Non-crosslinked high flexibility neutron shielding material and preparation method thereof
By surface modification of boron carbide powder, the problem of insufficient flexibility and mechanical properties of neutron shielding materials under high filling rates was solved, realizing a non-crosslinked neutron shielding material with high filling rate and good compatibility, possessing higher flexibility and mechanical strength.
Patent Information
- Application Number
- CN202311224960.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-21
AI Technical Summary
Existing neutron shielding materials suffer from insufficient flexibility and mechanical properties at high fill rates, especially cross-linked materials, which experience increased hardness and powder shedding after increasing the powder fill rate.
By surface modification of boron carbide powder, dispersion in solvent using specific types of surfactants and mixing with polymer matrix, a non-crosslinked, highly flexible neutron shielding material is formed, achieving high filling rate and good compatibility.
It achieves a powder filling rate of up to 85%, increases the material density to 1.71 g/m3, and has higher flexibility and mechanical strength, avoiding the problems of increased hardness and powder shedding caused by cross-linking.
Smart Images

Figure BDA0004462005830000071 
Figure BDA0004462005830000081
Abstract
Description
Technical Field
[0001] This invention relates to the field of flexible neutron shielding materials, and more specifically, to a non-crosslinked, highly flexible neutron shielding material and its preparation method. Background Technology
[0002] Currently, neutron shielding methods are generally divided into fast neutron moderation and slow neutron absorption. Fast neutrons are converted into slow neutrons after inelastic scattering with heavy nuclei such as iron and tungsten. Slow neutrons can be effectively absorbed by materials containing boron (such as boron carbide). Therefore, increasing the boron carbide content in neutron shielding materials can effectively reduce the material volume, improve the material's neutron absorption efficiency, save space, and reduce thickness and weight, which is of great significance, especially for wearable protective equipment.
[0003] Currently, neutron shielding materials based on boron carbide are mainly divided into two categories: ceramic sintering and boron carbide filling with organic substrates. The former are mostly rigid materials, while the latter, due to the use of organic substrates, give the material a certain degree of flexibility. Commonly used organic substrate materials include: non-metallic gels, silicone, epoxy resins, emulsion polymerization, and polyolefins. Non-metallic gels act like glue, binding the powders together, allowing for high boron carbide powder filling rates. However, after drying, the material lacks flexibility (boron carbide powder itself is a ceramic material with high hardness; tight stacking combined with high filling rates results in an almost rigid material). Silicone substrates are soft, with high elongation at break and good deformability, but they have poor compatibility with boron carbide powder, resulting in low powder filling rates. Silicone itself also has relatively low tensile strength. Epoxy resin substrates, even with high powder filling rates, are rigid and lack flexibility. In actual production, epoxy resin substrates often require slight foaming to improve material flexibility, which significantly reduces tensile strength and makes the powder prone to detachment. Meanwhile, epoxy resin, being a cross-linked material, also suffers from low elongation at break. Polyolefin-based substrates include polypropylene and ethylene-polyvinyl acetate copolymers, etc. Polypropylene has poor compatibility with boron carbide, resulting in a low filler content. Ethylene-polyvinyl acetate copolymers are slightly better, but even direct use cannot achieve a high filler content.
[0004] Chinese patent CN108250557A discloses a method using ethylene-polyvinyl acetate copolymer (EVA) as a base material. After crosslinking with a crosslinking agent, it can achieve a boron carbide powder filling rate of 80%. This material has better flexibility and adhesion to powder; however, due to the crosslinking effect, the material has a low elongation at break, the powder stacking is relatively loose, and the material density is only 1.3-1.6 g / cm³. 3 between.
[0005] In summary, flexible substrates currently cannot be filled with powders with high filling rates (the poor compatibility between powders and substrates makes it virtually impossible to achieve a high filling rate of over 70%, and methods that can achieve high filling rates result in materials with high hardness and poor flexibility). To increase the powder filling rate, cross-linking methods must be used. For example, epoxy resin substrates can achieve high filling rates and a certain degree of flexibility through cross-linking and pore-forming. However, due to cross-linking, the mechanical properties are also very poor, and the powder adhesion is poor, making it easy to fall off. In addition, cross-linking is costly and not suitable for industrial production. Summary of the Invention
[0006] In view of this, the purpose of the present invention is to provide a non-crosslinked, highly flexible neutron shielding material and its preparation method. The preparation method provided by the present invention can achieve a high powder filling rate without crosslinking, and the product has better flexibility and mechanical strength.
