Preparation method, product and application of a high-performance multifunctional carbon fiber sizing agent

By self-emulsifying multifunctional amino-modified cationic epoxy resin polymer sizing agent, the carboxyl group thermal decomposition at the interface of carbon fibers generates free radicals, and the covalent bonding connection with carbon fibers is solved, and the problem of insufficient emulsifier migration and adhesion strength is solved. The mechanical properties of composite materials are significantly improved.

CN117265879BActive Publication Date: 2024-11-01JILIN QIANREN NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311146012.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-07
Publication Date
2024-11-01
Estimated Expiration
2043-09-07

AI Technical Summary

Technical Problem

During the drying process, the emulsifier migration leads to strong moisture absorption, affecting storage stability and the mechanical properties of composite materials. It is difficult to connect carbon fibers to the sizing agent through covalent bonds, resulting in insufficient interfacial adhesion and mechanical properties.

Method used

Using self-emulsified multifunctional amino-modified cationic epoxy resin polymer sizing agent, unsaturated allyl double bonds are introduced through isocyanate reaction, combined with glacial acetic acid and water self-emulsification to form a high-performance carbon fiber sizing agent, and using carbon fiber interface Thermal decomposition of carboxyl groups produces free radicals, achieving covalent bonding, and improving adhesion and mechanical properties.

Benefits of technology

The interface bonding force of carbon fiber and the interlayer shear strength of composite materials are significantly improved, the bending strength and bending modulus, especially the interlayer shear strength is increased by 53%, and the wetting and adhesion between carbon fiber and epoxy resin matrix is ​​enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117265879B_ABST
    Figure CN117265879B_ABST
Patent Text Reader

Abstract

This patent relates to a preparation method, product and application of a high-performance multifunctional carbon fiber sizing agent. An amine-modified epoxy resin polymer is prepared by a chemical modification reaction of epoxy resin, and hydroxyl groups are generated in the main chain segment of the polymer. The allyl group is grafted onto the amine-modified epoxy resin polymer segment by the reaction of isocyanate with hydroxyl groups, and then glacial acetic acid and water are added to prepare a self-emulsifying sizing agent. The free radicals generated by the thermal decomposition of carboxyl groups at the carbon fiber interface are used to graft sizing agents with different double bond contents onto the carbon fiber surface, thereby improving the bonding strength between the carbon fiber and the sizing agent. At the same time, the hydroxyl groups and unsaturated double bonds introduced into the carbon fiber interface after sizing can undergo copolymerization with the epoxy resin / vinyl resin matrix, thereby enhancing the bonding strength between the carbon fiber and the epoxy resin matrix / vinyl resin matrix, and improving the interlaminar shear strength of the carbon fiber reinforced epoxy resin-based / vinyl resin-based composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This patent relates to a method for preparing a high-performance multifunctional carbon fiber sizing agent, and in particular to a method for preparing a self-assembling, self-emulsifying, amphiphilic cationic amine-modified epoxy resin polymer sizing agent, which can undergo a grafting reaction with the carbon fiber interface and can simultaneously improve the interfacial adhesion of carbon fiber reinforced epoxy resin-based and carbon fiber reinforced ethylene resin-based composite materials and the mechanical properties of the composite materials. Background Art

