Polyamide 56 resin composition, fibers, fiber bundles, fiber twists, fiber products and tire cord fabrics
By incorporating a polymer crystallization modifier into polyamide 56 resin, the fiber crystallization morphology was controlled, solving the problem of insufficient rigidity of polyamide 56 fibers, realizing the preparation of high-modulus fibers, and expanding their application range.
Patent Information
- Application Number
- CN202210679669.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-06-15
AI Technical Summary
Existing technologies have failed to effectively improve the Young's modulus of polyamide 56 fiber, resulting in insufficient rigidity, which limits its application areas and poses safety hazards.
By mixing polymeric crystallization modifiers, such as polyamide 66 resin, polyamide 46 resin, or cholesterol liquid crystal polymers, into polyamide 56 resin, the fiber crystallization morphology can be controlled, causing it to grow along a specific direction and increasing Young's modulus.
It significantly improves the Young's modulus of polyamide 56 fiber, addresses its insufficient rigidity, and expands its application range.
Smart Images

Figure CN117264410B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a polyamide 56 resin composition, polyamide 56 fiber, polyamide 56 fiber tow, and polyamide 56 fiber products, with the primary objective of improving the fiber modulus of polyamide 56 resin. Background Technology
[0002] The known polyamide 56 has an asymmetric crystalline structure and a slow crystallization rate, resulting in insufficient fiber strength and modulus after processing and spinning. Numerous precedents have been taught for improving the strength of polyamide 56 fibers, such as adjusting the spinning process or using inorganic nucleating agents to increase crystallinity to obtain high-strength fibers. However, regarding the technology for improving the modulus of polyamide 56, the industry has not yet proposed a suitable solution.
[0003] Polyamide 56 fiber has been gradually applied in industrial applications, such as tire cord fabric, conveyor belts, airbags, and ground fabrics. However, the insufficient modulus of polyamide 56 fiber may result in low material rigidity, limiting its application areas and leading to safety concerns.
[0004] To further explain, high-strength fibers do not necessarily possess high rigidity (high modulus). For example, rubber bands are difficult to break; a very large force is required to snap them (a manifestation of high strength), but they are very easy to stretch, requiring only a small force to deform (a manifestation of low modulus and low rigidity). Therefore, rigidity is often mistakenly understood as strength. The specific term for fiber rigidity is "Young's modulus," which is the ratio of stress to strain, indicating how easily the fiber deforms under a certain load. It reflects the range of deformation a fiber material can undergo under stress. However, fiber strength refers to the magnitude of the force that can be applied to the material before it breaks; it reflects the amount of force the fiber material can withstand before fracture. Therefore, fiber rigidity (modulus) and fiber strength are different physical concepts.
[0005] The main improvement of polyamide 56 fiber breaking strength is achieved through the spinning process. In addition, the composition of polyamide 56 can be changed by adding nucleating agents or other additives to increase the crystallization rate. The main purpose is to enable the plastic products to cool quickly after injection molding, thereby improving production efficiency. However, if the nucleating agent or the addition ratio is not suitable for the spinning process, it can easily lead to a decrease in fiber performance and breakage.
