A low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive and its preparation method

By coating the surface of boron nitride with a low-melting-point alloy to construct a conductive network, the problem of insufficient electromagnetic shielding performance of boron nitride epoxy adhesive is solved, achieving improved high conductivity and electromagnetic shielding performance, making it suitable for electronic devices and communication systems.

CN117210175BActive Publication Date: 2026-11-17ZHEJIANG TIANNU GROUP PAINT MFG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311222461.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-21
Publication Date
2026-11-17
Estimated Expiration
2043-09-21

AI Technical Summary

Technical Problem

The existing insulating boron nitride epoxy adhesive is unevenly dispersed, resulting in insufficient electromagnetic shielding performance, which cannot meet the needs of lightweight electronic devices and communication systems.

Method used

By coating a low-melting-point alloy onto the surface of boron nitride, an epoxy resin matrix network framework is constructed using lamellar boron nitride, and surface modifiers are used to improve interfacial wettability, allowing the low-melting-point alloy to form a conductive network on the surface of boron nitride, thereby enhancing interfacial polarization and improving electromagnetic shielding performance.

Benefits of technology

It improves electromagnetic shielding performance, achieves high conductivity and electromagnetic shielding effectiveness up to 20dB, and has a conductivity of 50S/m. It has wide applicability, is simple to prepare, environmentally friendly, and low in cost, making it suitable for multiple fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117210175B_ABST
    Figure CN117210175B_ABST
Patent Text Reader

Abstract

This invention relates to a low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive and its preparation method, comprising the following components by mass fraction: 35-25% epoxy resin matrix, 30-50% low-melting-point alloy-coated boron nitride filler, and 35-25% curing agent. This composite adhesive can effectively form electron transport channels and improve conductivity and electromagnetic shielding performance. At a relatively low filler content, this composite adhesive exhibits excellent conductivity and electromagnetic shielding performance, with a maximum electromagnetic shielding effectiveness greater than 20 dB and a maximum conductivity greater than 50 S / m. This invention has advantages such as simple preparation, environmental friendliness, high performance, low cost, and ease of commercial application. As an excellent electromagnetic shielding material, it can be widely used in electronic and electrical protection, device packaging, new energy vehicle industry, and aerospace fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electronic packaging and electromagnetic shielding materials, specifically relating to a low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive and its preparation method. Background Technology

[0002] Polymer electromagnetic shielding materials are a class of key materials widely used in electronic devices, communication systems, and military equipment. They possess advantages such as lightweight, flexibility, and ease of processing, enabling them to effectively shield electromagnetic radiation, protect equipment from interference, and reduce material weight and manufacturing costs. With the increasing prominence of electromagnetic interference caused by the continuous development of electronic devices, electromagnetic shielding capabilities have become particularly important. Traditional metallic electromagnetic shielding materials, such as iron, copper, and aluminum, while possessing good electromagnetic shielding performance, are limited in their application in lightweight and portable devices due to their high density and weight. Therefore, researchers have begun to explore polymer electromagnetic shielding materials to meet the needs of different application scenarios. Polymer electromagnetic shielding materials typically consist of conductive fillers and a polymer matrix. Conductive fillers are usually carbon nanotubes, carbon black, metal nanoparticles, or conductive polymers. These fillers impart electrical conductivity to the material, giving it the potential to shield electromagnetic radiation. Optimizing the type, shape, and content of the filler can significantly affect the material's electrical conductivity and mechanical properties.

[0003] The polymer matrix plays a crucial role in the flexibility, adhesion, and temperature resistance of polymer thermal interface materials. It is necessary to select an appropriate polymer matrix and achieve the desired properties by adjusting its chemical structure and degree of crosslinking. Furthermore, surface treatments between materials can significantly improve the interfacial adhesion of polymers and the construction of conductive networks within the matrix by fillers. Common treatment methods include surface cleaning, surface activation, and the use of adhesives.

[0004] Early electromagnetic shielding research focused primarily on traditional metallic materials such as steel, copper, and aluminum. While these materials perform well in electromagnetic shielding, their high density and weight limit their application in lightweight electronic devices and communication systems. Subsequently, conductive fillers, such as carbon black and graphite, were combined with polymer matrices to prepare conductive polymer composites. These composites offer advantages such as lightweight, flexibility, and plasticity, providing new avenues for lightweight design of electronic devices. Recent research has focused on improving the performance of conductive fillers to enhance the electromagnetic shielding effect of materials. For example, functionalization of carbon nanotubes can improve their dispersibility, reduce the material's filler content, and improve electromagnetic shielding performance. Simultaneously, the optimization of the shape and size of metallic nanoparticles is ongoing to achieve better electromagnetic wave absorption and reflection performance.