[0002] At present, most domestic carbon fiber companies use non-ionic or anionic epoxy resin emulsion sizing agents. Emulsion sizing agents are based on epoxy resin, and are prepared into epoxy resin aqueous emulsions with a certain amount of non-ionic or anionic emulsifiers. In order to improve the storage stability of epoxy resin emulsions, the amount of non-ionic or anionic emulsifiers generally exceeds 20% of the amount of epoxy resin. Since non-ionic or anionic emulsifiers are extremely hydrophilic, the emulsifier often migrates to the surface of the carbon fiber after sizing during the drying process, resulting in the carbon fiber surface having very strong moisture absorption, causing the sizing of the carbon fiber to harden in the cold winter, affecting the storage stability of the carbon fiber and the subsequent preparation of composite materials and the mechanical properties of the composite materials. The inventor of this patent proposed a self-assembling self-emulsifying amphiphilic cationic epoxy resin type high-performance fiber sizing agent / sizing agent / film-forming agent and its preparation method in patent CN109251305A. Although the patent solves the migration of external emulsifiers and the hardening of fibers after sizing due to moisture absorption, and at the same time improves the interfacial adhesion of composite materials through the charge force between the sizing agent and the carbon fiber interface, this charge force is negligible compared with the covalent bond force. Therefore, it is a challenge to invent a method for connecting carbon fibers and sizing agents through covalent bonds. Although a large number of carboxyl groups are generated on the surface of carbon fibers after electrochemical treatment, the reaction activity of carboxyl groups on the surface of carbon fibers is very low, and carboxyl groups on the surface of carbon fibers are easily decomposed at medium and high temperatures to produce free radicals and carbon dioxide. Therefore, the efficiency of the ring-opening grafting reaction between the carboxyl groups on the interface of carbon fibers and the epoxy groups in the epoxy resin type sizing agent emulsion is very low. In addition, epoxy resin sizing agents cannot undergo chemical bonding reactions with vinyl resins. Therefore, it is difficult to improve the mechanical properties of carbon fiber reinforced vinyl resin-based composites, especially the interlaminar shear strength, after epoxy resin sizing agents are applied to the carbon fiber surface. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a self-emulsifying multifunctional amino-modified cationic epoxy resin polymer sizing agent, and the sizing agent can be grafted with the carbon fiber interface, and the mechanical properties such as the interfacial adhesion of the carbon fiber and the interlayer shear strength of the vinyl resin-based / epoxy resin-based composite material are greatly improved through the bonding effect of covalent bonds.

[0004] Another object of the present invention is to provide a method for preparing a self-emulsifying multifunctional amine-modified cationic epoxy resin polymer sizing agent emulsion by reacting a hydrophilic polyetheramine and a hydrophobic fatty amine with an epoxy resin to prepare an amine-modified epoxy resin polymer, and at the same time generate hydroxyl groups (such as Figure 1 shown).

[0005] 1. A preparation method, product and application of a high-performance multifunctional carbon fiber sizing agent, characterized in that the unsaturated allyl double bond is introduced into the amine-modified epoxy resin polymer chain segment by the amine-modified hydroxyl group in the epoxy resin polymer molecular chain segment through the selective reaction of isocyanate, and then glacial acetic acid and water are added to prepare the high-performance carbon fiber sizing agent by self-emulsification. The sized carbon fiber is applied to the preparation of vinyl resin-based / epoxy resin-based composite materials. The specific steps are as follows:

[0006] 1) drying allyl ether alcohol to remove moisture, adding a certain amount of diisocyanate into a reaction kettle equipped with a mechanical stirring, a condensation reflux sealing device and a nitrogen protection system at room temperature;

[0007] 2) Slowly raise the temperature to a certain temperature and keep the temperature constant for a certain period of time;

[0008] 3) using di-n-butylamine titration to test the isocyanate reaction to the calculated value and then cooling to room temperature;

[0009] 4) adding a certain amount of dry amine-modified epoxy resin polymer into the above reaction kettle;

[0010] 5) slowly heating up to a certain temperature, and reacting at a constant temperature until all isocyanates are completely reacted; adding an appropriate amount of an organic solvent with a low boiling point and miscible with water according to the viscosity, and adding an aqueous solution of glacial acetic acid to the reactor for neutralization to form salts;

[0011] 6) After high-speed stirring, a certain amount of water is added for emulsification to obtain a self-assembling self-emulsifying amphiphilic cationic epoxy resin polymer sizing agent.

[0012] 7) After the cationic carbon fiber sizing agent is diluted to a certain solid content using deionized water, the surface of the carbon fiber is subjected to sizing modification;

[0013] 8) After sizing, the carbon fiber is dried at 110℃~170℃

[0014] As a further optimization of the present invention, the allyl ether alcohol in step 1) is ethylene glycol monoallyl ether, propylene glycol monoallyl ether, or polyethylene glycol monoallyl ether, polypropylene glycol monoallyl ether, or polyethylene glycol propylene glycol copolymer monoallyl ether.

