A heterostructured material, its preparation method and application

By using a foam metal-supported cobalt tetroxide/cobalt iron phosphate heterostructure material, the problems of insufficient conductivity and easy poisoning of cobalt-based oxide catalysts in urea oxidation reaction have been solved, achieving high efficiency, stable catalytic performance and long-term use.

CN117187867BActive Publication Date: 2026-11-17SUZHOU UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311112891.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-31
Publication Date
2026-11-17
Estimated Expiration
2043-08-31

AI Technical Summary

Technical Problem

Existing cobalt-based oxide catalysts have insufficient conductivity and are easily poisoned in the urea oxidation reaction, resulting in unstable catalytic performance and difficulty in maintaining high efficiency in long-term electrocatalysis.

Method used

A cobalt tetroxide/cobalt iron phosphate heterostructure material supported by foam metal is prepared by a two-step hydrothermal method and phosphating method to form a cobalt tetroxide and cobalt iron phosphate heterostructure interface, which enhances conductivity and reduces the poisoning effect of intermediates.

Benefits of technology

It improves the conductivity and stability of the catalyst, enhances catalytic performance, lowers the reaction energy barrier, and extends the catalyst's lifespan, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117187867B_ABST
    Figure CN117187867B_ABST
Patent Text Reader

Abstract

This invention discloses a heterostructured material using a foamed metal as a carrier. A cobalt tetroxide / cobalt iron phosphate composite material with a heterogeneous interface structure is formed on the surface of the foamed metal. The cobalt tetroxide / cobalt iron phosphate composite material exhibits distinct cobalt tetroxide and cobalt iron phosphate lattice fringes and forms a corresponding heterogeneous interface. This heterostructured material possesses good catalytic performance and stability. This invention also provides a method for preparing the heterostructured material, which synthesizes the material through a two-step hydrothermal method and a phosphating method. The raw materials used are inexpensive, the required equipment is simple, and it is suitable for large-scale production, demonstrating economic feasibility. This invention further discloses an application of the above-mentioned heterostructured material in the field of electrocatalytic urea oxidation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new materials technology, specifically relating to a heterogeneous structure material, its preparation method and application. Background Technology

[0002] Hydrogen energy, as a highly efficient, pollution-free, and sustainable new energy source, is considered one of the most promising clean energy sources of the 21st century. It can help alleviate the energy crisis caused by the depletion of fossil fuels and the environmental crisis caused by the deteriorating ecological environment. With the advancement of the "dual-carbon" policy, market demand for hydrogen energy will experience explosive growth. Therefore, developing green and efficient hydrogen production methods is crucial. Among various hydrogen production methods, water electrolysis is considered the most promising technology because it is not only clean, environmentally friendly, and sustainable, but also can be coupled with renewable energy sources such as solar and wind power.

[0003] Traditional water electrolysis systems include the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. Compared to HER, which involves two electron transfers, OER is a complex process involving multi-electron-proton coupling, with relatively slow reaction kinetics. It requires additional energy to overcome the reaction energy barrier and accelerate the reaction, thus OER is one of the main factors contributing to the high energy consumption of water electrolysis. Currently, there are two strategies to reduce energy consumption: one is to continue developing highly efficient OER catalysts; the other is to actively seek alternative reactions, using the oxidation reactions of small organic molecules such as urea, 5-hydroxymethylfurfural, benzyl alcohol, and ethanol to replace OER. These small organic molecules are easier to oxidize, effectively saving energy and playing a role in wastewater treatment or the conversion of high-value-added chemicals. Therefore, the search for suitable alternative reactions has received widespread attention in recent years. Among them, the urea oxidation reaction (UOR) under alkaline conditions is a simple and effective alternative reaction. A urea electrolysis cell composed of UOR and HER can reduce the theoretical voltage from 1.23V vs. RHE in water decomposition to 0.37V vs. RHE, theoretically saving ~70% of energy. Furthermore, UOR is the core chemical reaction in direct urea fuel cells and urea-rich wastewater purification systems. Therefore, UOR can be used as an alternative reaction to OER in coupled water electrolysis systems to achieve the dual goals of energy-saving hydrogen production and urea-containing wastewater treatment.

[0004] Although the thermodynamic potential of undifferentiated oxygen (UOR) is relatively low (0.37 V vs. RHE), it remains a complex reaction involving six-electron transfer, requiring the design of highly active catalysts to accelerate the reaction rate. Currently, researchers have developed a large number of transition metal-based materials for UOR catalysis, attributed to their ability to generate peroxides in situ under oxidizing conditions, which can serve as catalytic active sites to enhance performance. Among these, research on cobalt-based materials as UOR catalysts is relatively limited, especially on cobalt-based oxides, possibly due to their semiconductor properties and the poisoning phenomenon during catalysis. Therefore, improving the conductivity of cobalt-based oxides is a key issue in the development of cobalt-based UOR catalysts; more importantly, improving the anti-poisoning performance of cobalt-based catalysts is an urgent problem to be solved to enhance the stability of cobalt-based materials in UOR reactions. Summary of the Invention

[0005] In view of all or part of the shortcomings of the prior art described above, the object of the present invention is:

[0006] One objective of this invention is to provide a heterostructure material, specifically a foam metal-supported cobalt tetroxide / iron cobalt phosphide heterostructure material, wherein the presence of iron cobalt phosphide can significantly improve the conductivity of cobalt tetroxide, and the strong electronic interaction between the cobalt tetroxide and iron cobalt phosphide heterostructure interface reduces the poisoning effect of the UOR reaction intermediate on the catalyst, so that the catalyst still maintains good catalytic performance in the long-term electrocatalytic urea oxidation reaction.

