Biaxially stretched polyester film and secondary battery separator including the thereof

By adjusting the mixing ratio of inorganic particles and polyester resin and optimizing the winding conditions, the prepared biaxially stretched polyester film solved the problem of wrinkle transfer during the winding process of polyester film, ensuring the quality and stability of the secondary battery separator.

CN117222698BActive Publication Date: 2026-11-17TORAY ADVANCED MATERIALS KOREA INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280031540.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-05-18
Filing Date
2022-05-04
Publication Date
2026-11-17
Estimated Expiration
2042-05-04

AI Technical Summary

Technical Problem

Existing polyester films are prone to wrinkling over time when wound into rolls, which can then transfer to the secondary battery separator, affecting the separator quality.

Method used

Biaxially stretched polyester films were prepared to prevent wrinkles by adjusting the average particle size and content of inorganic particles and the mixing ratio of polyester resin, and by optimizing winding conditions such as winding tension, winding face pressure and winding speed.

Benefits of technology

It effectively prevents wrinkles from forming in the polyester film during the winding process, ensuring the quality of the secondary battery separator, avoiding the transfer of wrinkles to the separator, and improving the stability and production efficiency of the separator.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117222698B_ABST
    Figure CN117222698B_ABST
Patent Text Reader

Abstract

The biaxially stretched polyester film of the present invention is a biaxially stretched polyester film comprising inorganic particles and polyester resin. After the master roll containing the biaxially stretched polyester film is slit, it is rewound at a winding tension of 6.5 kg / m to 8.5 kg / m, a winding surface pressure of 35 kg / m to 50 kg / m, and a winding speed of 300 m / min to 350 m / min. The hardness of the roll is 90 to 95 points, which can prevent wrinkles from forming over time while it is wound. Therefore, when used as a sandwich liner for a secondary battery separator, it can prevent wrinkles from transferring to the separator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a biaxially stretched polyester film, and more specifically, to a biaxially stretched polyester film with redesigned surface properties and optimized winding conditions, thereby preventing wrinkles that occur over time from transferring onto the secondary battery separator when used as a sandwich liner for a secondary battery separator, and a secondary battery separator comprising the thereof. Background Technology

[0002] In recent years, as part of environmental protection and carbon dioxide emission reduction policies, electric vehicles are replacing internal combustion engine vehicles that use gasoline or diesel fuel. Consequently, the demand for electric vehicles is gradually expanding, and their adoption rate is continuously increasing. As mentioned above, with the increasing adoption rate of electric vehicles, the demand for essential secondary batteries is rapidly increasing, and the secondary battery market is also growing rapidly.

[0003] The aforementioned secondary battery is a battery composed of one or more rechargeable and dischargeable electrochemical cells. It can be used multiple times through recharging, making it convenient to use and environmentally friendly because it does not generate battery waste. Generally, a secondary battery consists of an anode and a cathode that determine the battery capacity and voltage and enable current flow, an electrolyte that acts as a medium to facilitate the movement of ions, and a separator that prevents contact between the anode and cathode.

[0004] In addition, as part of the secondary battery manufacturing process, the separators (PE material, soft) used in secondary batteries are coated with a safety reinforced separator (SRS) coating. During the rewinding process after coating, adhesion may occur between the separators. Therefore, a polyester film is inserted between the separators as an interlayer liner and bonded together to prevent the separators from sticking together during rewinding.

[0005] However, if the polyester film used as the interlayer liner has severe wrinkles, these wrinkles will transfer to the separator, which is a soft material, leading to a deterioration in the separator's quality. In particular, while existing polyester films are wrinkle-free when freshly produced in rolls, their durability is poor, causing air inside the film to be trapped and wrinkled. These wrinkles in the polyester film are then transferred to the separator, significantly affecting its quality.

[0006] Therefore, there is an urgent need to prevent the polyester film used in the sandwich liner of secondary battery separators from wrinkling over time and transferring it onto the separator.

[0007] Existing technical documents

[0008] Patent documents

[0009] (Patent Document 001) Korean Patent Publication No. 10-2018-0077585 Summary of the Invention

[0010] Technical issues

[0011] The present invention was developed to solve the above-mentioned problems. The purpose of the present invention is to provide a biaxially stretched polyester film that can prevent wrinkles from forming over time when the polyester film is wound into a roll after production, and a secondary battery separator including the thereof.