[0007] This invention provides a method for preparing a non-crosslinked, highly flexible neutron shielding material, comprising the following steps:
[0008] a) The boron carbide powder and the surface modifier are dispersed evenly in the presence of a solvent, and the solvent is dried to obtain the treated powder;
[0009] b) The processed powder obtained in step a) is mixed with the polymer substrate and molded to obtain a non-crosslinked, highly flexible neutron shielding material.
[0010] Preferably, the particle size of the boron carbide powder in step a) is 100 mesh to 500 mesh.
[0011] Preferably, the surface modifier in step a) is selected from anionic surfactants and / or nonionic surfactants.
[0012] Preferably, the solvent in step a) is ethanol or water; the amount of solvent used is 20ml to 80ml per 100g of boron carbide powder.
[0013] Preferably, the dispersion method in step a) is ball milling or high-speed stirring; the dispersion speed is 200 rpm to 400 rpm, and the time is 1 h to 3 h.
[0014] Preferably, the temperature of the drying solvent in step a) is 80℃~120℃ and the time is 8h~10h.
[0015] Preferably, the polymer substrate in step b) is selected from ethylene-polyvinyl acetate copolymer, ethylene-octene block copolymer or polyolefin elastomer;
[0016] The amount of boron carbide powder used is 50% to 85% of the total mass of the polymer substrate and the boron carbide powder;
[0017] The amount of the surface modifier is 0.1% to 3.5% of the total mass of the polymer substrate and boron carbide powder.
[0018] Preferably, the mixing method in step b) is intensive mixing or open mixing; the mixing temperature is 80℃~120℃ and the time is 5min~20min.
[0019] Preferably, the molding method in step b) is direct molding or compression molding; the molding temperature is 100℃~120℃, the pressure is 2MPa~10MPa, and the time is 300s~600s.
[0020] The present invention also provides a non-crosslinked, highly flexible neutron shielding material, which is prepared by the preparation method described in the above technical solution.
[0021] This invention provides a non-crosslinked, highly flexible neutron shielding material and its preparation method. The preparation method includes the following steps: a) dispersing boron carbide powder and a surface modifier uniformly in the presence of a solvent, drying the solvent to obtain the treated powder; b) mixing the treated powder obtained in step a) with a polymer substrate, and molding to obtain the non-crosslinked, highly flexible neutron shielding material. Compared with the prior art, the preparation method provided by this invention improves the compatibility between boron carbide powder and polymer substrate by modifying the boron carbide powder, achieving a high filling rate of the powder without crosslinking, and the product has better flexibility and mechanical strength.
[0022] Meanwhile, the preparation method provided by this invention is simple, mild, and easy to control, and has broad application prospects. Detailed Implementation
[0023] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0024] This invention provides a method for preparing a non-crosslinked, highly flexible neutron shielding material, comprising the following steps:
[0025] a) The boron carbide powder and the surface modifier are dispersed evenly in the presence of a solvent, and the solvent is dried to obtain the treated powder;
[0026] b) The processed powder obtained in step a) is mixed with the polymer substrate and molded to obtain a non-crosslinked, highly flexible neutron shielding material.
[0027] The present invention first disperses boron carbide powder and surface modifier uniformly in the presence of solvent, and then dries the solvent to obtain the treated powder.
[0028] In this invention, the particle size of the boron carbide powder is preferably 100 mesh to 500 mesh, more preferably 200 mesh to 300 mesh. This invention does not impose any special restrictions on the source of the boron carbide powder; commercially available products well-known to those skilled in the art can be used.
[0029] In this invention, the surface modifier is preferably selected from anionic surfactants and / or nonionic surfactants, more preferably nonionic surfactants, specifically including silane coupling agents, polyvinyl alcohol (PVA), and stearic acid surfactants (such as sodium stearate); the anionic surfactants specifically include octylphosphonate and dodecylphosphonate. This invention does not impose any special restrictions on the source of the surface modifier; commercially available products well-known to those skilled in the art can be used. This invention modifies the surface of boron carbide powder using specific types of surface modifiers without crosslinking and foaming, which is key to ultimately obtaining materials with high filling rates and good flexibility.