[0007] Another objective of this invention is to provide a method for preparing heterostructured materials. The method synthesizes the heterostructured materials through a two-step hydrothermal method and a phosphating method. The raw materials used are inexpensive, the required equipment is simple, it is suitable for large-scale production, and it has certain economic feasibility.

[0008] Another object of the present invention is to disclose the application of the above-mentioned heterostructure material in the field of electrocatalytic urea oxidation.

[0009] To achieve the above objectives, the present invention provides the following technical solution:

[0010] This invention provides a heterostructure material, wherein a foam metal is used as a carrier, and a cobalt tetroxide / cobalt iron phosphate composite material with a heterostructure interface is formed on the surface of the foam metal. The cobalt tetroxide / cobalt iron phosphate composite material has obvious cobalt tetroxide lattice stripes and cobalt iron phosphate lattice stripes, and forms a corresponding heterostructure interface.

[0011] The beneficial effects of this technical solution are as follows: First, the foamed metal, as the substrate of the heterostructure material, has a rich three-dimensional porous structure on its surface, which increases the overall specific surface area of ​​the catalyst and is conducive to mass transfer. More importantly, foamed metals, such as foamed nickel, have excellent electrical conductivity. In-situ growth of a composite material with a heterostructure interface on its surface, with the two tightly bonded, facilitates electron transfer between the substrate and the catalyst, i.e., the composite material. Second, the heterostructure material includes a cobalt tetroxide / cobalt iron phosphate heterostructure. Compared to simple cobalt tetroxide or cobalt iron phosphate catalysts, the electron transfer at the heterostructure interface of the cobalt tetroxide / cobalt iron phosphate heterostructure helps to regulate the electronic structure of the catalyst, thereby improving the conductivity of the cobalt-based oxide and enhancing the intrinsic catalytic activity of the catalyst, thus improving catalytic performance. Furthermore, the formation of the cobalt tetroxide / cobalt iron phosphate heterostructure interface can optimize the adsorption / desorption of reaction intermediates by cobalt-based materials in the urea oxidation reaction, reduce the catalyst poisoning problem caused by excessive adsorption of intermediates on the reactive sites, and thus enhance the long-term stability of UOR of the cobalt tetroxide / cobalt iron phosphate heterostructure material.

[0012] The foamed metal is selected from foamed nickel, foamed cobalt, foamed copper, or foamed aluminum. It should be noted that the heterostructure material described in this invention can be, for example, a cobalt tetroxide / iron-cobalt phosphide composite material supported on foamed nickel.

[0013] The microstructure of the cobalt tetroxide / cobalt iron phosphate composite material consists of nanocubes strung together on nanowires, exhibiting a composite morphology resembling a "candied hawthorn skewer." The nanowires are vertically aligned and formed on the foam metal surface, meaning they grow perpendicularly to the foam metal surface. Compared to catalysts with simple nanowire or nanocube morphologies, this unique composite morphology offers the following advantages: First, it facilitates a further increase in the electrochemical active area and the number of catalytic active sites; second, this unique structure provides an optimized pathway for the diffusion of electrons and electroactive substances, accelerating charge transfer, reducing electron transfer resistance, and effectively promoting mass transfer; most importantly, the electron transfer at the heterogeneous interface can regulate the electronic structure of the catalyst, optimize the adsorption / desorption of reactants and reaction intermediates at the catalytic active sites, lower the reaction energy barrier, and thus improve the intrinsic catalytic activity of the catalyst.

[0014] This invention also provides a method for preparing a heterostructured material, comprising the following steps:

[0015] S1: Add cobalt source and urea to water to dissolve and form a precursor solution;

[0016] S2: Using foamed metal as a carrier, a hydrothermal reaction is carried out with the precursor solution to obtain the first intermediate;

[0017] S3: The first intermediate undergoes a secondary hydrothermal reaction with potassium ferricyanide solution at a temperature above 30°C for 10-14 hours to obtain the second intermediate;

[0018] S4: Phosphate the second intermediate to obtain the heterostructure material.

[0019] The beneficial effect of this technical solution lies in the fact that it combines a two-step hydrothermal method with a phosphating method to prepare heterostructure materials. If the precursor solution and potassium ferricyanide solution are reacted simultaneously with the foam metal in a single hydrothermal step, the heterostructure material of this invention cannot be obtained. When the first intermediate undergoes a secondary hydrothermal reaction with the potassium ferricyanide solution, the reaction time should be controlled within 10-16 hours, preferably 10-14 hours, and the reaction temperature should be controlled above 30°C to hope to obtain a cobalt tetroxide / cobalt iron phosphate heterostructure. If the reaction time is too short, only a small amount of phosphide will be produced, failing to form a heterostructure and resulting in only a simple nanowire morphology. If the reaction time is too long, the nanowires will be etched away, preventing the formation of a heterostructure and the maintenance of the composite array structure, resulting in only a simple nanocube morphology with a disordered arrangement. If the secondary hydrothermal reaction temperature is below 30°C, for example, at room temperature, only a small amount of phosphide will be produced, failing to form a heterostructure. Therefore, the reaction time and temperature of the secondary hydrothermal reaction are crucial. The heterostructured material has a unique morphology and excellent UOR performance, and the method is low in cost and suitable for large-scale industrial production; the preparation method can be used to synthesize the above-mentioned foam metal-supported cobalt tetroxide / iron cobalt phosphide heterostructured material.