[0006] Patents CN111411405A, CN106835329B, and CN106868624B disclose a high-strength polyamide 56 filament and its preparation method, with the aim of improving the fiber's breaking strength. Patents CN113668076A and JP200968132 disclose a polyamide 56 fiber and tire cord fabric (tire cord fabric), with the technology focusing on adjusting spinning process parameters and improving the spinning process. Patent CN109666294A discloses a polyamide 56 composition with improved crystallization rate. Polyamides often use copper salts as heat stabilizers; adding copper salts to the polyamide 56 composition at an amount of 0.05~0.15wt% increases the composition's crystallization rate, making it suitable for preparing plastic products. Patent CN111518269A discloses a rapidly crystallizing polyamide 5X resin and its preparation method. It involves adding a nucleating agent during polymerization to accelerate the cooling crystallization rate and crystallinity. The resin, for example, contains a polyamide polymer nucleating agent, which is added during the polymerization stage in the form of an aqueous suspension (0.001%–0.02% by weight). This patent states that adding the nucleating agent during polymerization, compared to adding it later, has the advantages of requiring a smaller amount and achieving better crystallization. In other words, this patent excludes the possibility of using the nucleating agent in blending processes. Patent CN111826737A discloses a method for preparing polyamide 56 industrial yarn for airbags. The technique involves adding a nucleating agent during polymerization to accelerate the crystallization rate. Its key feature is the formation of more numerous and smaller spherulites during polymer cooling to promote crystallization and maintain fiber strength. The purpose of adding the nucleating agent in CN111826737A is to reduce the initial modulus of the fiber. However, fiber spinning involves stretching after melting and cooling. The stretching induces crystallization as the molecular chains align in the correct direction. This specific orientation (along the fiber's long axis) of the crystals during stretching is crucial in determining the fiber's modulus. If non-directional spherulites form before fiber stretching, stretching will hinder the growth of molecular chains along a specific direction, disrupting the orientation and leading to fiber breakage, resulting in poor modulus or even preventing production. Furthermore, the desired crystallization pattern for fibers is one that does not produce spherulites after melting and cooling, and the crystallization rate must be controlled. Too fast a crystallization rate easily leads to spherulites; too slow a rate results in low and incomplete crystallinity, both detrimental to fiber properties. Therefore, controlling the crystallization rate within a suitable range is a prerequisite for achieving high modulus in fibers. Summary of the Invention
[0007] None of the aforementioned patents have provided a suitable solution for improving the Young's modulus of polyamide 56 fibers. Therefore, this invention relates to a high-modulus polyamide 56 fiber, which is made by blending a polymeric crystallization modifier to enable the fiber crystallization morphology to grow in a specific direction (the long axis direction of the fiber), thereby achieving the purpose of improving the Young's modulus and improving the application problems caused by insufficient modulus (i.e., low rigidity) of the finished fiber.
[0008] According to various embodiments of the present invention, a polyamide 56 resin composition is provided, comprising polyamide 56 resin and a polymer crystallization morphology modifier. The polyamide 56 resin composition has a relative viscosity of about 40-100 in a 90% weight formic acid concentration, and the crystallization half-cycle t measured by differential scanning calorimetry is... 1 / 2 Less than approximately 1.5 minutes.
[0009] According to certain embodiments of the present invention, the polyamide 56 resin accounts for 80.0 to 99.9 wt% of the total weight of the polyamide 56 resin composition, and the polymer crystallization modifier accounts for 0.1 to 20.0 wt% of the total weight of the polyamide 56 resin composition.
[0010] According to certain embodiments of the present invention, the polymer crystallization morphology regulator is selected from polyamide crystallization morphology regulators, liquid crystal polymer crystallization morphology regulators, or combinations thereof.
[0011] According to certain embodiments of the present invention, the polyamide crystallization modifier is selected from polyamide 66 resin, polyamide 46 resin, or a combination thereof.
[0012] According to certain embodiments of the present invention, the liquid crystal polymer crystallization morphology regulator includes cholesterol liquid crystal polymers.
[0013] According to certain embodiments of the present invention, the polyamide 56 resin composition further includes an oxidant, a catalyst, a processing aid, a polyester polymer, or a combination thereof.
[0014] According to various embodiments of the present invention, a polyamide 56 fiber is provided, which is obtained by spinning the above-mentioned polyamide 56 resin composition.
[0015] According to certain embodiments of the present invention, polyamide 56 fibers have a fineness of about 75D to about 840D, and a crystallization half-cycle t measured by differential thermal scanning spectroscopy. 1 / 2 The fiber fineness is 75D, and its crystallization half-cycle is t. 1 / 2 Less than approximately 0.5 minutes, the fiber fineness is 420D, and its crystallization half-cycle is t. 1 / 2 Less than approximately 0.6 minutes, with a fiber fineness of 840D and a crystallization half-cycle of t. 1 / 2 Less than approximately 0.7 minutes.
[0016] According to certain embodiments of the present invention, the monofilament fineness of polyamide 56 fiber is 3 to 7.5 DPF.
[0017] According to certain embodiments of the present invention, the fineness of the polyamide 56 fiber is 420 D, and the stress modulus of the polyamide 56 fiber is about 2.9 N to about 3.1 N at a specified elongation of 2% (LASE 2%).
[0018] According to certain embodiments of the invention, the polyamide 56 fiber has a fineness of 420 D, and the polyamide 56 fiber has a stress modulus of about 5.5 N to about 6.0 N at a specific elongation of 5% (LASE 5%).
[0019] According to certain embodiments of the invention, the polyamide 56 fiber has a fineness of 420 D and a stress modulus of about 16.0 N to about 17.0 N at a specific elongation of 10% (LASE 10%).
