Aluminum-manganese-nickel co-doped cobalt carbonate precursor as well as preparation method and application thereof
By co-precipitation method, the use of complexing agent and surfactant in the co-doped aluminum-manganese nickel co-doped trioxide precursor, the uniform dispersion of aluminum-manganese nickel elements was achieved, and the low tap density of aluminum-doped trioxide in the prior art was solved and the The problem of poor particle size uniformity significantly improves the performance and production feasibility of lithium-ion batteries.
Patent Information
- Application Number
- CN202410990014.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
In the prior art, aluminum-doped cobalt tetroxide has low tap density and poor particle size uniformity, which affects its electrochemical performance, making it difficult to achieve uniform doping of aluminum-manganese nickel elements in cobalt carbonate precursors, resulting in limited application of cobalt tetroxide.
By co-precipitation method of co-precipitation of cobalt-aluminum mixed salt solution, manganese salt solution and nickel salt solution, the complexing agent is added to the aluminum salt and the surfactant is added to the manganese salt to ensure uniform dispersion of aluminum-manganese nickel elements and avoid segregation. Control the particle size and dispersion to achieve uniform particle size and uniform distribution of doped elements of the tricobalt tetroxide precursor.
It significantly improves the particle size uniformity and uniformity of doping elements of the tri-cobalt oxide precursor, improves the recycling performance of lithium cobalt oxide in high-voltage environments, and improves the capacity of lithium-ion batteries. The preparation method is simple and can be used for large-scale industrialization. Production.
Smart Images

Figure BDA0004958600250000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries and relates to an aluminum-manganese-nickel co-doped cobalt carbonate precursor and a preparation method and application thereof. Background Art
[0002] As a way to adapt to the development of electrochemical energy storage equipment and meet the increasing demand for sustainable energy, lithium-ion batteries have attracted great attention due to their low cost, high operating voltage, large battery release volume, and recyclability. Cobalt tetroxide products are mainly used in the preparation of lithium cobalt oxide, the positive electrode material of lithium-ion batteries. With the increasing demand for lithium-ion secondary batteries, the market demand for cobalt tetroxide powder is also increasing exponentially. At the same time, with the continuous development of the functions of 3C products, high-voltage lithium-ion batteries are favored by the market. To produce high-voltage lithium-ion batteries, the quality requirements of cobalt tetroxide need to be strictly controlled. Cobalt tetroxide for batteries has high purity requirements, and has high requirements for its physical properties such as tap density, particle size distribution, crystal morphology, electrochemical stability, and thermal stability.
[0003] In the prior art, the solid phase high temperature calcination method or the liquid phase coprecipitation method is usually used to prepare aluminum-doped cobalt oxide. Among them, the solid phase high temperature calcination method has defects such as high energy consumption, high equipment requirements, complex calcination process, and uneven bulk doping, so its application range is limited. The liquid phase coprecipitation method is one of the commonly used methods for preparing battery material precursors. This method has good reproducibility and relatively low energy consumption. For example, CN103746114A provides a method for preparing a lithium cobalt oxide positive electrode material, which relates to a positive electrode material for a lithium ion secondary battery. Prepare a cobalt salt solution and a precipitant solution, and use a controlled crystallization process to precipitate a cobalt carbonate precursor, wherein the cobalt carbonate precursor requires: median diameter D50: 13-20 μm, 0.40≤consistency≤0.50, and sinter the cobalt carbonate to obtain cobalt tetroxide; mix cobalt tetroxide, additives, and lithium compounds, and then sinter them. The sintered product is powdered and sieved to obtain a lithium cobalt oxide semi-finished product with D50: 13-20 μm and a consistency of 0.45-0.55; mix the lithium compound and the coating element M, and then add the obtained lithium cobalt oxide semi-finished product to a ball mill for mixing. The mixed material is sintered, and the sintered product is powdered and sieved to obtain a lithium cobalt oxide positive electrode material. However, due to the different solubility products of various elements, the sedimentation velocity difference is too large, resulting in uneven distribution of the doping elements in the main material.
[0004] CN108373175A discloses an aluminum-doped cobalt oxide and its preparation method and application, specifically disclosing that after mixing an aluminum salt with a complexing agent to obtain a solution, a cobalt salt solution, a carbonate ion-containing precipitant solution and the mixed solution are added to a reaction device in a parallel flow manner, and aluminum-doped cobalt carbonate is obtained by coprecipitation; the aluminum-doped cobalt carbonate is calcined to obtain the aluminum-doped cobalt oxide. This method overcomes the problem of large differences in the sedimentation rates of various elements in the process of preparing aluminum-doped cobalt oxide by conventional liquid phase coprecipitation method by a parallel flow feeding method. However, the cobalt oxide obtained by this method has a low tap density and poor particle size uniformity, which affects its electrochemical performance.