[0020] In step S4, the phosphating process includes: placing an excess phosphorus source and a second intermediate in separate ceramic boats, placing them together in a tube furnace, with the phosphorus source positioned upstream of the gas flow, raising the temperature to 250-450°C, and finally allowing it to cool naturally to room temperature. The phosphorus source may, but is not limited to, sodium hypophosphite monohydrate. The phosphating temperature is further preferably 350°C. If the phosphating temperature is too low, the phosphorus source cannot fully decompose and release phosphine gas (the actual active phosphating agent), thus failing to achieve sufficient phosphating. If the phosphating temperature is too high, the substrate, i.e., the carrier, such as nickel foam, cannot withstand the excessively high temperature.

[0021] In S1, the cobalt source can be cobalt chloride hexahydrate or cobalt nitrate hexahydrate, etc., and the molar ratio of the cobalt source to urea is 1:2-8, and can be further selected as 1:5. The concentrations of the cobalt source and urea are generally high to ensure the formation of sufficient first intermediate (cobalt-based nanowires).

[0022] In S2, the hydrothermal reaction temperature is 40-100℃, and the reaction time is 6-18h. Further, in S2, the preferred hydrothermal reaction temperature is 80℃, and the reaction time is 12h. The hydrothermal reaction temperature affects the morphology of the heterostructure; a temperature of 80℃ is beneficial for the subsequent formation of a special composite morphology of nanocubes strung on nanowires.

[0023] In S3, the reaction temperature of the secondary hydrothermal reaction is 40-100℃, and the reaction time is 12-14h. Further, the reaction temperature of the secondary hydrothermal reaction is 60℃, and the reaction time is 12h. The beneficial effect of this technical solution is that the foam metal-supported cobalt tetroxide / cobalt iron phosphate composite material synthesized at this reaction temperature and time has a suitable composite array structure of nanocubes and nanowires, and the nanowires are not completely etched away, exhibiting good nanomorphology, thus ensuring its excellent catalytic performance; moreover, the obtained foam metal-supported cobalt tetroxide / cobalt iron phosphate composite material has stable performance and can exert its catalytic effect for a long time.

[0024] In step S2, the product of the hydrothermal reaction is washed and dried to obtain the first intermediate; in step S3, the product of the second hydrothermal reaction is washed and dried to obtain the second intermediate; the drying method in S2 and S3 is to dry in a drying oven at 50-100℃ for 10-15 hours. Under these drying temperature and time conditions, most of the moisture in the product obtained after the two-step hydrothermal reaction can be effectively removed without causing significant surface oxidation, thus avoiding affecting the subsequent high-temperature phosphating process. A vacuum drying oven is preferred to further prevent oxidation.

[0025] Before step S2, the foamed metal can be pre-cleaned. Cleaning methods for foamed metals, such as nickel foam, include immersing and / or ultrasonically cleaning the nickel foam with an organic solvent and / or a low-concentration acid. The organic solvent can be acetone, and the acid can be 0.1-3 mol / L hydrochloric acid. Acetone has both fat and water solubility, effectively removing oil stains from the surface of the nickel foam. Hydrochloric acid within this concentration range can remove oxides from the surface of the nickel foam. Pre-treating the nickel foam allows the composite material to be more uniformly loaded onto the surface of the nickel foam, preventing the collapse or detachment of the active material. Alternatively, other reagents can be used for pre-treatment, such as ethanol or dilute sulfuric acid. The cleaning step can further include rinsing off residual reagents with water and drying the nickel foam. Drying methods can include natural air drying at room temperature or oven drying. A vacuum oven is preferred to prevent oxidation of the nickel foam during drying. The specific cleaning method can be as follows: use ethanol, acetone, and 0.1-3 mol / L hydrochloric acid for ultrasonic cleaning for 15-30 minutes in sequence, and finally use water for ultrasonic cleaning for 20-30 minutes, changing the water 6-8 times in between.

[0026] This invention also discloses an application of the heterostructure material in the above-mentioned technical solution in the field of electrocatalytic urea oxidation. Specifically, it can be used as a catalyst in the electrocatalytic urea oxidation reaction under alkaline conditions, with the heterostructure material serving as the anode of an electrolytic cell to catalyze the urea oxidation reaction under alkaline conditions. The formation of the cobalt tetroxide / cobalt iron phosphate heterostructure interface in the heterostructure material can effectively optimize the catalytic performance of the catalyst.

[0027] Specifically, the heterostructure material is used as an anode electrode to catalyze the electro-oxidation reaction of alkaline urea. The material uses foamed metal as a supporting substrate, so it can be used directly as an electrode without the need to add a binder (such as Nafion) during the electrode preparation process. This simplifies the electrode preparation process and avoids the reduction in electron transfer rate during the reaction process caused by the binder, as well as the drastic change in catalytic effect that may be caused by the detachment of the binder during long-term reaction. Therefore, using this heterostructure material directly as an electrode is beneficial to the simultaneous improvement of conductivity and stability.