[0012] The above and other objects and advantages of the present invention will become more apparent from the following description of preferred embodiments.

[0013] Solution to the problem

[0014] The above objective is achieved by a biaxially stretched polyester film, which is a biaxially stretched polyester film comprising inorganic particles and polyester resin. The roll containing the biaxially stretched polyester film is slit and then rewound at a winding tension of 6.5 kg / m to 8.5 kg / m, a winding surface pressure of 35 kg / m to 50 kg / m, and a winding speed of 300 m / min to 350 m / min. The hardness of the resulting roll is 90 to 95 points.

[0015] Preferably, the average particle size of the inorganic particles can be from 3.0 μm to 5.0 μm.

[0016] Preferably, the content of inorganic particles can be from 0.0008% by weight to 0.0015% by weight.

[0017] Preferably, the centerline average roughness SRa of the biaxially stretched polyester film can be 40 nm to 80 nm, and the ten-point average roughness SRz can be 800 nm to 1300 nm.

[0018] Preferably, the maximum roughness SRmax of the biaxially stretched polyester film can be from 1100 nm to 1800 nm.

[0019] Preferably, the haze of the biaxially stretched polyester film can be 4% or higher.

[0020] Preferably, the biaxially stretched polyester film has a peak count of 0.1 mm in the surface SPC. 2 The number of protrusions with a height of 0.15μm or more within the area can be more than 100.

[0021] Preferably, the inorganic particles can be silicon dioxide particles.

[0022] Preferably, the thickness of the biaxially stretched polyester film can be from 10 μm to 16 μm.

[0023] Furthermore, the aforementioned objective is achieved by using the biaxially stretched polyester film as a sandwich liner for a secondary battery separator.

[0024] Furthermore, the above objective is achieved by a secondary battery separator comprising the aforementioned biaxially stretched polyester film and a secondary battery comprising the same.

[0025] The effects of the invention

[0026] According to an embodiment of the present invention, the biaxially stretched polyester film allows air inside the wound film roll to escape smoothly by redesigning the surface properties of the polyester film and optimizing the winding conditions, so that wrinkles will not occur over time after film production and wrinkles caused by internal air will not appear during winding.

[0027] Furthermore, according to the present invention, since wrinkles do not occur over time, when used as a sandwich liner for a secondary battery separator, wrinkles will not transfer to the separator, thereby preventing quality problems caused by wrinkles during separator bonding processing, improving the quality of the secondary battery separator, and enabling a stable supply of products.

[0028] Furthermore, according to the present invention, when used as a sandwich liner for a secondary battery separator, wrinkles do not transfer to the separator, thus providing a secondary battery including a high-efficiency secondary battery separator, etc.

[0029] However, the effects of the present invention are not limited to those described above. Other effects not mentioned will be clearly understood by those skilled in the art from the following description. Attached Figure Description

[0030] Figure 1 This is a schematic cross-sectional view of a biaxially stretched polyester film according to an embodiment of the present invention. Detailed Implementation

[0031] The embodiments of the present invention will be described in detail with reference to the accompanying drawings to enable those skilled in the art to readily implement the invention. However, the present invention can be implemented in many different ways and is not limited to the embodiments described in this specification.

[0032] In the accompanying drawings, the thickness of each component shown is enlarged to more clearly illustrate the various layers and regions. Throughout the specification, the same reference numerals are used for identical or similar components. The expression "on" or "above" another component, such as referring to a layer, film, region, or plate, indicates not only that the component is placed "directly" on or "straight above" the other component, but also that another component is placed between the two components. Conversely, when one component is placed "straight above" another component, it means that there are no other components in between.

[0033] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In the event of any conflict, the specification including the definitions shall prevail. Although similar or equivalent methods and materials to those described herein may be used in the practice or testing of embodiments of the invention, suitable methods and materials are described below.

[0034] A biaxially stretched polyester film according to an embodiment of the present invention aims to provide a film that improves wrinkles that occur over time by adjusting the size of the inorganic particles used in the film preparation and changing the winding process conditions. The invention will be described in more detail below.

[0035] Figure 1 This is a schematic cross-sectional view of a biaxially stretched polyester film according to an embodiment of the present invention.