[0015] As a further optimization of the present invention, step 1) the allyl ether alcohol is dried and dehumidified by molecular sieve or dehumidified under reduced pressure at 80°C. For allyl ether alcohols with lower boiling points such as ethylene glycol monoallyl ether and propylene glycol monoallyl ether, 4A molecular sieve is used for drying and dehumidification, and for other allyl ether alcohols with higher boiling points, 80°C dehumidification is used for dehumidification under reduced pressure.

[0016] As a further optimization of the present invention, the diisocyanate raw material in step 1) is isophorone diisocyanate (IPDI), toluene-2,4-diisocyanate (TDI100), 2,4'-diphenylmethane diisocyanate, or hydrogenated 2,4'-diphenylmethane diisocyanate, and the two isocyanate groups in these diisocyanate raw materials show different reactivity due to steric effect and electronic effect.

[0017] As a further optimization of the present invention, in step 1), the molar ratio of allyl ether alcohol to diisocyanate is 1:1, and NCO / OH is 2:1.

[0018] As a further optimization of the present invention, step 2) reaction temperature. The isocyanate group (NCO) with higher reactivity in the diisocyanate raw material reacts with the allyl ether alcohol at a lower temperature, and the other isocyanate group (NCO) does not react. Specifically, the reaction temperature of 2,4'-diphenylmethane diisocyanate with allyl ether alcohol does not exceed 30°C; the reaction temperature of TDI100 with allyl ether alcohol does not exceed 70°C, and the reaction temperature of IPDI with allyl ether alcohol does not exceed 80°C (such as Figure 2 shown).

[0019] As a further optimization of the present invention, step 3) di-n-butylamine titration method is to use excess di-n-butylamine to react with isocyanate, and use hydrochloric acid titration and bromocresol green indicator to determine the unreacted di-n-butylamine, NCO value (%) = (V0-V1)*C HCl *4.2 / m

[0020] Where:

[0021] V0——the volume of HCl standard solution consumed in the blank test, mL;

[0022] V1——The volume of HCl standard solution consumed by the sample, mL;

[0023] C HCl ——Concentration of HCl standard solution, mol / L;

[0024] m——sample mass, g.

[0025] As a further optimization of the present invention, step 4) drying of the amino-modified epoxy resin polymer is performed by dehumidification at 130° C. under an argon / nitrogen atmosphere;

[0026] As a further optimization of the present invention, step 7) uses deionized water to dilute the cationic carbon fiber sizing agent to a certain solid content, and then performs sizing modification on the carbon fiber surface. The solid content of the sizing agent is affected by the carbonization process such as the drafting and winding speed, the length of the sizing tank, the surface roughness of the carbon fiber, and the terminal application of the carbon fiber. Generally, the solid content of the sizing agent in the sizing tank is 2% to 5%, ensuring that the carbon fiber sizing rate is 0.8% to 1.5%.

[0027] As a further optimization of the present invention, in step 8), the carbon fibers are dried at a medium-high temperature (110°C to 170°C) after sizing. The carbon fibers contain carboxyl groups on their surface, which are easily decomposed to produce free radicals at medium-high temperatures. The allyl unsaturated double bonds contained in the molecular chain segments of the sizing agent will undergo a double bond grafting reaction through the free radicals on the carbon fiber surface and a self-crosslinking reaction of the double bonds in the molecular chain segments of the sizing agent (such as Figure 3 shown).

[0028] As a further optimization of the present invention, the amount of the amino-modified epoxy resin polymer added in step 4) is affected by the hydroxyl content in its molecular chain segment and the amount of the allyl ether alcohol added in step 1). The optimal molar ratio of the double bonds introduced in the molecular chain segment of the self-emulsifying cationic carbon fiber sizing agent to the hydroxyl groups on the amino-modified polymer chain segment is 9:1, that is, the double bond molar content is 10%. When the molar ratio of the double bonds contained in the sizing agent to the hydroxyl groups on the polymer chain segment is lower than 1:9, that is, when the molar content of the double bonds is lower than 10%, the grafting rate between the sizing agent and the carbon fiber interface is low; on the contrary, when the molar ratio of the double bonds contained in the self-emulsified cationic carbon fiber sizing agent prepared in steps 1) to 6) to the hydroxyl groups on the polymer chain segment is higher than 1:9, that is, the molar content of the double bonds is higher than 10%, the self-crosslinking reaction density of the double bonds in the molecular chain segment of the sizing agent is too high, which affects the penetration of the epoxy resin matrix / vinyl resin matrix into the interface of the sized carbon fiber, and is not conducive to the wettability of the sized carbon fiber with the epoxy resin matrix / vinyl resin matrix in step 8), the adhesion and the interlayer shear strength of the composite material are enhanced.