[0005] Currently, researchers are exploring new methods and technologies to improve existing polymer-based electromagnetic shielding materials or develop new electromagnetic protection materials. For example, they are utilizing mechanisms such as self-assembly, self-healing, and phase transitions to enhance interfacial polarization and improve electromagnetic loss; optimizing electromagnetic interface reflection and scattering through multilayer, gradient, and porous structures; and adjusting the chemical and physical properties of the interface through surface treatment, additives, and doping to enhance interfacial polarization and thus improve electromagnetic loss. These methods and technologies provide new ideas and possibilities for improving the level of electromagnetic protection materials and expanding their application areas. Summary of the Invention

[0006] To overcome the problems of uneven boron nitride dispersion, insulation, and lack of electromagnetic shielding performance in insulating boron nitride epoxy adhesives, this invention provides a low-melting-point alloy-coated boron nitride epoxy resin composite adhesive with high conductivity and high electromagnetic shielding performance, which is simple to prepare, environmentally friendly, high-performance, low-cost, and easy to commercially apply, along with its preparation process. In this invention, the high aspect ratio of lamellar boron nitride is used to construct the basic network framework in the epoxy resin matrix. A surface modifier is used to improve the interfacial wettability of boron nitride, allowing the low-melting-point alloy to be smoothly coated onto the surface of the boron nitride microflakes. The low-melting-point alloy coated on the boron nitride surface can contact each other along the boron nitride to form a conductive network. Simultaneously, the differentiated interface formed by the insulating boron nitride and the conductive low-melting-point alloy can enhance interfacial polarization, increase electromagnetic loss, and thus improve electromagnetic shielding performance.

[0007] To achieve the purpose of this invention, the technical solution adopted is: a low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive, comprising the following components by mass fraction:

[0008] Epoxy resin matrix 35-25%;

[0009] Low-melting-point alloy coated with 30-50% boron nitride powder;

[0010] Hardener 35-25%.

[0011] In a preferred embodiment of the present invention, the composite adhesive is composed of the following components by mass fraction: 25% epoxy resin matrix, 50% low melting point alloy-coated boron nitride powder, and 25% curing agent.

[0012] In a preferred embodiment of the present invention, the epoxy resin matrix is ​​selected from bisphenol A type epoxy resin or bisphenol F type epoxy resin.

[0013] In a preferred embodiment of the present invention, the boron nitride is a multilayer boron nitride microplate with a hexagonal layered structure.

[0014] In a preferred embodiment of the present invention, the low-melting-point alloy is a (bismuth-indium-tin) Bi-In-Sn alloy system, wherein the proportions, by mass percentage, are 35% bismuth, 50% indium, and 15% tin.

[0015] In a preferred embodiment of the present invention, the curing agent is one or more of amine curing agents and acid anhydride curing agents.

[0016] This invention also protects a method for preparing the above-mentioned low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive, which is carried out according to the following steps:

[0017] (1) Disperse boron nitride powder in a solvent, add dopamine hydrochloride, stir the resulting mixture thoroughly at room temperature for 12 hours, then separate the powder product by centrifugation, and after washing with water and ethanol, take out the product, and vacuum dry it to obtain polydopamine modified boron nitride powder.

[0018] (2) First, stir the bismuth indium tin powder in a mass ratio of 35:50:15. Then, heat the mixed powder in a sealed container to 1000 degrees Celsius and maintain the temperature for 1 hour to melt the alloy. After cooling at room temperature, low melting point alloy particles are obtained for later use.

[0019] (3) The polydopamine-modified boron nitride powder obtained in step (1) is thoroughly stirred in an organic solvent, then sonicated for 0.5 to 1 hour, and then the low-melting-point alloy particles obtained in step (2) are added. The resulting product is heated to 150 degrees Celsius and the low-melting-point alloy is completely melted. The mixture is stirred at a constant speed for 2 to 4 hours to obtain boron nitride powder coated with low-melting-point alloy, and then dried to remove the organic solvent.