[0036] Reference Figure 1 According to an embodiment of the present invention, a biaxially stretched polyester film includes inorganic particles 100 and polyester resin 200 to have a structure in which the inorganic particles 100 are dispersed in the polyester resin 200.

[0037] The inorganic particles 100 used in this invention preferably contain silicon dioxide (SiO2), borosilicate, aluminosilicate and aluminum oxide, and more preferably contain silicon dioxide particles.

[0038] In one embodiment, the average particle size of the inorganic particles 100 is preferably 3.0 μm to 5.0 μm. When inorganic particles 100 with an average particle size of less than 3.0 μm are used, wrinkles become more severe during winding, and air is difficult to escape when the particles are rolled up, leading to wrinkles over time. Conversely, if the average particle size of the inorganic particles 100 exceeds 5.0 μm, the large particles press against each other between the membrane layers, causing the pressure in the filter to increase rapidly during membrane fabrication, resulting in increased production losses.

[0039] In one embodiment, the content of inorganic particles 100 is preferably 0.0008% to 0.0015% by weight relative to 100% of the entire biaxially stretched polyester film. If the content of inorganic particles 100 is less than 0.0008% by weight, the air layer between the film layers becomes insufficient, resulting in surface protrusions in certain portions of the film. These surface protrusions accumulate, making the protrusions on the wound roll more severe, leading to poor processing and reduced winding properties, thus increasing wrinkles in the MD direction during winding. Conversely, if the content of inorganic particles 100 exceeds 0.0015% by weight, defects arise due to the increase of foreign matter caused by particle aggregation, resulting in film rupture due to particles during stretching.

[0040] In one embodiment, the polyester resin 100 constituting the biaxially stretched polyester film can be formed by polymerizing dicarboxylic acid and diol, and may include polyethylene terephthalate (PET).

[0041] The dicarboxylic acids may include aromatic dicarboxylic acids such as terephthalic acid, naphthalenedicarboxylic acid, isophthalic acid, diphenylcarboxylic acid, diphenyl sulfone dicarboxylic acid, diphenoxyethane dicarboxylic acid, 5-sodium sulfone dicarboxylic acid, and phthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; and oxidized carboxylic acids such as p-hydroxybenzoic acid. Furthermore, as diols, aliphatic diols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, and neopentanediol can be used; polyoxyethylene diols such as diethylene glycol, polyethylene glycol, and polypropylene glycol; alicyclic diols such as cyclohexanediol; and aromatic diols such as bisphenol A and bisphenol S.

[0042] In one embodiment, the centerline average roughness SRa of the biaxially stretched polyester film according to an embodiment of the present invention is preferably 40 nm to 80 nm. If the centerline average roughness SRa is less than 40 nm, the space for air to escape between each layer during film stacking is small, resulting in wrinkles over time. If the centerline average roughness SRa is greater than 80 nm, the filter pressure increases during production due to excessive particle input, leading to reduced productivity.

[0043] In one embodiment, the ten-point average roughness SRz of the biaxially stretched polyester film is preferably between 800 nm and 1300 nm. If the ten-point average roughness SRz is less than 800 nm, the space for air to escape between each layer during film stacking is small, leading to wrinkles over time. If the ten-point average roughness SRz is greater than 1300 nm, the filter pressure increases during production due to excessive particle input, resulting in reduced productivity.

[0044] In one embodiment, the maximum roughness SRmax of the biaxially stretched polyester film is preferably between 1100 nm and 1800 nm. If the maximum roughness SRmax is less than 1100 nm, the space for air to escape between each layer during film stacking is small, resulting in wrinkles over time. If the maximum roughness SRmax is greater than 1800 nm, the filter pressure increases during production due to the introduction of too many particles, leading to a decrease in productivity.

[0045] In one embodiment, the haze of the biaxially stretched polyester film is preferably 4% or higher. If the haze is below 4%, the corresponding particle content is low, thus hindering air escape and causing wrinkles to form over time.

[0046] In one embodiment, the biaxially stretched polyester film has a peak count of 0.1 mm in the surface SPC. 2The number of protrusions with a height of 0.15 μm or more within the area is preferably 100 or more. If the number of protrusions is less than 100, the space for air to escape between the layers is small when the films are stacked, and wrinkles will occur over time.