[0028] Compared with the prior art, the present invention has at least the following beneficial effects:

[0029] (1) The microstructure of the heterostructure provided by the present invention can be expressed as a composite morphology of nanocubes strung on nanowires. The nanowires are grown vertically on the surface of the foam metal, which is beneficial to increase the electrochemical active area, promote mass transfer, accelerate charge transfer, and improve the catalytic activity of the catalyst.

[0030] (2) In the heterostructure material, cobalt tetroxide / cobalt iron phosphate forms a large number of heterostructure interfaces. The strong electronic interaction between the two substances regulates the electronic structure of the catalyst, optimizes the adsorption / desorption of reaction intermediates on the catalyst surface, and reduces the catalyst poisoning problem caused by the difficulty of desorption of intermediate products, thereby enhancing catalytic stability.

[0031] (3) The method used in this invention to prepare cobalt tetroxide / cobalt iron phosphate heterostructure material is a two-step hydrothermal method and high-temperature phosphating. The preparation method is simple and easy to implement. The required equipment and raw materials are abundant and inexpensive, and easy to obtain. In industrial production, it is easy to control costs and suitable for large-scale production.

[0032] (4) This invention discloses the application of the heterostructure material prepared above in the catalytic electro-oxidation reaction of urea under alkaline conditions. The cobalt tetroxide / cobalt iron phosphate heterostructure composite material has good catalytic performance and is suitable as a catalyst for the electro-oxidation reaction of urea under alkaline conditions. Moreover, the cobalt tetroxide / cobalt iron phosphate composite material supported by foam metal has stable performance and its catalytic performance has not decreased significantly during the long reaction process, which meets the requirements for catalyst stability in industrial production. Attached Figure Description

[0033] To more clearly illustrate the technical solutions in the specific embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0034] Figure 1 This is a flowchart of the method for preparing heterostructured materials provided by the present invention;

[0035] Figure 2 The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 SEM and TEM images of P@NF; where a is Co3O4 / Fe 0.3 Co 0.7 SEM image of P@NF at a 1 μm scale; b is Co3O4 / Fe 0.3 Co 0.7 TEM image of P@NF at a scale of 100 nm;

[0036] Figure 3 The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 HRTEM and Mapping plots of P@NF; where a is Co3O4 / Fe 0.3 Co 0.7HRTEM image of P@NF at a 5 nm scale; b is Co3O4 / Fe 0.3 Co 0.7 P@NF elemental distribution mapping at a 500nm scale;

[0037] Figure 4 The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 XRD pattern of P@NF;

[0038] Figure 5 The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 P@NF, and Co3O4@NF prepared in Comparative Example 6 and Fe prepared in Comparative Example 4 0.3 Co 0.7 XPS plot of P@NF; where a is Co3O4 / Fe 0.3 Co 0.7 XPS narrow scan comparison of Co 2p in P@NF and Co3O4@NF; b is Co3O4 / Fe 0.3 Co 0.7 P@NF and Fe 0.3 Co 0.7 XPS narrow scan comparison of Fe 2p in P@NF; c is XPS narrow scan comparison of P 2p; d is XPS narrow scan comparison of O1s;

[0039] Figure 6 This is a SEM image of the product prepared in Comparative Example 1;

[0040] Figure 7 This is an SEM image of the product prepared in Example 2;

[0041] Figure 8 This is an SEM image of the product prepared in Example 3;

[0042] Figure 9 This is a SEM image of the product prepared in Comparative Example 2;

[0043] Figure 10 This is a SEM image of the product prepared in Comparative Example 3.

[0044] Figure 11 This is a SEM image of the product prepared in Comparative Example 4.

[0045] Figure 12 The Co3O4@NF prepared in Comparative Example 6 and the Fe prepared in Comparative Example 4 0.3 Co 0.7XRD contrast diagrams of P@NF; where a is the XRD pattern of Co3O4@NF; b is the XRD pattern of Fe. 0.3 Co 0.7 XRD pattern of P@NF;

[0046] Figure 13 The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 P@NF, Co3O4@NF prepared in Comparative Example 6 and Fe prepared in Comparative Example 4 0.3 Co 0.7 Polarization curve of P@NF measured in 1M KOH + 0.33M urea electrolyte at a scan rate of 5mV / s. Figure 13 a) in the middle; Figure 13 In this context, b represents the Co3O4 / Fe prepared in Example 1. 0.3 Co 0.7 Comparison of polarization curves of P@NF for catalytic UOR and OER;

[0047] Figure 14 The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 Current-time curve of P@NF at 1.36V vs. RHE. Detailed Implementation

[0048] The technical solutions in specific embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. The steps in the following embodiments do not correspond one-to-one with the invention content section.