[0020] According to certain embodiments of the invention, the polyamide 56 fiber has a fineness of 840D and a stress modulus of about 5.5 N to about 6.2 N at a specific elongation of 2% (LASE 2%).
[0021] According to certain embodiments of the invention, the polyamide 56 fiber has a fineness of 840D and a stress modulus of about 11.0 N to about 12.5 N at a specific elongation of 5% (LASE 5%).
[0022] According to certain embodiments of the invention, the polyamide 56 fiber has a fineness of 840D and a fiber stress modulus of about 32.0 N to about 38.0 N at a specific elongation of 10% (LASE 10%).
[0023] According to various embodiments of the present invention, a polyamide 56 fiber bundle is provided, which is obtained by winding up multiple of the aforementioned polyamide 56 fibers in single strands or in parallel strands during spinning.
[0024] According to certain embodiments of the present invention, the polyamide 56 fiber bundle has a fineness of 75~840D when spun as a single strand and 150D~1680D when spun as a double strand.
[0025] According to various embodiments of the present invention, a polyamide 56 fiber twisted yarn is provided, which is obtained by the aforementioned polyamide 56 fiber through a twisting and plying process, wherein two-ply twisted polyamide 56 fibers have a fineness of 150~1680D and three-ply twisted polyamide 56 fibers have a fineness of 225D~2520D.
[0026] According to various embodiments of the present invention, a polyamide 56 fiber article is provided, which is made from the aforementioned polyamide 56 fiber, wherein the polyamide 56 fiber article includes tire cord fabric, conveyor belt, automotive fiber and its fabric, tarpaulin or heat-insulating and sun-shading fabric.
[0027] According to various embodiments of the present invention, a tire cord fabric is provided, which is obtained by impregnation process of the aforementioned polyamide 56 fiber twisted yarn, wherein the tire cord fabric has a stress modulus value of about 17N to about 21N when the specific elongation is 5%, and has a stress modulus value of about 41N to about 55N when the specific elongation is 10%. Attached Figure Description
[0028] To make the above and other objects, features, advantages and embodiments of the present invention more apparent and understandable, the accompanying drawings are described in detail below:
[0029] Figure 1 A stress comparison diagram showing a specific elongation rate according to an embodiment of the present invention and a comparative example is presented.
[0030] Figure 2 for Figure 1 A magnified view of a portion of the image. Detailed Implementation
[0031] This disclosure provides a polyamide 56 resin composition comprising polyamide 56 resin and a polymer crystallization morphology modifier. The polyamide 56 resin composition has a relative viscosity (RV) of approximately 40-100 in 90% formic acid by weight, and a crystallization half-cycle t measured by a differential scanning calorimeter. 1 / 2 Less than approximately 1.5 minutes. Relative viscosity was tested at 25°C using Ubbelohde tubes with 90 wt% formic acid, according to ASTM D789. The crystallinity of the polyamide 56 resin composition will affect the properties of the polyamide 56 fibers subsequently formed from it. For example, polyamide 56 resin compositions with a crystallization half-cycle of less than 1.5 minutes can effectively increase the stress modulus of the polyamide 56 fibers formed from them.
[0032] In some embodiments, the moisture content of the polyamide 56 resin is about 300 to 800 ppm. In some embodiments, the relative viscosity of the polyamide 56 resin is about 40 to 100. In some embodiments, the polyamide 56 resin accounts for 80.0 to 99.9 wt% of the total weight of the polyamide 56 resin composition.
[0033] In some embodiments, the polymeric crystallization modifier is selected from polyamide crystallization modifiers, liquid crystal polymer crystallization modifiers, or combinations thereof. The polymeric crystallization modifier has a melting point similar to that of polyamide 56 resin. In some embodiments, the polyamide crystallization modifier is selected from polyamide 66 resin, polyamide 46 resin, or combinations thereof. In some embodiments, the liquid crystal polymer crystallization modifier includes a cholesterol liquid crystal polymer. For example, the cholesterol liquid crystal polymer may be Xydar® or Vectra®. The cholesterol liquid crystal polymer used in this disclosure is melt-processable, for example, it can be processed and used at temperatures greater than 300°C.