[0047] In one embodiment, the thickness of the biaxially stretched polyester film is preferably between 10 μm and 16 μm. If the thickness is less than 10 μm, wrinkles will form during winding, and air escape will be hindered, leading to wrinkles over time. However, the thicker the biaxially stretched polyester film, the less likely it is to wrinkle over time; therefore, there is no limitation on the aforementioned upper limit.

[0048] A method for preparing a biaxially stretched polyester film according to an embodiment of the present invention includes: a first step of mixing inorganic particles with polyester resin, extruding and biaxially stretching them to prepare a master roll; a second step of slitting the master roll into a predetermined width; and a third step of rewinding the master roll with a predetermined winding tension, winding surface pressure and winding speed to prepare a rewound biaxially stretched polyester film roll.

[0049] First, in the first step of preparing a master roll by mixing inorganic particles with polyester resin, extruding, and biaxially stretching, inorganic particles are added to the polyester resin, mixed, extruded, and biaxially stretched in the MD and TD directions to prepare a biaxially stretched polyester film. At this time, the average particle size of the inorganic particles is preferably 3.0 μm to 5.0 μm, and the content of inorganic particles relative to 100% by weight of the entire biaxially stretched polyester film is preferably 0.0008% by weight to 0.0015% by weight. Furthermore, for ease of subsequent processes, it is preferable to wind the polyester film prepared in the first step into a master roll.

[0050] Secondly, in the second step of slitting the aforementioned master roll to a predetermined width, the polyester film wound in the form of a master roll is slit to the required width, i.e., the width required by the user. At this point, there is no particular limitation on the width of the polyester film achieved by slitting, and it can be freely adjusted according to the intended use of the polyester film and the needs of the company that requires it.

[0051] Secondly, the third step in preparing a rewound biaxially stretched polyester film roll by rewinding with predetermined winding tension, winding face pressure, and winding speed involves rewinding a polyester film of predetermined width by cutting it at a winding tension of 6.5 kg / m to 8.5 kg / m, a winding face pressure of 35 kg / m to 50 kg / m, and a winding speed of 300 m / min to 350 m / min. This prevents wrinkles from forming over time when the biaxially stretched polyester film is rewound under the above conditions.

[0052] Meanwhile, the second and third steps can be performed as separate processes. For the sake of process convenience, there can be a process form in which the third step is performed simultaneously during the slitting process of the second step.

[0053] In the above method for preparing biaxially stretched polyester film, the steps related to... Figure 1 The same repeating content as the biaxially stretched polyester film.

[0054] In one embodiment, when the master roll wound with the biaxially stretched polyester film is slitting and rewound for delivery to the user, the final wound roll with a winding tension of 6.5 kg / m to 8.5 kg / m, a winding surface pressure of 35 kg / m to 50 kg / m, and a winding speed of 300 m / min to 350 m / min preferably has a hardness of 90 to 95 points. If the roll hardness is less than 90 points, the roll sags and transverse wrinkles appear in the width direction of the film; if the roll hardness is greater than 95 points, wrinkles will occur over time.

[0055] When rewinding as described above, if the winding tension is less than 6.5 kg / m and the winding surface pressure is less than 35 kg / m, transverse wrinkles will appear when winding the master roll due to the tension and surface pressure, and the winding section will fall off, resulting in abnormal winding and inability to produce products. Conversely, if the winding tension is greater than 8.5 kg / m and the winding surface pressure is greater than 50 kg / m, the increase in the amount of air entering between different film layers will accelerate the occurrence of wrinkles.

[0056] In addition, if the winding speed is less than 300 m / min, the hardness of the roll increases, which causes wrinkles over time. If the winding speed is greater than 350 m / min, the winding speed becomes too fast, the amount of air entering between different film layers increases, and the occurrence of wrinkles is accelerated.

[0057] As described above, according to an embodiment of the present invention, a biaxially stretched polyester film is wound and prepared into a master roll, and when slit and rewound to be provided to the user, it is wound under the set conditions of a winding tension of 6.5 kg / m to 8.5 kg / m, a winding surface pressure of 35 kg / m to 50 kg / m, and a winding speed of 300 m / min to 350 m / min, so that the air inside the film can escape smoothly, thereby preventing wrinkles from appearing over time.

