the mineral surface, providing active sites for the adsorption of benzo[a]hydroxyxamic acid, thus increasing the floatability of scheelite. In production practices involving lead ion activation and benzo[a]hydroxyxamic acid collection of scheelite, aluminum-water glass complexes are often used to suppress gangue minerals such as calcite. Complexes formed by metal ions and inhibitors or collectors can increase the selectivity of the complexes. Therefore, the application of lead-benzo[a]hydroxyxamic acid complexes as collectors has been proposed, and high industrial test results have been achieved. However, this process still suffers from problems such as incomplete scheelite activation, incomplete gangue mineral suppression, high cost of benzo[a]hydroxyxamic acid, and reduced flotation recovery at low temperatures.
[0008] Based on the above, efficient flotation recovery of low-grade scheelite remains a typical bottleneck in tungsten resource development. This bottleneck is mainly manifested in low resource recovery rates and poor flotation separation effects, resulting in a significant portion of tungsten resources being unrecoverable. Therefore, fundamentally solving this problem requires developing new activators to activate this type of ore in order to achieve satisfactory flotation performance. Summary of the Invention
[0009] For low-grade tungsten ore, mainly composed of scheelite, this invention proposes a high-entropy activation flotation method for low-grade scheelite. This invention uses water glass as an inhibitor to suppress gangue minerals, then employs a combination of activators to increase the activation entropy change of the activators on the mineral surface, thereby improving the activation effect of scheelite. Finally, scheelite is collected using benzohydroxyxamic acid, achieving a high recovery rate and realizing the efficient recycling of tungsten ore resources.
[0010] The technical solution of this invention is as follows: A high-entropy activation flotation method for low-grade scheelite, the specific steps of which are as follows: (1) Mix lead nitrate, manganese nitrate and mercuric nitrate in a ratio of 1:3~9:0.03~0.08 to form scheelite composite activator A; (2) Grind the low-grade scheelite ore containing 0.30~0.35 wt.% WO3 until the degree of liberation of tungsten mineral monomers in the slurry is more than 80% to obtain a grinding slurry with a mass concentration of 25~30%. Add 400~600 g / t sodium carbonate to the grinding slurry and stir for 3~4 min. Then add 100~300 g / t water glass and stir for 3~4 min to obtain slurry I. (3) Add 800~1500 g / t of combined activator A to slurry I, stir and react for 3~4 min, add 100~200 g / t of ferrous sulfate, stir and react for 3~4 min to obtain slurry II; (4) Add 200-400 g / t of collector benzyl hydroxamic acid to pulp II, stir and react for 3-4 min, and then add 60-80 g / t of pine oil or No. 2 oil as a foaming agent to obtain pulp III; (5) The pulp III is subjected to flotation in a closed-circuit process of one roughing, one scavenging, three cleaning, and middlings returned in sequence, and finally scheelite concentrate and tailings are obtained.
[0011] Furthermore, the foaming agent is pine oil and No. 2 flotation oil (also known as No. 2 oil).
[0012] After the activator is adsorbed on the surface of scheelite, the surface activation entropy change is as follows:
[0013] Where: ΔS c The entropy change for surface activation of scheelite is given by: R is the gas constant; x iLet be the mole fraction of the i-th activator on the surface of scheelite, expressed as a decimal. For the scheelite surface before adsorption of a single activator, the surface composition is 1, i.e., i=1. At this point, the surface activation entropy change is zero, the mineral is not activated, and the flotation effect is poor. When using a high-entropy activator A for scheelite, the activator adsorbates four types of substances on the scheelite surface. Considering the original Ca active sites on the scheelite surface, the activator fully covers the mineral surface, i.e., i=5. By measuring the adsorption amount of each activator on the surface, x is calculated. i The value of ΔS can be used to calculate the surface activation entropy change ΔS. c Clearly, the surface activation entropy of scheelite increases significantly after activation with a combination of activators, which is beneficial for the adsorption of benzohydroxyxamic acid and thus improves the flotation recovery rate.
[0014] (1) The high-entropy activation of the present invention makes the entropy increase of the activation process reach a relatively large value, which makes the benzyl hydroxamic acid adsorbate on the surface of the activated scheelite more stable. Compared with the activation by using lead ions alone, the recovery rate of scheelite is significantly improved due to the significant increase in surface activation entropy. (2) The use of the combined activator of the present invention can significantly reduce the amount of inhibitor and collector. The addition of water glass will hinder the adsorption of activating components such as lead, manganese, mercury, and iron on the surface of gangue minerals. The gangue minerals are fully inhibited, which can overcome the problem of low reagent selectivity in traditional flotation methods; (3) The combination of activators in this invention does not require heating during the activation process, and the collector can be directly floated to obtain a recovery rate of more than 70%. Attached Figure Description
[0015] Figure 1 This is a flowchart illustrating the principles of the present invention. Implementation
[0016] Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be construed as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed in accordance with the techniques or conditions described in the literature in the field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased. Example
[0017] (1) Mix lead nitrate, manganese nitrate and mercuric nitrate in a ratio of 1:3:0.08 to form scheelite composite activator A; (2) Grind the low-grade scheelite containing 0.30 wt.% WO3 until the degree of liberation of tungsten mineral monomers in the slurry is more than 80% to obtain a grinding slurry with a mass concentration of 25%. Add 400 g / t sodium carbonate to the grinding slurry and stir for 3-4 min. Then add 300 g / t water glass and stir for 3-4 min to obtain slurry I. (3) Add 800 g / t of combined activator A to slurry I, stir and react for 3-4 min, add 100 g / t of ferrous sulfate, stir and react for 3-4 min to obtain slurry II; (4) Add 200 g / t of collector benzohydroxyxamic acid to pulp II, stir and react for 3-4 min, and then add 80 g / t of pine oil as a foaming agent to obtain pulp III; (5) The pulp III is subjected to flotation in a closed-circuit process of one roughing, one scavenging, three cleaning, and middlings returned in sequence, and finally scheelite concentrate and tailings are obtained.