[0034] In some embodiments, the polymeric crystallization modifier accounts for 0.1 to 20.0 wt% of the total weight of the polyamide 56 resin composition. For example, it is about 0.2, 0.5, 1.0, 3.0, 5.0, 7.0, 9.0, 11.0, 13.0, 15.0, 17.0, or 19.0 wt%. By adding the above-mentioned amounts of polymeric crystallization modifier, the polyamide 56 resin can be induced to shorten the crystallization half-cycle t. 1 / 2 This improves the overall orientation of polyamide 56 fibers formed by melt spinning of polyamide 56 resin components, thereby significantly increasing the fiber modulus, which means that the material deformation is smaller under the same external force.
[0035] Adding excessive amounts of polymer crystallization modifiers (e.g., more than 20 wt% of polymer crystallization modifiers) can lead to problems such as a low degree of decrease in the crystallization half-cycle and / or a decrease in crystallization enthalpy.
[0036] In some embodiments, the polyamide 56 resin composition further includes an oxidant, a catalyst, a polyester polymer, processing aids (such as heat stabilizers, lubricants), or a combination thereof. In some embodiments, the polyester polymer may be polyethylene terephthalate, propylene terephthalate, or butylene terephthalate.
[0037] In some embodiments, the above-mentioned polyamide 56 resin can be mixed with the above-mentioned polymer crystallization modifier and melt-blended at about 270~300°C to obtain a polyamide 56 resin composition.
[0038] This disclosure also provides a polyamide 56 fiber, which is obtained from the above-mentioned polyamide 56 resin composition by a spinning process. In some embodiments, the polyamide 56 fiber has a fineness of about 75D to about 840D, and a crystallization half-cycle t measured by differential thermal scanning spectroscopy. 1 / 2 The fiber fineness is 75D, and its crystallization half-cycle is t. 1 / 2 Less than approximately 0.5 minutes, the fiber fineness is 420D, and its crystallization half-cycle is t. 1 / 2 Less than approximately 0.6 minutes, with a fiber fineness of 840D and a crystallization half-cycle of t. 1 / 2 Less than about 0.7 minutes. In one example, the polyamide 56 fiber has a fineness of 420 D and a stress modulus of about 2.9 N to about 3.1 N at a specific elongation of 2% (LASE 2%); a stress modulus of about 5.5 N to about 6.0 N at a specific elongation of 5% (load at a specified elongation of 5%, LASE 5%); and a stress modulus of about 16.0 N to about 17.0 N at a specific elongation of 10% (LASE 10%). In another example, the polyamide 56 fiber has a fineness of 840 D and a stress modulus of about 5.5 N to about 6.2 N at a specific elongation of 2%; a stress modulus of about 11.0 N to about 12.5 N at a specific elongation of 5%; and a stress modulus of about 32.0 N to about 38.0 N at a specific elongation of 10%. In some embodiments, the monofilament fineness of polyamide 56 fiber is 3 to 7.5 (Denier per Filament, DPF).
[0039] The aforementioned crystallization half-cycle t 1 / 2 The measurement was performed using a differential thermal scanning spectroscopy analyzer (DSC-Q2000 from TA Instruments, USA). The measurement procedure involved taking a portion of the sample, weighing 5-10 mg of the sample, and performing the test. The measurement procedure was as follows: the temperature was increased to 300℃ at a rate of 10℃ / min and held for 2 min to eliminate thermal history; then the temperature was decreased to 30℃ at a rate of 10℃ / min to simulate the actual cooling rate during spinning; the temperature was then returned to the equilibrium temperature point, and the position of the crystallization peak and its half-width at half-maximum (HWHM) during the cooling process were measured to measure the crystallization rate. The narrower the HWHM, the shorter the time required to complete crystallization.
[0040] Polyamide 56 fibers formed from the aforementioned polyamide 56 resin composition have a highly stable crystalline structure and better molecular alignment (overall orientation), which can generate intermolecular cross-linking and enhance intermolecular forces, making the polyamide 56 fiber molecular chains anchored and less prone to slippage and deformation, thus exhibiting high stress modulus (high rigidity).