[0058] As described above, the biaxially stretched polyester film according to an embodiment of the present invention suppresses wrinkles that occur over time through the aforementioned physical properties, thereby preventing the problem of wrinkles transferring to the separator during the separator lamination process, and thus can be used as an interlayer liner for secondary battery separators.

[0059] Therefore, those skilled in the art will readily understand that the scope of the present invention also extends to biaxially stretched polyester films used as sandwich liner for secondary battery separators, secondary battery separators including the thereof, and secondary batteries including the aforementioned secondary battery separators.

[0060] The present invention will be described in more detail below through embodiments. These embodiments are provided for illustrative purposes only, and the scope of the invention is not limited to these embodiments.

[0061] [Example]

[0062] [Example 1]

[0063] 0.00087 wt% of inorganic particles (SiO2) with an average particle size of 3.75 μm and 99.99913 wt% of polyester resin (PET A9039, Toray Advanced Materials Co., Ltd.) were mixed. Next, the mixed polyester resin was vacuum dried, melted in an extruder at a temperature of 275°C to 285°C, extruded through a feed section using a T-die, and then bonded to a casting drum on cooling rollers by electrostatic application (pinning). An unstretched sheet was obtained through cooling and solidification. This sheet was then uniaxially stretched (longitudinal stretching) by the difference in circumferential speed between rollers on rollers heated to or above the glass transition temperature of the sheet. At this point, the longitudinal stretching ratio was 4.5 times. Next, after uniaxial stretching, a biaxial stretching ratio of 4.1 times was performed in the transverse direction perpendicular to the longitudinal direction. At this point, based on the tenter frame, the stretching temperature in the initial stage of the stretching zone is set to 100°C to 120°C, the stretching temperature in the middle stage of the stretching zone is set to 120°C to 140°C, and the temperature in the stretching heat setting zone is set to 200°C to 240°C.

[0064] The polyester film master roll is prepared as described above, and the thickness of the biaxially stretched polyester film is 12 μm.

[0065] Next, the prepared polyester film masterbatch is cut into 1,120 mm widths and then wound again with a winding tension of 7.6 kg / m, a winding surface pressure of 48 kg / m, and a winding speed of 340 m / min to prepare a biaxially stretched polyester film roll.

[0066] [Example 2]

[0067] Except that the inorganic particle content was 0.0008% by weight, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0068] [Example 3]

[0069] Except that the inorganic particle content was 0.0015% by weight, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0070] [Example 4]

[0071] Except that the size of the inorganic particles is 3 μm, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0072] [Example 5]

[0073] Except that the size of the inorganic particles is 5 μm, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0074] [Example 6]

[0075] Except for the winding tension of 6.5 kg / m, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0076] [Example 7]

[0077] Except for the winding tension of 8.5 kg / m, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0078] [Example 8]

[0079] Except for the winding surface pressure of 35 kg / m, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0080] [Example 9]

[0081] Except for the winding surface pressure of 50 kg / m, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0082] [Comparative Example]

[0083] [Comparative Example 1]

[0084] Except that the size of the inorganic particles was 2.9 μm, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0085] [Comparative Example 2]

[0086] Except that the inorganic particle content was 0.0016% by weight, biaxially stretched polyester film rolls were prepared using the same method as in Comparative Example 1.

[0087] [Comparative Example 3]

[0088] Except that the size of the inorganic particles was 5.1 μm, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0089] [Comparative Example 4]

[0090] Except that the inorganic particle content was 0.0007% by weight, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0091] [Comparative Example 5]

[0092] Except that the inorganic particle content was 0.0016% by weight, the membrane was prepared using the same method as in Example 1.

[0093] [Comparative Example 6]

[0094] Except for the winding tension of 8.6 kg / m, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0095] [Comparative Example 7]

[0096] Except for the winding tension of 6.4 kg / m, the membrane was prepared using the same method as in Example 1.

[0097] [Comparative Example 8]

[0098] Except for the winding surface pressure of 51 kg / m, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0099] [Comparative Example 9]

[0100] Except for the winding surface pressure of 34 kg / m, the membrane was prepared using the same method as in Example 1.