[0020] (4) Stir the epoxy resin matrix, low melting point alloy-coated boron nitride powder and curing agent according to the ratio for 5-10 minutes, then add to the encapsulation mold or apply to the area to be constructed, heat to 80-100℃, cure for 3-5 hours, then raise the temperature to 120-130℃ and cure for 1-2 hours to obtain low melting point alloy-coated boron nitride epoxy resin composite adhesive.

[0021] In a preferred embodiment of the present invention, in step (1), the solvent is a mixture of tris(hydroxymethyl)aminomethane buffer solution and ethanol; more preferably, the concentration of tris(hydroxymethyl)aminomethane is 10. -2 mol / L, pH 8.5.

[0022] In a preferred embodiment of the present invention, in step (3), the organic solvent is cyclohexanol.

[0023] In a preferred embodiment of the present invention, in step (4), a vacuum stirring degasser is used for stirring.

[0024] In the preparation process of this invention, other processing aids known in the prior art, such as defoamers, curing accelerators, and reactive diluents, may be added as needed.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) After coating the surface of boron nitride with a low melting point alloy, the original insulating properties are changed to high conductivity. After adding epoxy resin matrix, the conductivity of epoxy resin is improved and electromagnetic shielding properties are given due to the characteristic that layered two-dimensional materials can easily overlap to form a conductive network.

[0027] (2) The differentiated interface formed by insulating boron nitride and conductive low-melting-point alloy can enhance interface polarization, increase electromagnetic loss, and thus improve electromagnetic shielding performance.

[0028] (3) The product of the present invention has excellent conductivity and electromagnetic shielding performance, with the highest electromagnetic shielding effectiveness of 20dB; the highest conductivity is 50S / m; it has wide environmental adaptability, can be used under acidic or alkaline conditions, and can be used normally at 120 degrees Celsius;

[0029] (4) For the first time, the surface wettability of boron nitride was modified by chemical modification to improve the interfacial compatibility between low melting point alloy and boron nitride, so that the low melting point alloy was fully coated on the surface of polydopamine-modified boron nitride, and the mass production of filler and epoxy resin composite adhesive was realized.

[0030] (5) It is easy to prepare, environmentally friendly, high-performance, low-cost and easy to commercially apply. It is an excellent electromagnetic protection and shielding material that can be widely used in electronic heat dissipation, device packaging, new energy vehicle industry and aerospace. Attached Figure Description

[0031] The following explanation, in conjunction with the accompanying drawings, will provide further details.

[0032] Figure 1 The morphology of the boron nitride powder obtained in step (3) of Example 1 of the present invention is shown.

[0033] Figure 2 The image shows the SEM cross-sectional morphology of the low-melting-point alloy-coated boron nitride epoxy resin composite adhesive obtained in Example 1 of this invention.

[0034] Figure 3 The results are the performance test results of the low melting point alloy-coated boron nitride epoxy resin composite adhesive obtained in Example 1 of the present invention. Detailed Implementation

[0035] The present invention will be specifically described below through several embodiments, but the technical scope of the present invention is not limited to these embodiments. The results obtained in the embodiments and comparative examples are test results of the material's electrical conductivity and electromagnetic shielding performance.

[0036] Example 1

[0037] (1) Disperse 5 g of boron nitride powder in a mixture of 100 ml of tris(hydroxymethyl)aminomethane buffer solution (10 mM, pH 8.5) and 50 ml of ethanol, then add 0.1 g of dopamine hydrochloride. Stir the mixture thoroughly at room temperature for 12 hours. Then, centrifuge to obtain the powder product, wash with water and ethanol, remove the product, and dry it in a vacuum drying oven to obtain polydopamine-modified boron nitride powder;

[0038] (2) First, mix the bismuth indium tin powder evenly in a mass ratio of 35:50:15. Then, take 20 grams of the mixed powder and add it to a sealed heating furnace. Heat it to 1000 degrees Celsius and maintain it for 1 hour to melt the alloy. After cooling at room temperature, you will get low-melting-point alloy particles for later use.