[0041] In some embodiments, depending on the fineness of the formed polyamide 56 fiber, polyamide 56 fibers can be prepared by the following two methods. In some embodiments, the preparation of polyamide 56 fibers with a fineness of less than 420D includes the following steps: (1) Polyamide 56 ester particles are mixed with a polymer crystallization modifier and then melt-mixed at 270~300°C to form a spinning melt, which is then formed into filaments through a metering pump and a spinning nozzle, wherein a slow cooling adjustment device (temperature of 260~340°C) is provided to avoid rapid solidification of the raw filament. (2) The raw filament after the slow cooling device is cooled and solidified by cooling air and then oiled. (3) The cooled and solidified raw filament is subjected to a heat stretching and heat setting process. The heat stretching process uses three pairs of stretching rollers with a stretching ratio of 1.2~3.0. The speed of the first pair of rollers is 1000~3500M / min, and the speed of the second and third pairs of rollers is 1200~5000M / min. The speed of each pair of rollers is adjusted according to the stretching ratio. The second and third pairs of rollers can heat the raw yarn at 150°C to 160°C and have a heat setting function. (4) The above-mentioned extended and set raw yarn is wound in a winding device at 1200 to 5000 M / min to form a yarn bundle and obtain high modulus polyamide 56 fiber.
[0042] In some embodiments, the preparation of polyamide 56 fibers with a fineness equal to or greater than 420D includes the following steps: (1) Polyamide 56 ester particles after solid-state polycondensation are mixed with a polymer crystallization modifier and then melt-mixed at 270~300℃ to form a spinning melt, which is then formed into a filament bundle through a metering pump and a spinning nozzle, wherein a slow cooling adjustment device (temperature of 260~340℃) is provided to avoid rapid solidification of the raw filament. The polyamide 56 ester particles after solid-state polycondensation have a relative viscosity of 60~100 and a chip moisture content of 300~800ppm. (2) The raw filament after the slow cooling device is cooled and solidified by cooling air and then oiled. (3) The solidified raw filament is subjected to a three-stage heat stretching and a two-stage heat setting process using six pairs of hot rollers. In detail, the oiled raw yarn is subjected to a first-stage pre-stretch between the first pair of hot rollers and the second pair of hot rollers, a second-stage main stretch between the second pair of hot rollers and the third pair of hot rollers, a secondary stretch between the third pair of hot rollers and the fourth pair of hot rollers, a heat setting between the fourth pair of hot rollers and the fifth pair of hot rollers, and finally a relaxation heat setting between the fifth pair of hot rollers and the sixth pair of hot rollers. The total stretch ratio of the above stretching process is 4.4~6.0, the heat setting temperature is 180~230℃, the relaxation heat setting temperature is 120~200℃, the relaxation speed difference is 50~200m / min, and the winding speed is 2200~3300 m / min, preferably 2600~2800 m / min. (4) The above-mentioned stretched and set raw yarn is wound in a winding device at 2200~3300 M / min to form a yarn bundle, thereby obtaining high-modulus polyamide 56 fiber.
[0043] This disclosure also provides a polyamide 56 fiber tow, which is obtained by plying multiple of the above-mentioned polyamide 56 fibers together without twisting. In some embodiments, the fineness of the polyamide 56 fiber tow is 75-840D when spun as a single strand, and 150-1680D when spun as a ply.
[0044] This disclosure also provides a polyamide 56 fiber twisted yarn, which is made by twisting and plying the aforementioned polyamide 56 fiber, wherein the fineness of the two twisted polyamide 56 fiber is 150~1680D, and the fineness of the three twisted polyamide 56 fiber is 225D~2520D.
[0045] This disclosure also provides a polyamide 56 fiber article made from the aforementioned polyamide 56 fiber. In some embodiments, the polyamide 56 fiber article includes tire cord fabric, conveyor belt, automotive fiber and its fabric, canopy fabric, heat-insulating and sun-shading fabric or the like.
[0046] This disclosure also provides a tire cord fabric obtained by impregnating the aforementioned polyamide 56 fiber twisted yarn, wherein the tire cord fabric has a stress modulus of about 17N to about 21N at a specific elongation of 5%, and has a stress modulus of about 41N to about 55N at a specific elongation of 10% (LASE 10%).
[0047] The following embodiments are provided to illustrate specific implementations of the present invention and to enable those skilled in the art to practice the invention. However, the following embodiments should not be construed as limiting the invention.