[0005] Therefore, how to improve the particle size uniformity and element doping uniformity of cobalt tetroxide precursor materials is currently in urgent need of research. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an aluminum-manganese-nickel co-doped cobalt carbonate precursor and its preparation method and use. The preparation method provided by the present invention realizes the uniform doping of aluminum, nickel and manganese in the cobalt carbonate precursor material, which not only reduces the risk of low capacity caused by only increasing the aluminum content, but also reduces the risk of small particles exploding during the reaction, so that the obtained cobalt oxide precursor material has uniform particle size and uniform distribution of doping elements, and the preparation method described in the present invention is simple to operate and can realize industrial large-scale production.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing an aluminum-manganese-nickel co-doped cobalt carbonate precursor, the preparation method comprising the following steps:
[0009] Mixing a cobalt-aluminum mixed salt solution, a manganese salt solution, a nickel salt solution and a precipitant solution to perform a coprecipitation reaction to obtain the aluminum-manganese-nickel co-doped cobalt carbonate precursor;
[0010] Wherein, the cobalt-aluminum mixed salt solution includes a complexing agent; the manganese salt solution includes a first surfactant and a second surfactant, the first surfactant includes a crown ether surfactant, and the second surfactant includes a nonionic surfactant.
[0011] The preparation method provided by the present invention prepares raw materials for separate feeding, adds a complexing agent to the aluminum salt, avoids the segregation of the Al element, and the surfactant added to the manganese salt can effectively avoid the segregation of manganese ions during the reaction process, improves the uniform dispersion of the manganese element in the final product, and cooperates with each other so that the particles of the prepared cobalt carbonate precursor are not easy to agglomerate, the size is controllable, and the dispersibility is good, which not only reduces the risk of low capacity caused by only increasing the aluminum content, but also reduces the risk of small particles exploding during the reaction, so that the obtained cobalt oxide precursor material has uniform particle size and uniform distribution of doping elements, can effectively improve the recycling performance of lithium cobalt oxide under high pressure environment, and can significantly improve the capacity of lithium ion batteries. The preparation method of the present invention is simple to operate and can realize industrial large-scale production.
[0012] In the present invention, if all the raw materials for preparation are not fed separately, it is impossible to achieve uniform distribution of aluminum, manganese and nickel in the cobalt carbonate precursor material, and the uniformity of the particle size is also affected.
[0013] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0014] Preferably, in the cobalt-aluminum mixed salt solution, the molar ratio of aluminum to the complexing agent is 8:(1-2), for example 8:1, 8:1.1, 8:1.2, 8:1.3, 8:1.4, 8:1.5, 8:1.6, 8:1.7, 8:1.8, 8:1.9 or 8:2, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] In the present invention, the molar ratio of aluminum to the complexing agent is 8:(1-2). The addition of an appropriate amount of the complexing agent can adjust the hydrolysis degree of the metal ions in the solution, thereby controlling the formation speed and morphology of the precipitate.
[0016] Preferably, the total concentration of cobalt ions and aluminum ions in the cobalt-aluminum mixed salt solution is 110-150 g / L and does not include 110 g / L, for example, 115 g / L, 120 g / L, 125 g / L, 130 g / L, 135 g / L, 140 g / L, 145 g / L or 150 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] Preferably, the concentration of cobalt ions in the cobalt-aluminum mixed salt solution is 110-130 g / L, for example, 110 g / L, 115 g / L, 120 g / L, 125 g / L or 130 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, in the manganese salt solution, the mass ratio of the first surfactant, the second surfactant and the manganese in the manganese salt is (0.01-0.06):(0.03-0.08):1, for example, 0.01:0.03:1, 0.01:0.04:1, 0.01:0.05:1, 0.01:0.06:1, 0.01:0.07:1, 0.01:0.08:1, 0.03:0.04:1, 0.03:0.04:1, 0.01:0.05:1, 0.01:0.06:1, 0.01:0.07:1, 0.01:0.08:1, 0.03:0.04:1, 0.03:0.04:1, 0.03:0.04:1, 0 .03:0.04:1, 0.06:0.04:1, 0.06:0.04:1, 0.06:0.04:1, 0.08:0.04:1, 0.08:0.04:1, 0.08:0.04:1, 0.06:0.08:1, 0.06:0.05:1, 0.06:0.05:1 or 0.06:0.05:1, etc., but are not limited to the listed values, other values not listed within the numerical range are also applicable.