[0049] Example 1

[0050] This embodiment provides a heterostructure material and its preparation method (the preparation method can be referred to...). Figure 1 The method for preparing the heterostructure material, namely nickel foam-supported cobalt tetroxide / cobalt iron phosphate, in this embodiment is as follows:

[0051] (1) First, use ethanol and acetone to ultrasonically clean the foam nickel sheet of a specific shape and size for 15 minutes to remove organic matter and other impurities on its surface. Then, use 3 mol / L hydrochloric acid solution to ultrasonically clean for 15 minutes to remove metal oxides and other impurities on its surface. Finally, use a large amount of secondary water to ultrasonically clean for 20 minutes, changing the water 6-8 times in between, and rinsing until the cleaning liquid is neutral to ensure a completely clean nickel surface.

[0052] (2) Primary hydrothermal reaction: 0.285 g of CoCl2·6H2O (cobalt chloride hexahydrate) and 0.36 g of urea (molar ratio 1:5) were dissolved in 15 ml of deionized water to form a precursor solution. The precursor solution was transferred to a reaction vessel, and pretreated nickel foam (using nickel foam as a carrier) was added for hydrothermal reaction. The hydrothermal reaction temperature was 80 °C and maintained for 12 h. After naturally cooling to room temperature, the mixture was washed with water and dried in a vacuum drying oven at 75 °C for 10 h to obtain the first intermediate, which was then used for later use. The concentrations of cobalt source and urea are generally relatively high to ensure the formation of sufficient first intermediate (cobalt-based nanowires).

[0053] (3) Secondary hydrothermal reaction: Weigh 0.12g of potassium ferricyanide and dissolve it in 15ml of water to form a homogeneous solution. Then transfer the solution to the reaction vessel. Place the first intermediate obtained in (2) into the reaction vessel for secondary hydrothermal reaction. The temperature of the secondary hydrothermal reaction is 60℃ and maintained for 12h. After naturally cooling to room temperature, wash with water and dry in a vacuum drying oven at 75℃ for 10h to obtain the second intermediate for later use.

[0054] (4) Phosphating treatment: The second intermediate obtained in (3) and 1g of Na2HPO2·H2O (1g, to ensure sufficient phosphating) are placed in different ceramic boats and placed together in a tube furnace, wherein Na2HPO2·H2O is placed upstream of the gas, the temperature is raised to 350℃ at a heating rate of 5℃ / min and held for 5h, and finally naturally cooled to room temperature to obtain the heterostructure material.

[0055] The product obtained in this embodiment is Co3O4 / Fe 0.3 Co 0.7 P@NF heterostructure material refers to a cobalt tetroxide / cobalt iron phosphate composite material with a heterostructure formed on the surface of nickel foam using nickel foam as a carrier. In this embodiment, it is specifically Co3O4 / Fe 0.3 Co 0.7 P composite material, namely Co3O4 / Fe 0.3 Co 0.7 The P composite material exhibits distinct Co3O4 lattice fringes and Fe... 0.3 Co 0.7 P-lattice fringes form corresponding heterojunctions. The Co3O4 / Fe 0.3 Co 0.7 The microstructure of the P composite material consists of nanocubes strung together on nanowires, with the nanowires arranged vertically on the surface of the nickel foam.

[0056] Example 2

[0057] The only difference between Example 2 and Example 1 is that the hydrothermal reaction (corresponding to the hydrothermal reaction in S2) was carried out at 60°C for 12 hours. The resulting product was a composite material with an irregular morphology.

[0058] Example 3

[0059] The only difference between Example 3 and Example 1 is that the hydrothermal reaction (corresponding to the hydrothermal reaction in S2) was carried out at 100°C for 12 hours. The resulting product was a composite material with an irregular morphology.

[0060] Example 4

[0061] The only difference between Example 4 and Example 1 is that the secondary hydrothermal reaction (corresponding to the secondary hydrothermal reaction in S3) is carried out at 90°C for 12 hours. The resulting product is a composite material with an irregular morphology.

[0062] Comparative Example 1

[0063] The only difference between Comparative Example 1 and Example 1 is that no nickel foam is added in any of the steps, and the resulting product is a composite material without substrate load.

[0064] Comparative Example 2

[0065] The only difference between Comparative Example 2 and Example 1 is that the secondary hydrothermal reaction (corresponding to the secondary hydrothermal reaction in S3) was carried out at 60°C for 6 hours. The resulting product was a composite material containing a small amount of phosphide.

[0066] Comparative Example 3

[0067] The only difference between Comparative Example 3 and Example 1 is that the secondary hydrothermal reaction (corresponding to the secondary hydrothermal reaction in S3) was carried out at 60°C for 9 hours. The resulting product was a composite material containing a small amount of phosphide.

[0068] Comparative Example 4

[0069] The only difference between Comparative Example 4 and Example 1 is that the secondary hydrothermal reaction (corresponding to the secondary hydrothermal reaction in S3) was carried out at 60°C for 18 hours. The resulting product was a fully phosphated material. namely Fe 0.3 Co 0.7 P@ NF That is, nickel foam supported iron-cobalt phosphate.

[0070] Comparative Example 5

[0071] The only difference between Comparative Example 5 and Example 1 is that the secondary hydrothermal reaction (corresponding to the secondary hydrothermal reaction in S3) was carried out at room temperature for 12 hours. The resulting product was a composite material containing a small amount of phosphide.

[0072] Comparative Example 6

[0073] The difference between Comparative Example 6 and Example 1 is that the first intermediate was calcined in air at a heating rate of 3°C / min and maintained at 350°C for 2 hours, and then naturally cooled to room temperature to obtain Co3O4@NF, i.e., cobalt tetroxide supported on nickel foam.