[0048] Examples 1 to 15 provide polyamide 56 resin compositions comprising polyamide 56 resin and a polymer crystallization modifier. Comparative Example 1 is polyamide 56 resin without addition. Comparative Examples 2 and 3 are polyamide 56 resins with different proportions of inorganic sodium salt added. Comparative Example 4 is polyamide 66 resin without addition, and Comparative Example 5 is polyamide 66 resin with polyamide 46 resin added. The enthalpy of crystallization (ΔH) of Examples 1 to 15 and Comparative Examples 1 to 5 were measured using a differential scanning calorimeter (DSC-Q2000, TA Instruments, USA). Tcc ) and crystallization half-cycle t 1 / 2 The measurement results are shown in Table 1 below.
[0049] Table 1
[0050]
[0051] In Table 1, the polyamide 56 resin without the addition of a polymer crystallization modifier (Comparative Example 1) exhibits poor crystallization behavior due to its asymmetrical structure; for example, it has a longer crystallization half-cycle t. 1 / 2As can be seen from the embodiments of this disclosure, adding appropriate amounts of polyamide 66 (PA66), polyamide 46 (PA46), and cholesteric liquid crystal polymer (LCP) to polyamide 56 resin can shorten the crystallization half-cycle and improve crystallization stability. In Example 8, the addition of excessive polyamide 66 resulted in a negligible decrease in the crystallization half-cycle and a significant decrease in the crystallization enthalpy.
[0052] Comparative Examples 2 and 3 used sodium 2,2'-methylene-bis-(4,6-di-tert-butylphenyl)phosphate, a small-molecule inorganic sodium salt, as a nucleating agent added to polyamide 56 resin. Experimental data showed that adding the inorganic sodium salt did not significantly shorten the crystallization half-cycle; the half-cycle remained greater than 1.5.
[0053] As shown in Comparative Examples 4 and 5, the addition of polyamide 46 to polyamide 66 resin did not significantly change its crystallization half-cycle. Therefore, the experiment indicates that polyamide 46 cannot adjust the crystallization properties of polyamide 66, proving that the polymer crystallization morphology regulator has a significant effect on the crystallization regulation of polyamide 56, but not on polyamide 66. The crystallization properties of the polyamide resin will affect the modulus of the polyamide fibers subsequently formed. Polyamide fibers were formed by melt spinning using the polyamide 56 resin compositions of Examples 1, 3, 14, and 15, the polyamide 56 resin of Comparative Example 1, and the polyamide 66 resins of Comparative Examples 4 and 5, and their properties were further tested.
[0054] Examples 16 to 22 below provide polyamide 56 fibers formed by melt spinning of a polyamide 56 resin composition including polyamide 56 resin and a polymer crystallization modifier. Comparative Examples 6, 9, and 10 provide fibers formed by melt spinning of unadded polyamide 56 resin. Comparative Examples 7 and 8 provide fibers formed by melt spinning of unadded polyamide 66 resin and polyamide 46 (PA46) resin, respectively.
[0055] The fibers of Examples 16-22 and Comparative Examples 6-10 were subjected to a crystallization half-cycle t 1 / 2 Specific elongation modulus and specific total orientation tests. Crystallization half-cycle t 1 / 2The measurements were performed using a differential thermal scanning spectroscopy (DSC) analyzer. Specific elongation modulus was tested according to ASTM D885, using a constant tensile testing machine with 60 twists per meter, a gauge length of 250 mm, and an elongation rate of 300 mm / min. The stress modulus values (commonly referred to in the industry as Lase 2%, Lase 5%, and Lase 10% modulus values) were evaluated at specific elongation rates of 2%, 5%, and 10%. Specific total alignment was tested according to ASTM D276, using a polarizing microscope with a polarizer to evaluate the difference in light velocity along the parallel and perpendicular paths of the fiber. The optimized formula is as follows: Specific total alignment = (Retardation * 1000 / fiber diameter). The measurement results are shown in Tables 2 to 5.
[0056] As shown in Table 2 below, Example 16 is a fiber formed from a polyamide 56 resin composition (the polyamide 56 resin composition of Example 14) containing a high molecular weight crystallization modifier, cholesterol liquid crystal polymer (LCP). It can induce crystal growth in a specific direction, thereby increasing the specific total orientation. Compared with Comparative Example 6, which does not contain a high molecular weight crystallization modifier, it has better crystallization behavior.
[0057] In Table 2 below, Examples 17-18 are fibers formed from polyamide 56 resin compositions containing polyamide 66 (the polyamide 56 resin compositions of Examples 1 and 3, respectively), Comparative Example 7 is a fiber formed from polyamide 66 resin without added polyamide 66, and Comparative Example 8 is a fiber formed from polyamide 66 resin with added polyamide 46 (PA46). As can be seen from Comparative Examples 7-8, although polyamide 66 resin and polyamide 56 are both polyamide resins, their crystallization behavior cannot be improved by adding the polymer crystallization morphology regulator disclosed herein.