[0019] In the present invention, the mass ratio of the first surfactant, the second surfactant and the manganese in the manganese salt is (0.01-0.06):(0.03-0.08):1, which can achieve uniform doping of manganese and avoid agglomeration of material particles.
[0020] Preferably, the content of manganese ions in the manganese salt solution is 1000-3000 ppm, for example, 1000 ppm, 1300 ppm, 1500 ppm, 1800 ppm, 2000 ppm, 2300 ppm, 2500 ppm, 2800 ppm or 3000 ppm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the nickel ion content in the nickel salt solution is 3000-5000 ppm, for example, 3000 ppm, 3300 ppm, 3500 ppm, 3800 ppm, 4000 ppm, 4300 ppm, 4500 ppm, 4800 ppm or 5000 ppm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the feed rate of the cobalt-aluminum mixed salt solution is 15 to 35 L / h, for example, 15 L / h, 20 L / h, 25 L / h, 30 L / h or 35 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the feed rate of the manganese salt solution is 0.2-1 L / h, for example 0.2 L / h, 0.3 L / h, 0.4 L / h, 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h or 1 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the feeding rate of the nickel salt solution is 0.5-2 L / h, for example 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h, 1 L / h, 1.1 L / h, 1.2 L / h, 1.3 L / h, 1.4 L / h, 1.5 L / h, 1.6 L / h, 1.7 L / h, 1.8 L / h, 1.9 L / h or 2 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] In the present invention, by regulating the feed flow rate of the manganese salt solution and the feed flow rate of the nickel salt solution, the doping content of the manganese element and the nickel element can be better controlled, thereby achieving a significant improvement in battery performance, including improving the energy density, cycle life, and energy storage efficiency of the battery, and meeting the needs of different fields for high-performance batteries.
[0026] Preferably, the pH value of the coprecipitation reaction is 7-8, for example, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9 or 8, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the reaction temperature of the coprecipitation reaction is 40-45°C, for example, 40°C, 41°C, 42°C, 43°C, 44°C or 45°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the stirring speed of the coprecipitation reaction is 180-220 rpm, for example, 180 rpm, 190 rpm, 200 rpm, 210 rpm or 220 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] Preferably, the product of the coprecipitation reaction is washed and dried.
[0030] Preferably, the D50 of the aluminum-manganese-nickel co-doped cobalt carbonate precursor is 15 to 20 μm, for example, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] In the present invention, D50 of the aluminum-manganese-nickel co-doped cobalt carbonate precursor is the stopping particle size.
[0032] As a preferred technical solution, the preparation method comprises the following steps:
[0033] A cobalt-aluminum mixed salt solution with a total concentration of cobalt ions and aluminum ions of 110 to 150 g / L, a manganese salt solution with a manganese ion content of 1000 to 3000 ppm, a nickel salt solution with a nickel ion content of 3000 to 5000 ppm and a precipitant solution are mixed, the manganese salt solution is fed at a rate of 0.2 to 1 L / h, the nickel salt solution is fed at a rate of 0.5 to 2 L / h, and a pH value of 7 to 8 is used to perform a coprecipitation reaction to obtain the aluminum-manganese-nickel co-doped cobalt carbonate precursor;
[0034] Wherein, the cobalt-aluminum mixed salt solution includes a chelating agent, and the molar ratio of aluminum to the chelating agent is 8:(1-2); the manganese salt solution includes a first surfactant and a second surfactant, and the mass ratio of the first surfactant, the second surfactant and manganese in the manganese salt is (0.01-0.06):(0.03-0.08):1, the first surfactant includes a crown ether surfactant, and the second surfactant includes a nonionic surfactant.
[0035] It should be noted that, except for the above-mentioned characteristic limitations, the specific types of substances, preparation parameters and preparation processes in the preparation process are all conventional technical solutions;
[0036] Optionally, the coprecipitation reaction can be carried out in a base liquid, with a precipitant solution as the reaction base liquid, and the concentration of the precipitant solution is 160 to 220 g / L, for example, 160 g / L, 170 g / L, 180 g / L, 190 g / L, 200 g / L, 210 g / L or 220 g / L, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0037] Optionally, the precipitant includes but is not limited to at least one of sodium bicarbonate, sodium hydroxide or sodium carbonate;
[0038] Optionally, the type of the salt solution in the preparation raw material includes but is not limited to at least one of sulfate, chloride, nitrate or acetate;
[0039] Optionally, the washing adopts an ammonium bicarbonate solution, and the concentration of ammonium bicarbonate in the washing process is 40-60 g / L, such as 40 g / L, 45 g / L, 50 g / L, 55 g / L or 60 g / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0040] Optionally, the crown ether surfactant includes but is not limited to at least one of 18-crown-6, dibenzo-18-crown-6 or 15-crown-5;
[0041] Optionally, the nonionic surfactant includes but is not limited to HL-610 nonionic surfactant.