[0030] In this invention, the solvent is preferably ethanol or water; the amount of solvent used is preferably 20 ml to 80 ml per 100 g boron carbide powder, more preferably 50 ml per 100 g boron carbide powder.
[0031] In this invention, the dispersion process is preferably specifically as follows:
[0032] Boron carbide powder is mixed with a surface modifier, diluted with a solvent, and then dispersed. The dispersion method is preferably ball milling or high-speed stirring. The dispersion speed is preferably 200 rpm to 400 rpm, and the dispersion time is preferably 1 h to 3 h. Specifically, the ball milling speed is preferably 300 r / min, and the stirring time is 1 h. The high-speed stirring speed is preferably 300 r / min, and the stirring time is 2 h. This ensures that the boron carbide powder and the surface modifier are fully stirred, crushed, and dispersed.
[0033] In this invention, the temperature of the drying solvent is preferably 80℃~120℃, and the time is preferably 8h~10h; in a preferred embodiment of this invention, the solvent is ethanol, and drying is carried out at 80℃ for 10h; in another preferred embodiment of this invention, the solvent is water, and drying is carried out at 120℃ for 10h.
[0034] After obtaining the processed powder, the present invention mixes the processed powder with a polymer substrate and then molds it to obtain a non-crosslinked, highly flexible neutron shielding material.
[0035] In this invention, the polymer substrate is preferably selected from ethylene-polyvinyl acetate copolymer (EVA), ethylene-octyl block copolymer (OBC), or polyolefin elastomer (POP), and more preferably ethylene-polyvinyl acetate copolymer. This invention does not impose any special restrictions on the source of the polymer substrate; commercially available products well-known to those skilled in the art can be used, such as DuPont EVA40w, Dow Chemical Infuse, Dow Chemical Engage, Dow Chemical Versify, Mobil EXACT, Mobil VISTAMAXX, and Mitsui Chemicals TAFMER series. Different polymer substrates selected in this invention will result in slight differences in the mechanical strength of the final product, but the overall difference is not significant. As long as the boron carbide powder addition amount and sheet thickness are limited, the cold and hot neutron transmittance can reach below 1e-7.
[0036] In this invention, the amount of boron carbide powder is preferably 50% to 85% of the total mass of the polymer substrate and the boron carbide powder, more preferably 70% to 85%; the amount of surface modifier is preferably 0.1% to 3.5% of the total mass of the polymer substrate and the boron carbide powder, more preferably 1.5% to 3%.
[0037] In this invention, the mixing method is preferably intensive mixing or open mixing; the mixing temperature is preferably 80℃~120℃, and the mixing time is preferably 5min~20min, more preferably 10min.
[0038] In this invention, the forming method is preferably direct forming or compression molding; the forming temperature is preferably 100℃~120℃, the pressure is preferably 2MPa~10MPa, and the time is preferably 300s~600s; wherein, direct forming means directly producing sheets after open mixing, with a preferred temperature of 110℃, a preferred pressure of 5MPa, and a preferred time of 300s; compression molding means taking out the sheet after internal mixing and sending it to a forming mold for hot pressing to form a sheet, with a preferred temperature of 100℃, a preferred pressure of 5MPa, and a preferred time of 450s.
[0039] In this invention, the non-crosslinked, highly flexible neutron shielding material is preferably a sheet with a thickness of 2mm to 5mm, more preferably 2mm to 3mm, which can meet the neutron shielding protection requirements.
[0040] Currently, existing technologies typically employ cross-linking methods to prepare neutron shielding materials. For example, this involves dissolving the substrate and added additives such as benzoyl peroxide and dicumyl peroxide in toluene, adding powder, and then cross-linking the EVA powder at high temperature before molding the resulting paste using a mold. In contrast, this invention directly blends the substrate and surface-modified boron carbide using open milling or internal mixing methods. The mixture can then be directly molded or pressed into sheets using a hydraulic press. This eliminates the need for large amounts of solvents, making it more suitable for industrial production. Furthermore, because this invention uses specific surface modifiers to treat the boron carbide powder, it exhibits better compatibility with the substrate, significantly improving the interfacial bonding between the powder and the substrate. Therefore, a powder filling rate of up to 85% can be achieved without cross-linking, and the powder stacking is more compact due to the absence of cross-linking, resulting in a material density of up to 1.71 g / m³. 3 This allows the shielding material to be thinned; at the same time, the non-crosslinked substrate makes the material have a higher elongation at break, more flexibility, and better tensile strength.