[0074] The main preparation conditions involved in Examples 1-4 and Comparative Examples 1-6 are summarized in Table 1 below:

[0075] Table 1 Summary of relevant preparation conditions in the examples and comparative examples

[0076]

[0077]

[0078] I. Co3O4 / Fe 0.3 Co 0.7 Characterization of P@NF

[0079] The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 P@NF was used as the test sample and characterized using scanning electron microscopy (SEM), transmission electron microscopy (TEM), high-resolution transmission electron microscopy (HRTEM), elemental mapping, X-ray diffraction (XRD), and X-ray photoelectron spectroscopy (XPS). Co3O4@NF prepared in Comparative Example 6 and Fe synthesized in Comparative Example 4 were compared. 0.3 Co 0.7 P@NF was used as a control sample, and XPS was used to analyze Co3O4@NF and Fe. 0.3 Co 0.7 The electron binding energies of the elements contained in P@NF were compared and tested.

[0080] The characterization results are described and analyzed in detail below with reference to the attached figures:

[0081] Figure 2 a and Figure 2 In the figures, b represents the Co3O4 / Fe prepared in Example 1. 0.3 Co 0.7 SEM and TEM images of P@NF, such as Figure 2As shown in a, a large number of nanocubes were grown on nickel foam substrate using a two-step hydrothermal method combined with a high-temperature phosphating method, forming a morphology of regularly stacked nanorods; further characterization was performed using TEM. Figure 2 b) revealed that these nanocubes are interconnected internally by a nanowire, forming a unique "candied hawthorn"-like structure. This structure further increases the Co3O4 / Fe ratio. 0.3 Co 0.7 The P@NF nanorods offer a larger electrochemical active surface area, exposing more active sites and enhancing the intrinsic activity of the catalyst. Furthermore, the abundant porous structure formed between the nanorods facilitates the transport of reactants, providing ample reactants for the catalytic reaction and promoting its progress.

[0082] Figure 3 a and Figure 3 In the figures, b represents the Co3O4 / Fe obtained in Example 1. 0.3 Co 0.7 HRTEM diagram and element mapping diagram of P@NF. From Figure 3 In the 'a' column, we can see that they belong to Co3O4 and Fe respectively. 0.3 Co 0.7 The clear lattice fringes of P, in which Corresponding to the (331) crystal plane of cubic Co3O4 (the dashed box in the upper left corner is a magnified view), and Corresponding to the orthorhombic Fe 0.3 Co 0.7 The (011) crystal plane of P (the dashed box in the upper right corner is a magnified view), and Co3O4 (331) and Fe are shown in the figure. 0.3 Co 0.7 The two lattice fringes of P(011) have significantly different orientations, proving the formation of a heterogeneous interface. Figure 3 (The dashed curve in the middle of 'a'). Figure 3 b in the text is Co3O4 / Fe 0.3 Co 0.7 The elemental distribution mapping diagram of P@NF shows that the four elements Co, Fe, O and P are evenly distributed throughout the nanorod, further confirming the elemental composition of the catalyst. Figure 4 It is Co3O4 / Fe 0.3 Co 0.7 The XRD pattern of P@NF, compared with the standard XRD pattern, shows that the test sample simultaneously exhibits Co3O4 (JCPDS: 42-1467) and Fe. 0.3 Co 0.7 The characteristic diffraction peaks of P (JCPDS: 29-0497) indicate that Co3O4 / Fe 0.3 Co 0.7Formation of P@NF heterostructure material.

[0083] To further illustrate the electronic structure of Co3O4 / Fe 0.3 Co 0.7 P@NF heterostructure material, using Co3O4@NF prepared in Comparative Example 6 and Fe 0.3 Co 0.7 P@NF synthesized in Comparative Example 4 as control samples, the XPS spectra of Co3O4 / Fe 0.3 Co 0.7 P@NF, Co3O4@NF and Fe 0.3 Co 0.7 P@NF were comparatively analyzed. From Figure 5 a in the figure, it can be seen that both Co3O4 / Fe 0.3 Co 0.7 P@NF and Co3O4@NF exhibit characteristic peaks of Co 2p, wherein the two peaks located at about 783 eV and 798 eV are respectively attributed to the Co 2p3 / 2 and Co 2p1 / 2 orbitals. Compared with Co3O4@NF, the electron binding energy of the Co 2p3 / 2 orbital in Co3O4 / Fe 0.3 Co 0.7 P@NF shifts positively by 0.5 eV. While in b of Figure 5 , Co3O4 / Fe 0.3 Co 0.7 P@NF and Fe 0.3 Co 0.7 P@NF both exhibit characteristic peaks of Fe 2p, and the two peaks located near 713 eV and 724 eV correspond to the Fe 2p3 / 2 and Fe 2p1 / 2 orbitals respectively. Compared with Fe 0.3 Co 0.7 P@NF, the electron binding energy of the Fe 2p3 / 2 orbital in Co3O4 / Fe 0.3 Co 0.7 P@NF shifts negatively by 0.4 eV. Combining the above positive shift of the electron binding energy of Co, it can be known that there is a strong electronic interaction between Co3O4 and Fe 0.3 Co 0.7 P in the heterostructure. This electron transfer can adjust the electronic structure of the heterostructure material, regulate the adsorption / desorption of the heterostructure material on reaction intermediates, thereby enhancing its catalytic performance. Figure 5 c and d in the figure are the narrow scan spectra of P 2p and O 1s of Example 1 respectively, which indicate the existence of the two elements P and O and their respective existing states.