[0042] In a second aspect, the present invention provides an aluminum-manganese-nickel co-doped cobalt carbonate precursor, wherein the aluminum-manganese-nickel co-doped cobalt carbonate precursor is prepared by the preparation method described in the first aspect.
[0043] In a third aspect, the present invention provides a cobalt trioxide precursor, which is obtained by calcining the aluminum-manganese-nickel co-doped cobalt carbonate precursor as described in the second aspect.
[0044] In the present invention, the method of calcining a cobalt carbonate precursor co-doped with aluminum, manganese and nickel to obtain cobalt tetroxide is a conventional technical solution. The specific calcination process can be adaptively selected and adjusted by those skilled in the art according to actual needs.
[0045] Specifically, the calcination can be a one-stage calcination or a segmented calcination;
[0046] Optionally, the heating rate of the one-stage calcination is 8 to 12°C / min, such as 8°C / min, 9°C / min, 10°C / min, 11°C / min or 12°C / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0047] Optionally, the temperature of the one-stage calcination is 600-750°C, such as 600°C, 650°C, 700°C or 750°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0048] Optionally, the holding time of the one-stage calcination is 90 to 200 min, for example 90 min, 100 min, 130 min, 150 min, 180 min or 200 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] In a fourth aspect, the present invention provides a lithium cobalt oxide positive electrode material, wherein the lithium cobalt oxide positive electrode material is obtained by mixing and sintering the cobalt oxide precursor as described in the third aspect and a lithium source.
[0050] In a fifth aspect, the present invention further provides a lithium-ion battery, wherein the lithium-ion battery comprises the lithium cobalt oxide positive electrode material as described in the fourth aspect.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] The preparation method provided by the present invention prepares raw materials for separate feeding, adds a complexing agent to the aluminum salt, avoids the segregation of the Al element, and the surfactant added to the manganese salt can effectively avoid the segregation of manganese ions during the reaction process, improves the uniform dispersion of the manganese element in the final product, and cooperates with each other so that the particles of the prepared cobalt carbonate precursor are not easy to agglomerate, the size is controllable, and the dispersibility is good, which not only reduces the risk of low capacity caused by only increasing the aluminum content, but also reduces the risk of small particles exploding during the reaction, so that the obtained cobalt oxide precursor material has uniform particle size and uniform distribution of doping elements, can effectively improve the recycling performance of lithium cobalt oxide under high pressure environment, and can significantly improve the capacity of lithium ion batteries. The preparation method of the present invention is simple to operate and can realize industrial large-scale production. DETAILED DESCRIPTION
[0053] The technical scheme of the present invention is further illustrated by specific examples below. Those skilled in the art should understand that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0055] In the description of this application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0056] Example 1
[0057] This embodiment provides an aluminum-manganese-nickel co-doped cobalt carbonate precursor, and the preparation method of the aluminum-manganese-nickel co-doped cobalt carbonate precursor is as follows:
[0058] (1) preparing a cobalt-aluminum mixed salt solution of a cobalt salt (cobalt sulfate) solution and an aluminum salt (aluminum sulfate) solution with a mixed concentration of 120 g / L (wherein the concentration of cobalt ions is 110 g / L), the cobalt-aluminum mixed salt solution also containing a tartaric acid complexing agent (the molar ratio of the tartaric acid complexing agent to aluminum is 1:8), preparing a nickel salt solution (nickel sulfate) with a nickel ion content of 3000 ppm, preparing a manganese salt solution (manganese sulfate) with a manganese ion content of 1000 ppm, the manganese salt solution including dibenzo-18 crown-6 and HL-610 nonionic surfactants (the mass ratio of dibenzo-18 crown-6 to HL-610 nonionic surfactant to manganese is 0.01:0.03:1), and preparing an ammonium bicarbonate solution (precipitant solution) with a concentration of 160 g / L as a reaction base liquid;
[0059] (2) In a reactor with a nitrogen atmosphere and a pressure of 0.3 MPa, the reactor size is 1.5 L, and an ammonium bicarbonate solution is added as a base liquid, wherein the volume proportion of the base liquid in the reactor is 40%, and the pH value of the base liquid is 7.4;
[0060] Then, the cobalt-aluminum mixed salt solution, the manganese salt solution and the manganese salt solution are added to the bottom solution in parallel to carry out a coprecipitation reaction;
[0061] The pH value of the reaction nucleation stage was regulated within the range of 7.4-8.6 (the particle size D50 of the particles reached 4 μm, and the reaction nucleation stage ended), the pH value of the particle growth stage was maintained at about 7.1, the reaction temperature was 42°C, the rotation speed was 220 rpm, the feed rate of the cobalt-aluminum mixed salt solution was set at 20 L / h, the feed rate of the nickel salt was set at 0.5 L / h, and the feed rate of the mixed manganese salt was set at 0.2 L / h;
[0062] After the D50 of the aluminum-manganese-nickel co-doped cobalt carbonate reaches 16 μm, the reaction is stopped; the obtained aluminum-manganese-nickel co-doped cobalt carbonate precursor is washed with a dilute ammonium carbonate (ammonium bicarbonate) solution with a concentration of 40 g / L. After washing, it is dried in an oven at 110° C. to obtain an aluminum-manganese-nickel co-doped cobalt carbonate precursor material.