[0041] This invention also provides a non-crosslinked, highly flexible neutron shielding material, prepared using the method described above. The non-crosslinked, highly flexible neutron shielding material provided by this invention exhibits high tensile strength and elongation at break, flexibility, and no powder shedding (all other similar domestically produced products on the market shed powder, while imported products do not shed powder but are extremely expensive).
[0042] The product provided by this invention is preferably a sheet material, and its back is preferably covered with adhesive material so that it can be directly pasted onto a cement wall.
[0043] This invention provides a non-crosslinked, highly flexible neutron shielding material and its preparation method. The preparation method includes the following steps: a) dispersing boron carbide powder and a surface modifier uniformly in the presence of a solvent, drying the solvent to obtain the treated powder; b) mixing the treated powder obtained in step a) with a polymer substrate, and molding to obtain the non-crosslinked, highly flexible neutron shielding material. Compared with the prior art, the preparation method provided by this invention improves the compatibility between boron carbide powder and polymer substrate by modifying the boron carbide powder, achieving a high filling rate of the powder without crosslinking, and the product has better flexibility and mechanical strength.
[0044] Meanwhile, the preparation method provided by this invention is simple, mild, and easy to control, and has broad application prospects.
[0045] To further illustrate the present invention, the following embodiments provide a detailed description. All raw materials used in the following embodiments of the present invention are commercially available; wherein, the boron carbide powder has a particle size of 200 mesh to 300 mesh.
[0046] Example 1
[0047] 200g of boron carbide powder was mixed with polydimethylsiloxane, diluted with 100mL of ethanol solution, and ball-milled at 300rpm for 1h. The mixture was then dried at 80℃ for 10h to obtain the treated powder. The treated powder was then mixed with ethylene-octene block copolymer (Dow Chemical Infuse 9107) at 120℃ for 10 minutes using an open mill. The mass ratio of boron carbide powder, polydimethylsiloxane, and ethylene-octene block copolymer was 70:30:1.5. Finally, the roller spacing was adjusted to 3mm, and the mixed product was directly molded (temperature 110℃, pressure 5MPa, time 300 seconds) to obtain a 3mm thick sheet. The sheet had a smooth appearance and was free of cracks.
[0048] Example 2
[0049] 200g of boron carbide powder was mixed with alkylphenol polyoxyethylene ether, diluted with 100mL of ethanol solution, and ball-milled at 300rpm for 1h. The mixture was then dried at 80℃ for 10h to obtain the treated powder. The treated powder was then mixed with a polyolefin elastomer (Dow Chemical Engage8401) at 100℃ for 10 minutes using an internal mixer. The mass ratio of boron carbide powder, alkylphenol polyoxyethylene ether, and polyolefin elastomer was 80:20:2. Finally, the mixed product was removed and placed in a 2.5mm thick mold for compression molding (using a venting system, hot pressing temperature of 100℃, pressure of 5MPa, and molding time of 450 seconds) to obtain a 2.5mm thick sheet. The sheet had a smooth appearance and was free of cracks.
[0050] Example 3
[0051] 200g of boron carbide powder was mixed with sodium stearate, diluted with 100mL of ethanol solution, and ball-milled at 300rpm for 1h. The mixture was then dried at 80℃ for 10h to obtain the treated powder. The treated powder was then mixed with ethylene-polyvinyl acetate copolymer (EVA, VA content 40%) at 80℃ for 10 minutes using an open mill. The mass ratio of boron carbide powder, sodium stearate, and ethylene-polyvinyl acetate copolymer was 85:15:3. Finally, the roller spacing was adjusted to 2.5mm, and the mixed product was directly molded (temperature 110℃, pressure 5MPa, time 300 seconds) to obtain a 2.5mm thick sheet. The sheet had a smooth appearance and was free of cracks.