[0029] This patent aims at the deficiencies of the prior art and invents a self-emulsifying amine-modified cationic epoxy resin polymer sizing agent. The preparation of the sizing agent emulsion avoids the use of a large amount of emulsifier and the migration of the emulsifier to the surface of the carbon fiber when the carbon fiber is dried after sizing, which causes the carbon fiber to easily absorb moisture, affecting the storage stability of the carbon fiber and the wettability and adhesion between the carbon fiber interface and the resin matrix when the carbon fiber is composited with the resin matrix. This patent further invents that allyl ether alcohol reacts with diisocyanate to graft unsaturated double bonds onto the amine-modified epoxy resin polymer chain segment, and through the thermal decomposition of the carboxyl group on the carbon fiber interface to generate free radicals, the self-emulsifying cationic amine-modified epoxy resin polymer sizing agent is successfully connected to the carbon fiber surface through covalent bonds, which greatly improves the adhesion between the carbon fiber and the sizing agent. At the same time, the unsaturated double bonds remaining on the carbon fiber interface after sizing can undergo copolymerization with the vinyl resin matrix, which greatly enhances the adhesion between the carbon fiber and the vinyl resin matrix, and improves the interlaminar shear strength, bending strength and bending modulus of the carbon fiber reinforced vinyl resin matrix composite material, among which the interlaminar shear strength is increased by 53%.

[0030] The structure of the amine-modified epoxy resin polymer is similar to that of the epoxy resin matrix. The similar miscibility characteristics are used to greatly improve the wettability and adhesion between the carbon fiber and the epoxy resin matrix after sizing. At the same time, the amine-modified epoxy resin polymer contains a large number of hydroxyl groups and tertiary amine groups on the molecular chain segments. At high temperatures, the tertiary amine groups can catalyze the ring-opening reaction between the hydroxyl groups and the epoxy resin matrix, effectively improving the adhesion between the carbon fiber and the epoxy resin matrix, and greatly improving the interlaminar shear strength of the carbon fiber / epoxy resin-based composite material. Compared with the self-assembled self-emulsifying cationic epoxy resin sizing agent, the interlaminar shear strength is further improved by 16%. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Synthesis of amine-modified epoxy resin polymers;

[0032] Figure 2 Selective reaction of allyl ether alcohols with diisocyanates;

[0033] Figure 3 The double bonds in the amine-modified epoxy resin polymer are grafted onto the carbon fiber interface and the sizing agent is cross-linked with itself;

[0034] Figure 4 Carbon fiber sizing, drying and winding process. DETAILED DESCRIPTION

[0035] Embodiment 1:

[0036] Use 30g acetone to dissolve 26.6g octadecylamine and 24.7g polyetheramine (molecular weight is 1000), add 49.1g E-1NT epoxy resin (epoxy equivalent 185g / eq) in the reactor, install the seal and condensation device, introduce nitrogen, set the temperature to 40℃, wait for the temperature to reach 40℃ and stabilize for 10min, add a water separator, set the temperature to 70℃, remove the water separator device when no more solvent evaporates, slowly raise the temperature to 100℃, react for 1h, then raise the temperature to 130℃, keep the temperature constant for 3h, then cool to 50℃, add 100.4g acetone dried with 4A molecular sieve, cool to room temperature and seal for standby use. The molecular weight of the amino-modified epoxy resin emulsion is 10000.

[0037] Embodiment 2:

[0038] 50g of acetone dried with 4A molecular sieves and 10.21g of ethylene glycol monoallyl ether dried with molecular sieves were put into a reaction kettle, and nitrogen was introduced after installing a thermometer and a condensing device. 17.41g of TDI100 was added under stirring at room temperature, and the temperature was slowly raised to 60°C. The acetone was removed, and the reaction was carried out at a constant temperature for 2h, then the temperature was lowered to room temperature and sealed for use.