[0063] This embodiment also provides an aluminum-manganese-nickel co-doped cobalt oxide, and the preparation method of the cobalt oxide is as follows:
[0064] The prepared aluminum-manganese-nickel co-doped cobalt carbonate precursor material was heated to a calcination temperature of 750° C. at a heating rate of 8° C. / min and then kept warm for 90 minutes to obtain the aluminum-manganese-nickel co-doped cobalt tetroxide.
[0065] Example 2
[0066] This embodiment provides an aluminum-manganese-nickel co-doped cobalt carbonate precursor, and the preparation method of the aluminum-manganese-nickel co-doped cobalt carbonate precursor is as follows:
[0067] (1) preparing a cobalt-aluminum mixed salt solution of a cobalt salt (cobalt sulfate) solution and an aluminum salt (aluminum sulfate) solution with a mixed concentration of 150 g / L (wherein the concentration of cobalt ions is 130 g / L), the cobalt-aluminum mixed salt solution also containing a tartaric acid complexing agent (the molar ratio of the tartaric acid complexing agent to aluminum is 2:8), preparing a nickel salt solution with a nickel ion content of 5000 ppm, preparing a manganese salt solution with a manganese ion content of 3000 ppm, the manganese salt solution containing dibenzo-18 crown-6 and HL-610 nonionic surfactants (the mass ratio of dibenzo-18 crown-6 to HL-610 nonionic surfactant to manganese is 0.06:0.08:1), and preparing an ammonium bicarbonate solution (precipitant solution) with a concentration of 220 g / L as a reaction base liquid;
[0068] (2) In a reactor with a nitrogen atmosphere and a pressure of 0.3 MPa, the reactor size is 1.5 L, and an ammonium bicarbonate solution is added as a base liquid, wherein the volume proportion of the base liquid in the reactor is 45%, and the pH of the base liquid is 7.5;
[0069] Then, the cobalt-aluminum mixed salt solution, the manganese salt solution and the manganese salt solution are added to the bottom solution in parallel to carry out a coprecipitation reaction;
[0070] The pH value of the reaction nucleation stage is regulated within the range of 7.4-8.6 (the particle size D50 of the particles reaches 4 μm, and the reaction nucleation stage ends), the pH value of the particle growth stage is maintained at about 7.2, the reaction temperature is 40°C, the rotation speed is 180 rpm, the feed rate of the cobalt-aluminum mixed salt solution is set at 35 L / h, the feed rate of the nickel salt is set at 2 L / h, and the feed rate of the mixed manganese salt is set at 1 L / h;
[0071] After the D50 of the aluminum-manganese-nickel co-doped cobalt carbonate reaches 20 μm, the reaction is stopped; the obtained aluminum-manganese-nickel co-doped cobalt carbonate precursor is washed with a dilute ammonium carbonate (ammonium bicarbonate) solution with a concentration of 50 g / L. After washing, it is dried in an oven at 110° C. to obtain an aluminum-manganese-nickel co-doped cobalt carbonate precursor material.
[0072] This embodiment also provides an aluminum-manganese-nickel co-doped cobalt oxide, and the preparation method of the cobalt oxide is as follows:
[0073] The prepared aluminum-manganese-nickel co-doped cobalt carbonate precursor material was heated to a calcination temperature of 700° C. at a heating rate of 10° C. / min and then kept warm for 150 minutes to obtain the aluminum-manganese-nickel co-doped cobalt tetroxide.