[0039] (3) The 5 g of polydopamine-modified boron nitride powder obtained in step (1) is thoroughly stirred in an appropriate amount of cyclohexanol, then sonicated for 0.5-1 h. Then, 1 g of low-melting-point alloy particles obtained in step (2) are added. The resulting product is heated to 150 degrees Celsius and the low-melting-point alloy is completely melted. The mixture is stirred at a constant speed for 2-4 h to obtain low-melting-point alloy-coated boron nitride powder (morphology see...). Figure 1 ), and dry the cyclohexanol solvent;

[0040] (4) Mix 25g of epoxy resin matrix, 50g of low-melting-point alloy-coated boron nitride powder, and 25g of curing agent according to the specified ratio. Use a vacuum mixer to stir for 5-10 minutes, then add the mixture to a packaging mold or apply it to the area to be treated. Heat to 80-100 degrees Celsius and cure for 3-5 hours. Then raise the temperature to 120-130 degrees Celsius and cure for 1-2 hours to obtain a low-melting-point alloy-coated boron nitride epoxy resin composite adhesive. Its SEM cross-sectional morphology is shown in [Figure number missing]. Figure 2 The performance test results are shown below. Figure 3 .

[0041] Example 2

[0042] The implementation method is the same as in Example 1, except that the low melting point alloy coated boron nitride filler obtained in step (3) is changed to 40 grams, the epoxy resin matrix is ​​changed to 30 grams, the curing agent is changed to 30 grams, and the other components and their quantities remain unchanged.

[0043] Example 3

[0044] The implementation method is the same as in Example 1, except that the low melting point alloy coated boron nitride filler obtained in step (3) is changed to 30 grams, the epoxy resin matrix is ​​changed to 35 grams, the curing agent is changed to 35 grams, and the other components and their weights remain unchanged.

[0045] Example 4

[0046] The implementation method is compared with Example 1. The composite adhesive includes 50 grams of pure boron nitride as filler, 25 grams of epoxy resin matrix, and 25 grams of curing agent. Other components and their quantities remain unchanged.

[0047] Example 5

[0048] The implementation method is compared with Example 1. The composite adhesive (excluding low melting point alloy-coated boron nitride powder) includes 50g of epoxy resin matrix, 50g of curing agent, and other components and their quantities remain unchanged.

[0049] Example 6

[0050] The implementation method is compared with Example 1. The composite adhesive includes 50 grams of pure low-melting-point alloy particles as filler, 25 grams of epoxy resin matrix, 25 grams of curing agent, and other components and their quantities remain unchanged.

[0051] The above-mentioned composite material performance test results are as follows: Figure 3 As shown. Figure 3 The test results show that the composite adhesive prepared by this invention has high electromagnetic shielding and high conductivity. A comparison between Examples 1-3 and Example 5 (pure epoxy resin) demonstrates that adding a low-melting-point alloy-coated boron nitride to the epoxy resin matrix effectively forms conductive pathways, significantly improving the conductivity and electromagnetic shielding capabilities of the composite adhesive. Furthermore, the conductivity and electromagnetic shielding capabilities of the composite adhesive increase significantly with increasing low-melting-point alloy content.

[0052] A comparison of Examples 1 and 4 demonstrates that after the filler is coated with a low-melting-point alloy, its conductivity changes from an insulating state to a conductive state. The low-melting-point alloy increases the contact between the boron nitride lamellar filler layers, reduces contact resistance, and forms effective conductive channels between the layers, significantly improving conductivity. It also provides electromagnetic shielding properties.

[0053] A comparison of Examples 1 and 6 demonstrates that boron nitride primarily serves to bridge the conductive network. Without the basic conductive framework formed by boron nitride, the low-melting-point alloys remain isolated and cannot form a conductive network, nor can they provide excellent electromagnetic shielding performance.

[0054] The above embodiments illustrate and describe the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention and are not intended to limit the scope of the invention in any way. Various changes and modifications can be made to the invention without departing from its scope, and all such changes and modifications fall within the scope of the claims.