[0018] The WO3 grade of the tungsten concentrate is 22.74%, and the WO3 recovery rate is 71.19%. Example
[0019] (1) Mix lead nitrate, manganese nitrate and mercuric nitrate in a ratio of 1:5:0.07 to form scheelite composite activator A; (2) Grind the low-grade scheelite containing 0.33 wt.% WO3 until the degree of liberation of tungsten mineral monomers in the slurry is more than 80% to obtain a grinding slurry with a mass concentration of 28%. Add 500 g / t sodium carbonate to the grinding slurry and stir for 3-4 min. Then add 200 g / t water glass and stir for 3-4 min to obtain slurry I. (3) Add 1000 g / t of combined activator A to slurry I, stir and react for 3-4 min, add 150 g / t of ferrous sulfate, stir and react for 3-4 min to obtain slurry II; (4) Add 300 g / t of collector benzohydroxyxamic acid to pulp II, stir and react for 3-4 min, and then add 70 g / t of pine oil as a foaming agent to obtain pulp III; (5) The pulp III is subjected to flotation in a closed-circuit process of one roughing, one scavenging, three cleaning, and middlings returned in sequence, and finally scheelite concentrate and tailings are obtained.
[0020] The tungsten concentrate has a WO3 grade of 23.86% and a WO3 recovery rate of 72.19%. Example
[0021] (1) Mix lead nitrate, manganese nitrate and mercuric nitrate in a ratio of 1:9:0.08 to form scheelite composite activator A; (2) Grind the low-grade scheelite containing 0.35 wt.% WO3 until the degree of liberation of tungsten mineral monomers in the slurry is more than 80% to obtain a grinding slurry with a mass concentration of 30%. Add 600 g / t sodium carbonate to the grinding slurry and stir for 3-4 min. Then add 300 g / t water glass and stir for 3-4 min to obtain slurry I. (3) Add 1500 g / t of combined activator A to slurry I, stir and react for 3-4 min, add 200 g / t of ferrous sulfate, stir and react for 3-4 min to obtain slurry II; (4) Add 400 g / t of collector benzyl hydroxamic acid to slurry II, stir and react for 3-4 min, and then add 80 g / t of No. 2 oil as a foaming agent to obtain slurry III; (5) The pulp III is subjected to flotation in a closed-circuit process of one roughing, one scavenging, three cleaning, and middlings returned in sequence, and finally scheelite concentrate and tailings are obtained.
[0022] In this embodiment, the WO3 grade of the tungsten concentrate is 24.83%, and the WO3 recovery rate is 72.63%.
[0023] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.
Claims
1. A high-entropy activation flotation method for low-grade scheelite, characterized in that... Follow these steps: (1) Mix lead nitrate, manganese nitrate and mercuric nitrate in a ratio of 1:3~9:0.03~0.08 to form scheelite composite activator A; (2) Grind the low-grade scheelite ore containing 0.30~0.35 wt.% WO3 until the degree of liberation of tungsten mineral monomers in the slurry is more than 80% to obtain a grinding slurry with a mass concentration of 25~30%. Add 400~600 g / t sodium carbonate to the grinding slurry and stir for 3~4 min. Then add 100~300 g / t water glass and stir for 3~4 min to obtain slurry I. (3) Add 800~1500 g / t of combined activator A to slurry I, stir and react for 3~4 min, add 100~200 g / t of ferrous sulfate, stir and react for 3~4 min to obtain slurry II; (4) Add 200-400 g / t of collector benzyl hydroxamic acid to pulp II, stir and react for 3-4 min, and then add 60-80 g / t of frother to obtain pulp III; (5) The pulp III is subjected to flotation in a closed-circuit process of one roughing, one scavenging, three cleaning, and middlings returned in sequence, and finally scheelite concentrate and tailings are obtained.
2. The high-entropy activation flotation method for low-grade scheelite according to claim 1, characterized in that, The foaming agent is pine oil.
Citation Information
Patent Citations
Beneficiation method for high-calcium scheelite
CN112705354A
Zinc oxide ore high-entropy activation flotation method
CN115318448A