[0058] Table 2
[0059]
[0060] As shown in Table 3 below, Example 19, a fiber with a fineness of 420D formed from a polyamide 56 resin composition containing polyamide 66 (the polyamide 56 resin composition of Example 3), exhibits better crystallization behavior than Comparative Example 9, which does not contain a polymer crystallization modulator. This results in a shorter crystallization half-cycle and improved overall orientation. Furthermore, by including polyamide 66, Example 19 effectively improves the fiber stress modulus values (i.e., LASE 2%, LASE 5%, and LASE 10% modulus values) at specific elongation rates of 2%, 5%, and 10%.
[0061] Table 3
[0062]
[0063] As shown in Table 4 below, Example 20 is a fiber with a fineness of 840D formed from a polyamide 56 resin composition containing polyamide 66 (the polyamide 56 resin composition of Example 3), and Examples 21-22 are fibers formed from polyamide 56 resin compositions containing cholesterol liquid crystal polymers (the polyamide 56 resin compositions of Examples 14 and 15, respectively). Compared to Comparative Example 10, which does not contain a polymer crystallization modulator, Examples 20-22 of this disclosure have better crystallization behavior. Furthermore, by including the aforementioned polymer crystallization modulator, the fiber stress modulus values of Examples 20-22 can be effectively improved at specific elongation rates of 2%, 5%, and 10%. Figure 1 and Figure 2 For the comparison of stress diagrams (modulus) at a specific elongation between Example 21 and Comparative Example 10, the LASE 2%, LASE 5%, and LASE 10% of Example 21 (fiber formed from a polyamide 56 resin composition containing cholesterol liquid crystal polymer) were significantly better than those of Comparative Example 10.
[0064] Table 4
[0065]
[0066] In summary, the stress modulus of polyamide 56 fibers formed from the polyamide 56 resin composition of this disclosure can be effectively improved at specific elongation rates of 2%, 5%, and 10%. Although polyamide 66 resin is also a polyamide resin, its stress modulus cannot be improved by adding the polymer crystallization modulator of this disclosure.
[0067] In Table 5 below, Example 23 and Comparative Example 11 are tire cord fabrics made from polyamide 56 fiber twisted yarn (840D / 2ply). As can be seen from Table 5, the tire cord fabric of Example 23, made from polyamide 56 fiber with added liquid crystal polymer, has better stress modulus values (i.e., LASE 2%, LASE 5%, and LASE 10% modulus values) than Comparative Example 11 without additives at specific elongation rates of 2%, 5%, and 10%.
[0068] Table 5
[0069]
[0070] As described above, embodiments of this disclosure provide a polyamide 56 resin composition comprising a polymeric crystallization modifier and polyamide 56 resin. By adjusting the mixing ratio of the polymeric crystallization modifier and the polyamide 56 resin, its crystallization properties can be controlled, thereby controlling the stress modulus of the polyamide 56 fibers formed therefrom. Specifically, the polymeric crystallization modifier can induce the polyamide 56 resin to grow and crystallize along a specific direction, increasing the specific total orientation of crystallization, ultimately resulting in a significant increase in fiber modulus. The polyamide 56 fibers of this disclosure with high stress modulus can be further applied to industrial applications, such as tire cord fabrics, conveyor belts, automotive fibers and their fabrics, tarpaulins, or heat-insulating and sun-shading fabrics, and other fiber products.
[0071] Although the present invention has been disclosed above by way of embodiments, it is not intended to limit the present invention. Any person skilled in the art can make various modifications and refinements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims.
Claims
1. A polyamide 56 resin composition, characterized in that, The composition includes polyamide 56 resin and a polymeric crystallization modifier, wherein the polymeric crystallization modifier is selected from liquid crystal polymeric crystallization modifiers, including cholesterol liquid crystal polymers. The polymeric crystallization modifier accounts for 0.1~3.0 wt% of the total weight of the polyamide 56 resin composition. The relative viscosity of the polyamide 56 resin composition in 90% formic acid is 40-100, and the crystallization half-cycle t measured by differential scanning calorimetry is... 1 / 2 The measurement procedure for this half-cycle of crystallization is less than 1.5 minutes. The temperature is increased to 300°C at 10°C / min, held for 2 minutes, and then decreased to 30°C at 10°C / min.