[0084] 2. Study on Influencing Factors of Heterostructure Formation and Morphology

[0085] (1) Influence of support (substrate): Figure 6 The image shows a SEM image of the product prepared in Comparative Example 1, as follows. Figure 6 As shown, without a substrate, the resulting product has a heterogeneous structure, but it is an irregularly shaped composite material, meaning it does not form the unique morphology of nanocubes strung together on nanowires. The presence or absence of a substrate, such as nickel foam, will affect the product morphology.

[0086] (2) The effect of primary hydrothermal temperature: Figure 7 This is an SEM image of the product prepared in Example 2. Figure 8 This is a SEM image of the product prepared in Example 3. Figure 7 and Figure 8 As shown, when the primary hydrothermal temperature is low or high, the resulting product has a heterogeneous structure but is an irregularly shaped composite material, meaning it does not form the special morphology of nanocubes strung together on nanowires. In other words, when the primary hydrothermal temperature is unsuitable, it is impossible to obtain a composite material with a regular morphology and a composite matrix arrangement. The primary hydrothermal temperature has a significant impact on the morphology of the product.

[0087] (3) The effect of secondary hydrothermal time: Figure 9 The image shows the SEM image of the product prepared in Comparative Example 2. Figure 10 This is a SEM image of the product prepared in Comparative Example 3. Figure 11 This is a SEM image of the product obtained in Comparative Example 4. The duration of the secondary hydrothermal treatment directly affects the product. If the secondary hydrothermal treatment time is too short, such as 6 hours in Comparative Example 2 and 9 hours in Comparative Example 3, insufficient secondary hydrothermal treatment time will result in an inability to obtain a heterostructure, i.e., only a small amount of phosphide, failing to form a complete heterostructure. Furthermore, the phosphide content is too low, making it undetectable by XRD characterization. Figure 9 It can be seen that no nanocube structure was formed. Figure 10 No obvious morphology of nanocubes strung together on nanowires was formed. If the secondary hydrothermal time is too long, such as 18 hours in Comparative Example 4, a heterostructure cannot be obtained, and the product is a fully phosphated material, i.e., Fe. 0.3 Co 0.7 P@NF. From Figure 11 It can be seen that no obvious nanowire structure has been formed, and the arrangement is irregular. For example... Figure 9-11 As shown, by adjusting the time of secondary hydrothermal etching (6h, 9h and 18h), i.e. Comparative Examples 2, 3 and 4, products with insufficient secondary etching and over-etching were obtained, which were products containing a small amount of phosphide and products with complete phosphating, respectively. Neither of them could produce a heterostructure. Through experiments, it can be seen that a secondary hydrothermal time of 10-14h, especially 12-14h, is conducive to the formation of heterostructure.

[0088] (4) Effect of secondary hydrothermal temperature: The temperature of secondary hydrothermal treatment also has a certain impact on the product. At room temperature, secondary hydrothermal treatment cannot form a heterogeneous structure. In Example 4, the secondary hydrothermal temperature reached 90℃. Although a heterogeneous structure could be obtained, the morphology was irregular and the special "candied hawthorn" structure was not formed. Through experiments, it can be seen that secondary hydrothermal temperature above 30℃, especially above 40℃, is expected to form a heterogeneous structure. At the same time, secondary hydrothermal treatment needs to be carried out below 80℃ to obtain the complex morphology of the special "candied hawthorn" structure.

[0089] The impact of subsequent high-temperature treatment: Figure 12 In this context, 'a' represents the absence of a secondary hydrothermal reaction and the replacement of the phosphating step with subsequent high-temperature oxidation (i.e., Comparative Example 6), resulting in a single-component Co3O4@NF (JCPDS: 42-1467). Additionally, by extending the secondary hydrothermal reaction time to 18 hours (i.e., Comparative Example 4), while maintaining the same remaining steps as in Example 1, we obtained a single-component Fe. 0.3 Co 0.7 P@NF( Figure 12 (See b in JCPDS: 29-0497), indicating that secondary hydrothermal treatment is actually an etching process. When the reaction time is long enough, the nanowire template can be completely etched, resulting in a single phosphide after subsequent phosphating. If the nanowires are completely etched, a unique composite morphology cannot be formed, resulting in a simple nanocube morphology. Therefore, without a heterogeneous interface, conductivity and catalytic performance cannot be improved. More importantly, the lack of a heterogeneous interface prevents the resolution of catalyst poisoning, leading to instability. Even with a heterogeneous interface, without the composite morphology of nanocubes strung on nanowires, optimized electron and electroactive material diffusion pathways cannot be obtained, hindering charge transfer and reducing electron transfer resistance. These experiments demonstrate the importance of controlling reaction time and temperature for the product composition, morphology, and structure. Optimizing reaction time and temperature helps in the formation of heterostructured materials.