[0074] Example 3
[0075] This embodiment provides an aluminum-manganese-nickel co-doped cobalt carbonate precursor, and the preparation method of the aluminum-manganese-nickel co-doped cobalt carbonate precursor is as follows:
[0076] (1) preparing a cobalt-aluminum mixed salt solution of a cobalt salt (cobalt sulfate) solution and an aluminum salt (aluminum sulfate) solution with a mixed concentration of 130 g / L (wherein the concentration of cobalt ions is 120 g / L), the cobalt-aluminum mixed salt solution also containing a tartaric acid complexing agent (the molar ratio of the tartaric acid complexing agent to aluminum is 1.5:8), preparing a nickel salt solution with a nickel ion concentration of 4000 ppm, preparing a manganese salt solution with a manganese ion concentration of 2000 ppm, the manganese salt solution including 18-crown-6 and HL-610 nonionic surfactants (the mass ratio of dibenzo-18 crown-6 to HL-610 nonionic surfactant to manganese is 0.01:0.03:1), and preparing an ammonium bicarbonate solution (precipitant solution) with a concentration of 160 g / L as a reaction base liquid;
[0077] (2) In a 2 L reactor under a nitrogen atmosphere and a pressure of 0.3 MPa, an ammonium bicarbonate solution was added as a base liquid, wherein the base liquid accounted for 45% of the volume of the reactor and the pH of the base liquid was 7.4;
[0078] Then, the cobalt-aluminum mixed salt solution, the manganese salt solution and the manganese salt solution are added to the bottom solution in parallel to carry out a coprecipitation reaction;
[0079] The pH value of the reaction nucleation stage was regulated within the range of 7.4-8.6 (the particle size D50 of the particles reached 4.5 μm, and the reaction nucleation stage ended), the pH value of the particle growth stage was maintained at about 7.1, the reaction temperature was 42°C, the rotation speed was 220 rpm, the feed rate of the cobalt-aluminum mixed salt solution was set at 25 L / h, the feed flow rate of the nickel salt was set at 1 L / h, and the feed flow rate of the mixed manganese salt was set at 0.5 L / h;
[0080] After the D50 of the aluminum-manganese-nickel co-doped cobalt carbonate reaches 18 μm, the reaction is stopped; the obtained aluminum-manganese-nickel co-doped cobalt carbonate precursor is washed with a dilute ammonium carbonate (ammonium bicarbonate) solution with a concentration of 40 g / L. After washing, it is dried in an oven at 110°C to obtain an aluminum-manganese-nickel co-doped cobalt carbonate precursor material.
[0081] This embodiment also provides an aluminum-manganese-nickel co-doped cobalt oxide, and the preparation method of the cobalt oxide is as follows:
[0082] The prepared aluminum-manganese-nickel co-doped cobalt carbonate precursor material was heated to a calcination temperature of 750° C. at a heating rate of 8° C. / min and then kept warm for 90 minutes to obtain the aluminum-manganese-nickel co-doped cobalt tetroxide.
[0083] Example 4
[0084] The difference between this embodiment and embodiment 1 is that in step (1) of this embodiment, the molar ratio of tartaric acid complexing agent to aluminum is 3:8.
[0085] The rest of the preparation methods and parameters were the same as those in Example 1.
[0086] Example 5
[0087] The difference between this embodiment and embodiment 1 is that the feed flow rate of the nickel salt solution in step (2) of this embodiment is 2.5 L / h.
[0088] The rest of the preparation methods and parameters were the same as those in Example 1.
[0089] Example 6
[0090] The difference between this embodiment and embodiment 1 is that the feed flow rate of the nickel salt solution in step (2) of this embodiment is 0.3 L / h.
[0091] The rest of the preparation methods and parameters were the same as those in Example 1.
[0092] Example 7
[0093] The difference between this embodiment and embodiment 1 is that the feed flow rate of the manganese salt solution in step (2) of this embodiment is 1.5 L / h.
[0094] The rest of the preparation methods and parameters were the same as those in Example 1.
[0095] Example 8
[0096] The difference between this embodiment and embodiment 1 is that the feed flow rate of the manganese salt solution in step (2) of this embodiment is 0.1 L / h.
[0097] The rest of the preparation methods and parameters were the same as those in Example 1.
[0098] Comparative Example 1
[0099] The difference between this comparative example and Example 1 is that in step (1) of this comparative example, cobalt sulfate, aluminum sulfate, nickel sulfate and manganese sulfate are directly mixed to obtain a mixed salt solution, and the mixed salt solution also includes tartaric acid complexing agent, dibenzo-18 crown-6 and HL-610 non-ionic surfactants. The concentration of cobalt ions in the mixed salt solution is 110 g / L, the concentration of cobalt-aluminum mixed ions is 120 g / L, the molar ratio of tartaric acid complexing agent to aluminum is 1:8, the nickel ions are 3000 ppm, the manganese ions are 1000 ppm, and the mass ratio of dibenzo-18 crown-6 to HL-610 non-ionic surfactant to manganese is 0.01:0.03:1.