2. The polyamide 56 resin composition as described in claim 1, further comprising an oxidant, a catalyst, a processing aid, a polyester polymer, or a combination thereof.
3. A polyamide 56 fiber, characterized in that, The polyamide 56 fiber is obtained by spinning the polyamide 56 resin composition according to any one of claims 1 to 2.
4. The polyamide 56 fiber as described in claim 3, wherein the fineness of the polyamide 56 fiber is 75D, and the crystallization half-cycle t is measured by differential scanning calorimetry. 1 / 2 Less than 0.5 minutes.
5. The polyamide 56 fiber as described in claim 3, wherein the fineness of the polyamide 56 fiber is 420D, and the crystallization half-cycle t is measured by differential thermal scanning spectroscopy. 1 / 2 Less than 0.6 minutes.
6. The polyamide 56 fiber as claimed in claim 5, wherein the fineness is 420 D, and the polyamide 56 fiber has a stress modulus of 2.9 N to 3.1 N at a specific elongation of 2%.
7. The polyamide 56 fiber as claimed in claim 5, wherein the fineness is 420 D, and the polyamide 56 fiber has a stress modulus of 5.5 N to 6.0 N at a specific elongation of 5%.
8. The polyamide 56 fiber as claimed in claim 5, wherein the fineness is 420 D, and the polyamide 56 fiber has a stress modulus of 16.0 N to 17.0 N at a specific elongation of 10%.
9. The polyamide 56 fiber as claimed in claim 3, wherein the fineness of the polyamide 56 fiber is 840D, and the crystallization half-cycle t measured by differential thermal scanning spectroscopy is... 1 / 2 Less than 0.7 minutes.
10. The polyamide 56 fiber of claim 9, wherein the fineness is 840D, and the polyamide 56 fiber has a stress modulus of 5.5 N to 6.2 N at a specific elongation of 2%.
11. The polyamide 56 fiber of claim 9, wherein the fineness is 840D, and the polyamide 56 fiber has a stress modulus of 11.0N to 12.5N at a specific elongation of 5%.
12. The polyamide 56 fiber of claim 9, wherein the fineness is 840D, and the polyamide 56 fiber has a stress modulus of 32.0N to 38.0N at a specific elongation of 10%.
13. The polyamide 56 fiber as claimed in claim 3, wherein the monofilament fineness of the polyamide 56 fiber is 3 to 7.
5.
14. A polyamide 56 fiber bundle, characterized in that, The polyamide 56 fiber bundle is obtained by winding up the polyamide 56 fibers as described in claim 3, either as a single strand or as a double strand, during spinning.
15. The polyamide 56 fiber bundle as described in claim 14, wherein the fineness of the polyamide 56 fiber bundle is 75~840D when spun as a single strand and 150~1680D when spun as a double strand.
16. A polyamide 56 fiber twisted yarn, characterized in that, The polyamide 56 fiber twisted yarn is made by twisting and plying the polyamide 56 fiber as described in claim 3, wherein the fineness of the two twisted polyamide 56 fiber is 150~1680D, and the fineness of the three twisted polyamide 56 fiber is 225D~2520D.
17. A tire cord fabric, characterized in that, The tire cord fabric is obtained by impregnation of polyamide 56 fiber twisted yarn as described in claim 16, wherein the tire cord fabric has a stress modulus of 17N to 21N at a specific elongation of 5% and a stress modulus of 41N to 55N at a specific elongation of 10%.
18. A polyamide 56 fiber product, characterized in that, The polyamide 56 fiber product is made from the polyamide 56 fiber as described in claim 3, wherein the polyamide 56 fiber product includes tire cord fabric, conveyor belt, automotive fiber and its fabric, tarpaulin or heat-insulating and sun-shading fabric.
Citation Information
Patent Citations
A polyamide 5X medium-strength filament and its preparation method
CN106835329B
A polyamide 5X high-strength yarn and its preparation method
CN106868624B
Polyamide 56 composition with increased crystallization rate and application thereof
CN109666294A
High-strength polyamide 56 industrial yarn, manufacturing method thereof and application thereof
CN111411405A
Polyamide 5X resin capable of rapidly crystallizing and preparation method thereof
CN111518269A