[0101] [Comparative Example 10]

[0102] Except for the winding speed of 290 m / min, biaxially stretched polyester film rolls were prepared using the same method as in Example 1.

[0103] The physical properties of the biaxially stretched polyester film rolls prepared in Examples 1 to 9 and Comparative Examples 1 to 10 were evaluated by the following experimental examples, and the results are shown in Table 1.

[0104] [Experimental Example]

[0105] (1) Evaluation of wrinkles that develop over time

[0106] The film rolls wound with the biaxially stretched polyester film prepared according to the examples and comparative examples were packaged and stored. After 2 days, the packaging was unpacked and the surface condition of the wound rolls was visually inspected to determine whether wrinkles had appeared. At this time, the length of the wound film was 8,200 m, and it was evaluated as follows.

[0107] Good: No wrinkles develop over time across the entire width of the membrane.

[0108] Poor: Time-related wrinkles occur across the entire width of the membrane.

[0109] (2) The hardness of the rolled coil

[0110] According to the JIS K 7312 standard, a precision hardness tester (model: Type C) manufactured by ASKER was placed on the surface of the wound film roll and the hardness of the left and right ends of the roll was measured once each to determine the hardness value.

[0111] (3) Measurement of SRa, SRz, and SRmax (membrane surface roughness)

[0112] The SRa, SRz, and SRmax values ​​of a single film surface were measured using a three-dimensional surface roughness measuring instrument (model: SE3500K) manufactured by Kosaka Laboratory Ltd.

[0113] (4) Number of SPC protrusions

[0114] The SPC (Peak Count) of a single film surface was measured using a three-dimensional surface roughness measuring instrument (model: SE3500K) manufactured by Kosaka Research Institute Co., Ltd., and the result was calculated at a depth of 0.1 mm. 2 The number of protrusions with a height of 0.15 μm or more within the measurement area.

[0115] (5) Haze measurement

[0116] The haze of a membrane was measured using a haze meter (model: COH-300A) from NIPPON DENSHOKU INDUSTRIES Co.,LTD.

[0117] Table 1

[0118] Classification wrinkles of age Roll hardness SRa SRz SRmax SPC protrusion count Haze Example 1 good 92 53nm 825nm 1218nm 160 4.40% Example 2 good 91 51nm 812nm 1433nm 143 4.10% Example 3 good 90 67nm 1239nm 1580nm 250 5.50% Example 4 good 94 48nm 807nm 1175nm 128 4.20% Example 5 good 90 75nm 1222nm 1753nm 200 6.10% Example 6 good 91 53nm 825nm 1218nm 160 4.40% Example 7 good 94 53nm 825nm 1218nm 160 4.40% Example 8 good 91 53nm 825nm 1218nm 160 4.40% Example 9 good 93 53nm 825nm 1218nm 160 4.40% Comparative Example 1 Difference 97 41nm 802nm 1027nm 90 3.90% Comparative Example 2 Difference 96 45nm 825nm 1099nm 160 5.20% Comparative Example 3 good 88 81nm 1312nm 1826nm 263 5.90% Comparative Example 4 Difference 96 39nm 799nm 1065nm 92 3.90% Comparative Example 5 good 88 62nm 1236nm 1335nm 123 5.30% Comparative Example 6 Difference 96 53nm 825nm 1218nm 160 4.40% Comparative Example 8 Difference 97 53nm 825nm 1218nm 160 4.40% Comparative Example 10 Difference 96 53nm 825nm 1218nm 160 4.40%

[0119] As shown in Table 1, in Examples 1 to 9, it can be confirmed that adding 0.0008% to 0.0015% by weight of inorganic particles with an average particle size of 3.0 μm to 5.0 μm to polyester resin and extruding and biaxially stretching to form a master roll of polyester film, and then slitting and rewinding it, by setting the winding tension to 6.5 kg / m to 8.5 kg / m, the winding surface pressure to 35 kg / m to 50 kg / m, and the winding speed to 300 m / min to 350 m / min to prepare a rewound roll, can provide a biaxially stretched polyester film that improves wrinkles that occur over time.

[0120] On the other hand, in the case of Comparative Example 1, it can be seen that wrinkles occur over time due to the small size of inorganic particles and high roll hardness. If SRmax is below the minimum range, the number of protrusions is less than 100, and the haze is less than 4%.