[0100] The rest of the preparation methods and parameters were the same as those in Example 1.
[0101] Comparative Example 2
[0102] The difference between this comparative example and Example 1 is that the cobalt-aluminum mixed salt solution in step (1) of this comparative example does not contain a complexing agent.
[0103] The rest of the preparation methods and parameters were the same as those in Example 1.
[0104] Comparative Example 3
[0105] The difference between this comparative example and Example 1 is that the manganese salt solution in step (1) of this comparative example does not contain dibenzo-18-crown-6.
[0106] The rest of the preparation methods and parameters were the same as those in Example 1.
[0107] Comparative Example 4
[0108] The difference between this comparative example and Example 1 is that the manganese salt solution in step (1) of this comparative example does not contain HL-610 nonionic surfactant.
[0109] The rest of the preparation methods and parameters were the same as those in Example 1.
[0110] [Battery preparation and performance testing]
[0111] Battery preparation:
[0112] The cobalt oxide precursor materials and lithium carbonate provided in Examples 1-8 and Comparative Examples 1-4 were weighed respectively at a molar ratio of lithium to cobalt of 1.025, mixed evenly, and sintered in a box furnace at 1100° C. for 9 hours in an air atmosphere; the primary sintered product after sintering was crushed, iron removed, and sieved to obtain a lithium cobalt oxide material;
[0113] 80 wt % of positive electrode active material (lithium cobalt oxide prepared in Examples 1-8 and Comparative Examples 1-4, respectively) 10 wt % of Super-P and 10 wt % of polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone (NMP) solution to prepare an electrode slurry, which is coated on an aluminum foil and dried to obtain a positive electrode;
[0114] The lithium sheet is the negative electrode;
[0115] The separator is a Φ19 PP microporous membrane (Celgard2400);
[0116] The composition of the electrolyte is: a mixture of 1M LiPF6 and EC, DMC and EMC (EC:DMC:EMC volume ratio = 1:1:1).
[0117] The positive electrode, separator, negative electrode and electrolyte are assembled to obtain a button battery.
[0118] The lithium ion batteries provided in Examples 1-8 and Comparative Examples 1-4 were subjected to performance tests under the following test conditions: 3.0-4.48 V, current density IC=180 mAh / g, and test temperature of 25±1° C. The discharge capacity and cycle performance of the lithium ion batteries were tested, and the test results are shown in Table 1.
[0119] Table 1
[0120]
[0121] From Table 1, we can get:
[0122] From the data results of Example 1 and Example 4, it can be seen that if the molar ratio of the complexing agent to aluminum is too large, more aluminum ions are complexed, resulting in incomplete reaction. In this case, the morphology of the precursor becomes loose and the tap density decreases. In addition, excessive complexing agent will also cause the complexed metal ions to be discharged with the supernatant, resulting in a waste of raw materials and increasing the difficulty of subsequent wastewater treatment.
[0123] It can be seen from the data results of Example 1 and Examples 5-8 that the present invention can better control the doping content of manganese and nickel elements by regulating the feed flow rates of nickel salt solution and manganese salt solution, thereby achieving a significant improvement in battery performance, including improving energy density, cycle life, and battery energy storage efficiency, and meeting the needs of high-performance batteries in different fields; while too large or too small a feed flow rate will lead to unstable doping amount and uneven distribution of doping elements in the precursor.
[0124] It can be seen from the data results of Example 1 and Comparative Example 1 that if the feed is not separated, the doping content of the doping element cannot be accurately controlled due to the different precipitation rates of each element, which in turn affects the discharge capacity.
[0125] It can be seen from the data results of Example 1 and Comparative Examples 2-4 that in the process of separate feeding, if the complexing agent and the first surfactant and the second surfactant are not added in coordination, high tap density, good particle dispersion and the effect of controlling particle growth and morphology cannot be achieved.
[0126] In summary, the preparation method provided by the present invention prepares the raw materials and feeds them separately, adds a chelating agent to the aluminum salt, avoids the segregation of the Al element, and the surfactant added to the manganese salt can effectively avoid the segregation of manganese ions during the reaction, improves the uniform dispersion of the manganese element in the final product, and cooperates with each other, so that the particles of the prepared cobalt carbonate precursor are not easy to agglomerate, the size is controllable, and the dispersibility is good, which not only reduces the low capacity risk caused by only increasing the aluminum content, but also reduces the risk of small particles exploding during the reaction, so that the obtained cobalt oxide precursor material has uniform particle size and uniform distribution of doping elements, which can effectively improve the recycling performance of lithium cobalt oxide under high pressure environment, and can significantly improve the capacity of lithium ion batteries, and the preparation method described in the present invention is simple to operate and can realize industrial large-scale production.