[0039] Embodiment 3:

[0040] 14.62g of diethylene glycol monoallyl ether was put into a reaction kettle, heated to 80°C with stirring, dehumidified under reduced pressure for 2h, then cooled to room temperature, the dehumidification was stopped, nitrogen was passed, 17.41g of TDI100 was added, the temperature was slowly raised to 60°C, reacted at a constant temperature for 2h, then cooled to room temperature and sealed for use.

[0041] Embodiment 4:

[0042] 50g of acetone dried with 4A molecular sieves and 10.21g of ethylene glycol monoallyl ether dried with molecular sieves were put into a reaction kettle, and nitrogen was introduced after installing a thermometer and a condensing device. 22.23g of IPDI was added under stirring at room temperature, and the temperature was slowly raised to 80°C. The acetone was removed, and the reaction was carried out at a constant temperature for 3 hours. Then the temperature was lowered to room temperature and sealed for use.

[0043] Embodiment 5:

[0044] 50g of acetone dried with 4A molecular sieves and 10.21g of ethylene glycol monoallyl ether dried with molecular sieves were put into a reaction kettle, and nitrogen was introduced after installing a thermometer and a condenser. 25.03g of 2,4'-diphenylmethane diisocyanate was added under stirring at room temperature. After reacting at room temperature for 2 hours, the temperature was slowly raised to 60°C. After removing the acetone, the temperature was lowered to room temperature and sealed for standby use.

[0045] Embodiment 6:

[0046] 200.8 g of the amino-modified epoxy resin polymer prepared in Example 1 was accurately weighed and added to a reaction kettle, 7.40 g of glacial acetic acid was added, and 234.27 g of water was added to prepare an amino-modified epoxy polymer emulsion sizing agent (sizing agent S0, solid content 30%) with a double bond molar content of 0% and a particle size of 109.1 nm. The emulsion was stored at room temperature for 6 months or centrifuged at 3000 rpm for 30 min without precipitation.

[0047] Embodiment 7:

[0048] 200.8 g of the amino-modified epoxy resin polymer prepared in Example 1 was accurately weighed and added to the reactor. After installing the seal and condensing device, nitrogen was introduced and the temperature was set to 40° C. After the temperature reached 40° C. and stabilized for ten minutes, 3.46 g of the product in Example 2 was added, and the temperature was slowly raised to 75° C. after stirring evenly. After reacting for 2 hours, the temperature was lowered to 40° C., 7.40 g of glacial acetic acid was added, and 242.67 g of water was added to prepare an amino-modified epoxy polymer emulsion sizing agent (sizing agent S1, solid content 30%) with a double bond molar content of 5%, the particle size was 110.2 nm, and the emulsion was stored at room temperature for 6 months or centrifuged at 3000 rpm for 30 min without precipitation.

[0049] Embodiment 8:

[0050] Accurately weigh 200.8g of the amino-modified epoxy resin polymer prepared in Example 1, add it to the reactor, install the seal and condensation device, introduce nitrogen, set the temperature to 40°C, and after the temperature reaches 40°C and stabilizes for 10min, add 6.92g of the product in Example 2, stir evenly and slowly raise the temperature to 75°C, react for 2h and then cool to 40°C, add 7.40g of glacial acetic acid, add 251.35g of water, and synthesize an amino-modified epoxy polymer emulsion sizing agent (sizing agent S2, solid content 30%) with a double bond molar content of 10%, with a particle size of 118.2nm, and the emulsion is stored at room temperature for 6 months or centrifuged at 3000 rpm for 30min without precipitation.

[0051] Embodiment 9:

[0052] Accurately weigh 200.8g of the amino-modified epoxy resin polymer prepared in Example 1, add it to the reactor, install the seal and condensation device, introduce nitrogen, set the temperature to 40°C, and after the temperature reaches 40°C and stabilizes for ten minutes, add 10.38g of the product in Example 2, stir evenly and slowly heat up to 75°C, react for 2h and then cool to 40°C, add 7.40g of glacial acetic acid, add 258.49g of water, and synthesize an amino-modified epoxy polymer emulsion sizing agent (sizing agent S3, solid content 30%) with a double bond molar content of 15%, with a particle size of 121.1nm, and the emulsion is stored at room temperature for 6 months or centrifuged at 3000 rpm for 30min without precipitation.