[0121] Furthermore, it can be seen that although more small-sized inorganic particles were added in Comparative Example 2, the roll was hard, wrinkled over time, and SRmax was below the minimum range.

[0122] In addition, in Comparative Example 3, it can be seen that due to the excessive size of the inorganic particles, SRa, SRz and SRmax all exceed the maximum value, and the physical properties of the prepared film become soft due to the low hardness of the roll, causing it to sink to the bottom and resulting in winding defects.

[0123] In addition, in Comparative Example 4, the size of the inorganic particles was the same as in Example 1, but only 0.0007% by weight of inorganic particles less than the standard content was added. Therefore, SRa, SRz and SRmax were all less than the minimum value, the number of protrusions was less than 100, the haze was less than 4%, and wrinkles occurred over time due to the excessive hardness of the roll.

[0124] In addition, in Comparative Example 5, the roll stiffness was too low, causing the membrane to soften and sag towards the bottom, resulting in a winding defect. Furthermore, the pressure of the filter increased excessively during the production process, reducing productivity.

[0125] In addition, in Comparative Example 6, the winding tension after slitting was set to a higher 8.6 kg / m, which increased the hardness of the roll and caused wrinkles to form over time.

[0126] In addition, in Comparative Example 8, the winding tension was the same as in Example 1, but because the winding surface pressure was set higher, the hardness of the roll increased, and wrinkles occurred over time.

[0127] In addition, in Comparative Example 10, the roll hardness increased due to the low winding speed, and wrinkles appeared over time accordingly.

[0128] In particular, apart from those shown in Table 1, in Comparative Examples 7 and 9 where the winding tension or winding surface was low, it was confirmed that winding defects such as poor winding cross-section, extrusion, and folding occurred when the film was wound after preparation.

[0129] The preferred embodiments of the present invention have been described in detail above, but the scope of the present invention is not limited thereto. Various modifications and improvements made by those skilled in the art based on the basic concepts of the present invention as defined in the appended claims are also within the scope of the present invention.

Claims

1. A biaxially stretched polyester film, comprising inorganic particles and polyester resin, characterized in that, After slitting the master roll containing the biaxially stretched polyester film, the roll is rewound at a winding tension of 6.5 kg / m to 8.5 kg / m, a winding surface pressure of 35 kg / m to 50 kg / m, and a winding speed of 300 m / min to 350 m / min. The resulting roll has a hardness of 90 to 95 points. The content of the aforementioned inorganic particles is from 0.0008% to 0.0015% by weight, and The average particle size of the aforementioned inorganic particles is 3.0 μm to 5.0 μm.

2. The biaxially stretched polyester film according to claim 1, characterized in that, The centerline average roughness SRa of the above-mentioned biaxially stretched polyester film is 40 nm to 80 nm, and the ten-point average roughness SRz is 800 nm to 1300 nm.

3. The biaxially stretched polyester film according to claim 2, characterized in that, The maximum roughness SRmax of the biaxially stretched polyester film is 1100 nm to 1800 nm.

4. The biaxially stretched polyester film according to claim 1, characterized in that, The haze of the above-mentioned biaxially stretched polyester film is above 4%.

5. The biaxially stretched polyester film according to claim 1, characterized in that, The aforementioned biaxially stretched polyester film showed a peak count of 0.1 mm in surface SPC. 2 The number of protrusions with a height of 0.15μm or more within the area is more than 100.

6. The biaxially stretched polyester film according to claim 1, characterized in that, The aforementioned inorganic particles are silicon dioxide particles.

7. The biaxially stretched polyester film according to claim 1, characterized in that, The thickness of the biaxially stretched polyester film is 10 μm to 16 μm.

8. The biaxially stretched polyester film according to any one of claims 1 to 7, characterized in that, The aforementioned biaxially stretched polyester film is used as a sandwich liner for secondary battery separators.

9. A secondary battery separator, characterized in that, Includes biaxially stretched polyester film according to any one of claims 1 to 7.

10. A secondary battery, characterized in that, Includes the secondary battery separator according to claim 9.

Citation Information

Patent Citations

  • Biaxial stretched polyester film and manufacturing method thereof

    KR1020180077585A

  • Biaxially oriented polyester film roll

    WO2020090673A1