[0127] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an aluminum-manganese-nickel co-doped cobalt carbonate precursor, It is characterized in that The preparation method comprises the following steps: Mixing a cobalt-aluminum mixed salt solution, a manganese salt solution, a nickel salt solution and a precipitant solution to perform a coprecipitation reaction to obtain the aluminum-manganese-nickel co-doped cobalt carbonate precursor; Wherein, the cobalt-aluminum mixed salt solution includes a complexing agent; the manganese salt solution includes a first surfactant and a second surfactant, the first surfactant includes a crown ether surfactant, and the second surfactant includes a nonionic surfactant.
2. The preparation method according to claim 1, It is characterized in that In the cobalt-aluminum mixed salt solution, the molar ratio of aluminum to the complexing agent is 8:(1-2); Preferably, the total concentration of cobalt ions and aluminum ions in the cobalt-aluminum mixed salt solution is 110-150 g / L (excluding 110 g / L), and the concentration of cobalt ions in the cobalt-aluminum mixed salt solution is 110-130 g / L.
3. The preparation method according to claim 1 or 2, It is characterized in that In the manganese salt solution, the mass ratio of the first surfactant, the second surfactant and the manganese in the manganese salt is (0.01-0.06):(0.03-0.08):1; Preferably, the content of manganese ions in the manganese salt solution is 1000 to 3000 ppm; Preferably, the content of nickel ions in the nickel salt solution is 3000-5000 ppm.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that The feeding rate of the cobalt-aluminum mixed salt solution is 15 to 35 L / h; Preferably, the feeding rate of the manganese salt solution is 0.2 to 1 L / h; Preferably, the feeding rate of the nickel salt solution is 0.5-2 L / h.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The pH value of the coprecipitation reaction is 7-8, the reaction temperature of the coprecipitation reaction is 40-45° C., and the stirring speed of the coprecipitation reaction is 180-220 rpm; Preferably, the product of the coprecipitation reaction is washed and dried; Preferably, the D50 of the aluminum-manganese-nickel co-doped cobalt carbonate precursor is 15-20 μm.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: A cobalt-aluminum mixed salt solution with a total concentration of cobalt ions and aluminum ions of 110 to 150 g / L, a manganese salt solution with a manganese ion content of 1000 to 3000 ppm, a nickel salt solution with a nickel ion content of 3000 to 5000 ppm and a precipitant solution are mixed, the manganese salt solution is fed at a rate of 0.2 to 1 L / h, the nickel salt solution is fed at a rate of 0.5 to 2 L / h, and a pH value of 7 to 8 is used to perform a coprecipitation reaction to obtain the aluminum-manganese-nickel co-doped cobalt carbonate precursor; Wherein, the cobalt-aluminum mixed salt solution includes a chelating agent, and the molar ratio of aluminum to the chelating agent is 8:(1-2); the manganese salt solution includes a first surfactant and a second surfactant, and the mass ratio of the first surfactant, the second surfactant and manganese in the manganese salt is (0.01-0.06):(0.03-0.08):1, the first surfactant includes a crown ether surfactant, and the second surfactant includes a nonionic surfactant.
7. An aluminum-manganese-nickel co-doped cobalt carbonate precursor, It is characterized in that The aluminum-manganese-nickel co-doped cobalt carbonate precursor is prepared by the preparation method according to any one of claims 1 to 6.
8. A cobalt tetraoxide precursor, It is characterized in that The cobalt trioxide precursor is obtained by calcining the aluminum-manganese-nickel co-doped cobalt carbonate precursor as claimed in claim 7.
9. A lithium cobalt oxide positive electrode material, It is characterized in that The lithium cobalt oxide positive electrode material is obtained by mixing and sintering the cobalt trioxide precursor as claimed in claim 8 and a lithium source.
10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the lithium cobalt oxide positive electrode material as claimed in claim 9.
Citation Information
Patent Citations
Preparation method of cobalt-aluminum oxide for lithium-ion power battery
CN105098171A
Flower-like aluminium-doped cobaltosic oxide and production method and application thereof
CN110015698A
Nickel-manganese double-metal doped large-particle cobalt carbonate as well as preparation method and application thereof
CN114804222A
Manganese-doped cobaltosic oxide as well as preparation method and application thereof
CN115215381A
Four-element synergistically doped high-voltage LiCoO2 and preparation method thereof
CN115417458A
Cited By
Composite cobaltosic oxide precursor material and preparation method and application thereof
CN120565666A