[0053] Embodiment 10:

[0054] 1. Carbon fiber sizing process

[0055] The carbon fiber tow is immersed in a self-emulsifying cationic amine-modified epoxy resin polymer sizing agent tank containing different double bond contents. The CF is continuously pulled into and immersed in the tank with an automatic flushing device to complete the sizing process. The solid content of the sizing agent in the sizing agent tank is 2.5%, and the sizing rate is about 1%. Figure 4 The sizing CF was then immediately dried at 110-170°C for 2 h to evaporate the water. Four different amine-modified epoxy polymer sizing agents with different double bond ratios (0%, 5%, 10%, 15%) were used in the impregnation process.

[0056] 2. Carbon fiber desizing process after sizing

[0057] The sized and dried carbon fiber is placed in a Soxhlet extractor, and acetone is used to reflux and extract the sizing agent that has not undergone interface grafting reaction and self-crosslinking reaction at the carbon fiber interface. The mass of the carbon fiber before and after acetone extraction is weighed, and the percentage of sizing agent that has undergone grafting reaction and self-crosslinking reaction at the carbon fiber interface is calculated, that is, the sizing agent content remaining on the carbon fiber surface:

[0058] Sc={1-[(W CF -W CFS ) / W CF *S%]}*100%

[0059] Sc is the percentage of sizing agent for grafting reaction and cross-linking reaction at the carbon fiber interface

[0060] W CF :Carbon fiber weight before acetone extraction

[0061] W CFS : Carbon fiber weight after acetone extraction

[0062] S%: Carbon fiber sizing rate

[0063] 3. Moisture absorption rate of carbon fiber after sizing

[0064] The sizing carbon fiber was stored at room temperature for one month, and then dried in a drying oven at 110°C for 4 hours. The mass change of the carbon fiber before and after drying was tested, and the moisture absorption rate (m) of the carbon fiber was calculated:

[0065] m=(W1-W2) / W1*100%

[0066] Where W1 is the mass of carbon fiber before drying, and W2 is the mass of carbon fiber after drying

[0067] 4. Preparation of vinyl resin composites

[0068] Unidirectional carbon fiber reinforced vinyl resin composites for interlaminar shear strength tests were prepared by hot pressing. Four samples of 2*6*200mm specimens V1, V2, V3, V4 were prepared by impregnating carbon fibers with resin using the hand lay-up method (vinyl resin, curing agent TBPEH and TBPB were mixed in a mass ratio of 100:1:1), stacked and placed in a mold, left to degas at room temperature for 30 minutes, and then molded, and then cured at 150°C for 2 hours. 5. Preparation of AG80 epoxy resin composites

[0069] Unidirectional carbon fiber reinforced AG80 epoxy resin composites for interlaminar shear strength test were prepared by hot pressing method. Four samples of 2*6*200mm samples E1, E2, E3, E4 were prepared by impregnating carbon fiber with resin using hand lay-up method (AG80 epoxy resin / DDS weight ratio is 10:4). The mixture of AG80 and DDS was melted into a transparent solution at 135°, and then the solution was applied to the carbon fiber unidirectional yarn. Then, the resin-impregnated carbon fiber unidirectional yarn was placed in a mold preheated at 135°C and treated with a release agent. After closing the mold, it was placed in a 135°C oven for 90 minutes, and the mold was fixed with bolts, heated to 180°C, and kept warm for 120 minutes before naturally cooling to room temperature.