[0090] III. Co3O4 / Fe 0.3 Co 0.7 Application of P@NF as a urea oxidation electrode

[0091] The Co3O4 / Fe prepared in Example 1 0.3 Co 0.7 P@NF was used as the test sample, along with Co3O4@NF prepared in Comparative Example 6 and Fe synthesized in Comparative Example 4. 0.3 Co 0.7 P@NF was used as a control sample to test the catalytic performance of the three as urea electro-oxidation electrodes under alkaline conditions.

[0092] Figure 13 In this context, 'a' represents Co3O4 / Fe.0.3 Co 0.7 P@NF, Co3O4@NF and Fe 0.3 Co 0.7 Polarization curves of P@NF measured in 1M KOH + 0.33M urea solution at a scan rate of 5 mV / s. Compared to Co3O4@NF and Fe... 0.3 Co 0.7 P@NF, Co3O4 / Fe 0.3 Co 0.7 P@NF exhibits a lower onset potential and a higher current density under the same conditions, indicating that Co3O4 / Fe 0.3 Co 0.7 P@NF exhibits superior UOR catalytic activity. As can be seen from the above comparison results, Co3O4 / Fe 0.3 Co 0.7 The formation of heterogeneous interfaces between P atoms enhances its UOR performance. This invention further tests and compares Co3O4 / Fe... 0.3 Co 0.7 The UOR and OER performance of P@NF, such as Figure 13 As shown in b, at the same current density, the potential required to catalyze UOR is much lower than that for OER, indicating that the present invention can achieve energy saving.

[0093] Figure 14 Co3O4 / Fe 0.3 Co 0.7 Current-time curve of P@NF at 1.36V vs. RHE. From Figure 14 As can be seen from this, under constant voltage, Co3O4 / Fe 0.3 Co 0.7 The current of P@NF did not decrease significantly after a long period of continuous electrolysis, indicating that the Co3O4 / Fe 0.3 Co 0.7 P@NF exhibits good durability and stability. This stability stems partly from the Co3O4 / Fe ratio. 0.3 Co 0.7 The stability of P@NF itself, and on the other hand, the Co3O4 / Fe 0.3 Co 0.7 P@NF as the working electrode eliminates the need for additional binders, thus avoiding instability caused by binder detachment during long-term testing. Therefore, Co3O4 / Fe 0.3 Co 0.7 P@NF can be used as a urea oxidation electrode under alkaline conditions for a long time, which meets the industrial requirements for catalyst stability.

[0094] The above description of the embodiments is only for the purpose of helping to understand the method and core idea of ​​the present invention. It should be noted that those skilled in the art can make several improvements and modifications to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a heterogeneous structure material, characterized in that, Includes the following steps: S1: Add cobalt source and urea to water to dissolve and form a precursor solution; S2: Using foamed metal as a carrier, a hydrothermal reaction is carried out with the precursor solution. The reaction temperature of the hydrothermal reaction is 40-100℃. The product of the hydrothermal reaction is washed and dried. The drying method is to dry it in a drying oven at 50-100℃ to obtain the first intermediate. S3: The first intermediate undergoes a secondary hydrothermal reaction with potassium ferricyanide solution. The reaction temperature of the secondary hydrothermal reaction is 40-100℃, and the reaction time is 10-14h. The product of the secondary hydrothermal reaction is washed and dried. The drying method is to dry it in a drying oven at 50-100℃ to obtain the second intermediate. S4: The second intermediate is subjected to phosphating treatment, which includes: placing an excess phosphorus source and the second intermediate in different ceramic boats, placing them together in a tube furnace, placing the phosphorus source upstream of the gas, raising the temperature to 250-450°C, and finally naturally cooling to room temperature to obtain the heterostructure material.

2. The preparation method according to claim 1, characterized in that, In S1, the cobalt source is cobalt chloride hexahydrate or cobalt nitrate hexahydrate, and the molar ratio of the cobalt source to urea is 1:2-8; in S2, the reaction time of the hydrothermal reaction is 6-18 hours.

3. The preparation method according to claim 1, characterized in that, In S3, the reaction time of the secondary hydrothermal reaction is 12-14 hours.

4. The preparation method according to claim 1, characterized in that, In S2 and S3, the drying time is 10-5 hours.

5. A heterogeneous structural material, characterized in that, The heterostructure material is prepared according to any one of claims 1-4, wherein the heterostructure material uses foam metal as a carrier, and a cobalt tetroxide / iron cobalt phosphide composite material with a heterostructure interface is formed on the surface of the foam metal. The cobalt tetroxide / iron cobalt phosphide composite material has obvious cobalt tetroxide lattice stripes and iron cobalt phosphide lattice stripes, and forms a corresponding heterostructure interface.

6. The heterogeneous structure material according to claim 5, characterized in that, The foam metal is selected from foamed nickel, foamed cobalt, foamed copper, or foamed aluminum.

7. The heterogeneous structure material according to claim 5, characterized in that, The microstructure of the cobalt tetroxide / cobalt iron phosphate composite material consists of nanocubes strung together on nanowires, with the nanowires arranged vertically on the surface of the foam metal.

8. The application of the heterostructure material according to any one of claims 5-7, or the heterostructure material prepared by the preparation method according to any one of claims 1-4, in the field of electrocatalytic urea oxidation.

9. The application according to claim 8, characterized in that, The heterostructured material serves as the anode of the electrolytic cell to catalyze the urea oxidation reaction under alkaline conditions.