[0052] Comparative Example 1
[0053] 200g of boron carbide powder was mixed with hexadecyltrimethylammonium bromide, diluted with 100mL of acetic acid aqueous solution (pH=5), and ball-milled at 300rpm for 1 hour. The mixture was then dried at 120℃ for 10 hours to obtain the treated powder. The treated powder was then mixed with ethylene-polyvinyl acetate copolymer at 80℃ for 10 minutes using a two-roll mill. The mass ratio of boron carbide powder, hexadecyltrimethylammonium bromide, and ethylene-polyvinyl acetate copolymer was 85:15:3. Finally, the roller spacing was adjusted to 2.5mm, and the mixed product was directly molded (temperature 110℃, pressure 5MPa, time 300 seconds) to obtain a 2.5mm thick sheet. This sheet had an uneven appearance and was prone to cracking. Therefore, the surfactant used in Comparative Example 1 was unsuitable and did not provide sufficient modification, resulting in poor product formability.
[0054] Comparative Example 2
[0055] 200g of boron carbide powder was mixed with alkylphenol polyoxyethylene ether and polyolefin elastomer in a mass ratio of 80:20:2. The mixture was then added to an internal mixer and kneaded at 100°C for 10 minutes. The kneaded product was then removed and placed into a 2.5mm thick mold for compression molding (using a venting system, hot pressing temperature of 100°C, pressure of 5MPa, and molding time of 450 seconds) to obtain a 2.5mm thick sheet. The sheet had a smooth appearance and was free of cracks.
[0056] Various performance tests were conducted on the products obtained from the above embodiments and comparative examples. The mechanical properties of the sheets were tested according to the national standard GB / T 528-2009, with a tensile rate of 500 mm / min. The results are shown in Table 1.
[0057] Table 1. Performance data of the products obtained from the examples and comparative examples.
[0058]
[0059]
[0060] Note: All transmittance is below 10^-7, which means there is no radiation measurement by default.
[0061] As shown in Table 1, the product obtained by the preparation method provided in this embodiment of the invention has higher tensile strength and elongation at break while meeting the requirements of neutron shielding protection. The direct mixing modification effect of Comparative Example 2 is not good enough, and the mechanical properties of the product decrease. Moreover, the high filling rate of the powder can be achieved without crosslinking, and the product has a smooth appearance without cracking.
[0062] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a non-crosslinked, highly flexible neutron shielding material, characterized in that, Includes the following steps: a) The boron carbide powder and the surface modifier are dispersed evenly in the presence of a solvent, and the solvent is dried to obtain the treated powder; b) The processed powder obtained in step a) is mixed with the polymer substrate and molded to obtain a non-crosslinked, highly flexible neutron shielding material. The boron carbide powder mentioned in step a) has a particle size of 100 mesh to 500 mesh; The surface modifier mentioned in step a) is selected from anionic surfactants and / or nonionic surfactants; The polymer substrate mentioned in step b) is selected from ethylene-polyvinyl acetate copolymer, ethylene-octene block copolymer or polyolefin elastomer; The amount of boron carbide powder used is 50% to 85% of the total mass of the polymer substrate and the boron carbide powder; The amount of the surface modifier is 0.1% to 3.5% of the total mass of the polymer substrate and boron carbide powder.
2. The preparation method according to claim 1, characterized in that, The solvent mentioned in step a) is ethanol or water; the amount of solvent used is 20ml to 80ml per 100g of boron carbide powder.
3. The preparation method according to claim 1, characterized in that, The dispersion method described in step a) is ball milling or high-speed stirring; the dispersion speed is 200 rpm to 400 rpm, and the time is 1 h to 3 h.
4. The preparation method according to claim 1, characterized in that, The temperature of the drying solvent in step a) is 80℃~120℃, and the time is 8h~10h.
5. The preparation method according to claim 1, characterized in that, The mixing method described in step b) is either internal mixing or open mixing; the mixing temperature is 80℃~120℃, and the time is 5min~20min.
6. The preparation method according to claim 1, characterized in that, The molding method described in step b) is direct molding or compression molding; the molding temperature is 100℃~120℃, the pressure is 2MPa~10MPa, and the time is 300s~600s.
7. A non-crosslinked, highly flexible neutron shielding material, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 6.
Citation Information
Patent Citations
Soft low-hydrogen neutron shielding material and preparation method thereof
CN108250557A
Ultra-thin neutron radiation preventive composite shielding material and preparation method thereof
CN102693767A
Radiation protection material
CN109545415A