Claims

1. A low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive, characterized in that, Components including the following mass fractions: Epoxy resin matrix 35-25%; Low-melting-point alloy coated with 30-50% boron nitride powder; Curing agent 35-25%; The preparation method of the low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive is carried out according to the following steps: (1) Disperse boron nitride powder in a solvent, add dopamine hydrochloride, stir the resulting mixture thoroughly at room temperature for 12 hours, then separate the powder product by centrifugation, and after washing with water and ethanol, take out the product, and vacuum dry it to obtain polydopamine modified boron nitride powder. (2) First, stir the bismuth indium tin powder in a mass ratio of 35:50:

15. Then, heat the mixed powder in a sealed container to 1000 degrees Celsius and maintain the temperature for 1 hour to melt the alloy. After cooling at room temperature, low melting point alloy particles are obtained for later use. (3) The polydopamine-modified boron nitride powder obtained in step (1) is thoroughly stirred in an organic solvent, then sonicated for 0.5 to 1 hour, and then the low-melting-point alloy particles obtained in step (2) are added. The resulting product is heated to 150 degrees Celsius and the low-melting-point alloy is completely melted. The mixture is stirred at a constant speed for 2 to 4 hours to obtain boron nitride powder coated with low-melting-point alloy, and then dried to remove the organic solvent. (4) Stir the epoxy resin matrix, low melting point alloy-coated boron nitride powder and curing agent according to the ratio for 5-10 minutes, then add to the encapsulation mold or apply to the area to be constructed, heat to 80-100℃, cure for 3-5 hours, then raise the temperature to 120-130℃ and cure for 1-2 hours to obtain low melting point alloy-coated boron nitride epoxy resin composite adhesive.

2. The composite adhesive according to claim 1, characterized in that, It consists of the following components by mass fraction: 25% epoxy resin matrix, 50% low-melting-point alloy-coated boron nitride powder, and 25% curing agent.

3. The composite adhesive according to claim 1, characterized in that, The epoxy resin matrix is ​​selected from bisphenol A type epoxy resin or bisphenol F type epoxy resin.

4. The composite adhesive according to claim 1, characterized in that, The boron nitride described is a multilayer boron nitride microplate with a hexagonal layered structure.

5. The composite adhesive according to claim 1, characterized in that, The low-melting-point alloy is a (bismuth-indium-tin) Bi-In-Sn alloy system, with a mass percentage of 35% bismuth, 50% indium, and 15% tin.

6. The composite adhesive according to claim 1, characterized in that, The curing agent is one or more of amine curing agents and acid anhydride curing agents.

7. The method for preparing the low-melting-point alloy-coated boron nitride epoxy resin electromagnetic shielding composite adhesive according to any one of claims 1-6, characterized in that, Follow these steps: (1) Disperse boron nitride powder in a solvent, add dopamine hydrochloride, stir the resulting mixture thoroughly at room temperature for 12 hours, then separate the powder product by centrifugation, and after washing with water and ethanol, take out the product, and vacuum dry it to obtain polydopamine modified boron nitride powder. (2) First, stir the bismuth indium tin powder in a mass ratio of 35:50:

15. Then, heat the mixed powder in a sealed container to 1000 degrees Celsius and maintain the temperature for 1 hour to melt the alloy. After cooling at room temperature, low melting point alloy particles are obtained for later use. (3) The polydopamine-modified boron nitride powder obtained in step (1) is thoroughly stirred in an organic solvent, then sonicated for 0.5 to 1 hour, and then the low-melting-point alloy particles obtained in step (2) are added. The resulting product is heated to 150 degrees Celsius and the low-melting-point alloy is completely melted. The mixture is stirred at a constant speed for 2 to 4 hours to obtain boron nitride powder coated with low-melting-point alloy, and then dried to remove the organic solvent. (4) Stir the epoxy resin matrix, low melting point alloy-coated boron nitride powder and curing agent according to the ratio for 5-10 minutes, then add to the encapsulation mold or apply to the area to be constructed, heat to 80-100℃, cure for 3-5 hours, then raise the temperature to 120-130℃ and cure for 1-2 hours to obtain low melting point alloy-coated boron nitride epoxy resin composite adhesive.

8. The preparation method according to claim 7, characterized in that, In step (1), the solvent is a mixture of tris(hydroxymethyl)aminomethane buffer solution and ethanol.

9. The preparation method according to claim 8, characterized in that, The concentration of tris(hydroxymethyl)aminomethane was 10. -2 mol / L, pH 8.

5.

10. The preparation method according to claim 7, characterized in that, In step (3), the organic solvent is cyclohexanol.

11. The preparation method according to claim 7, characterized in that, In step (4), a vacuum stirrer is used for stirring.

Citation Information

Patent Citations

  • Low-melting-point metal micro-nano powder conductive adhesive and preparation method thereof

    CN109135612A

  • Epoxy composite material with heterostructure and preparation method thereof