[0070] Embodiment 11:

[0071] Grafting and cross-linking reaction of sizing agent at carbon fiber interface. According to the CF desizing process after sizing as described in Example 10 (2), sizing agents S0, S1, S2, and S3 are sized on the carbon fiber surface and dried before desizing using acetone. As the double bond content in the molecular chain segment of the amino-modified epoxy resin polymer sizing agent increases, the grafting reaction between the sizing agent and the carbon fiber interface and the cross-linking reaction of the sizing agent itself increase. The sizing agent remaining on the carbon fiber surface after acetone extraction increases. The test results are shown in Table 1. The percentage of sizing agent that undergoes grafting and cross-linking reactions at the carbon fiber interface:

[0072] Table 1

[0073] Embodiment 12:

[0074] Interlaminar shear strength (ILSS) of carbon fiber reinforced vinyl resin / epoxy resin composite materials after sizing. According to Examples 10(4) and 10(5), four carbon fiber reinforced vinyl resin and carbon fiber reinforced AG80-DDS epoxy resin composite samples were prepared respectively. The interlaminar shear strength (ILSS) of the composite materials was tested using the GB / T30969-2014. Polymer-based composite material three-point short beam shear strength test method. The test results are shown in Table 2. ILSS of carbon fiber reinforced vinyl resin composite materials:

[0075] Table 2

[0076] Sizing agent <![CDATA[S0]]> <![CDATA[S1]]> <![CDATA[S2]]> <![CDATA[S3]]> CF / VinylesterILSS(MPa) 46.1 62.5 70.5 65.3 CF / AG80-DDSILSS(MPa) 87.6 94.1 104.3 98.5

Claims

1. A method for preparing a high-performance multifunctional carbon fiber sizing agent, characterized in that: The hydroxyl groups generated on the main chain of the amine-modified epoxy resin polymer are used to graft allyl groups onto the chain segments of the amine-modified epoxy resin polymer through the reaction of isocyanate with the hydroxyl groups, and then the hydroxyl groups are salted with glacial acetic acid and emulsified with water to prepare a self-emulsifying cationic sizing agent. The specific steps are as follows: 1) After removing trace water or moisture from allyl ether alcohol, a certain amount of diisocyanate raw material is added to a reaction kettle equipped with a mechanical stirring, a condensation reflux sealing device and a nitrogen protection system at room temperature; 2) Slowly raise the temperature to a certain temperature and keep the temperature constant for a certain period of time; 3) Testing the isocyanate by di-n-butylamine titration method, and then cooling to room temperature after reaching the calculated value; 4) adding a certain amount of dry amine-modified epoxy resin polymer into the above reaction kettle; 5) slowly heating up to a certain temperature, and reacting at a constant temperature until all isocyanates are completely reacted; adding an appropriate amount of an organic solvent with a low boiling point and miscible with water according to the viscosity, and adding an aqueous solution of glacial acetic acid to the reactor for neutralization to form salts; 6) After high-speed stirring, a certain amount of water is added for emulsification to obtain a self-emulsifying cationic carbon fiber sizing agent; The amine-modified epoxy resin polymer is prepared by reacting a hydrophilic polyether amine and a hydrophobic fatty amine with an epoxy resin, and simultaneously a hydroxyl group is generated in a chain segment of the amine-modified epoxy resin polymer; In step 1), the two isocyanate groups in the diisocyanate raw material have different reactivity with the hydroxyl groups and must react selectively; In the step 2), different diisocyanates are selected and different reaction temperatures are used; by regulating the reaction temperature, the isocyanate groups with higher reaction activity in the diisocyanate raw material react with the allyl ether alcohol.

2. The method for preparing a high-performance multifunctional carbon fiber sizing agent according to claim 1, characterized in that: In the step 1) and the step 4), the amount of the amino-modified epoxy resin polymer added is affected by the hydroxyl content in its molecular chain segment and the amount of allyl ether alcohol added, and the optimal molar ratio of the double bonds introduced in the molecular chain segment of the self-emulsifying cationic carbon fiber sizing agent to the hydroxyl groups on the amino-modified polymer chain segment is 9:1, that is, the optimal molar content of the double bonds is 10%.

3. A high-performance multifunctional carbon fiber sizing agent prepared by the preparation method according to any one of claims 1-2.

4. The application method of the high-performance multifunctional carbon fiber sizing agent according to claim 3, characterized in that: When the carbon fiber is dried at medium to high temperature after sizing, the allyl double bonds contained in the molecular chain segments of the sizing agent undergo free radical grafting reaction with the carbon fiber interface and the double bonds in the sizing agent molecules undergo self-crosslinking reaction at the same time. The specific steps are as follows: 1) diluting the high-performance multifunctional carbon fiber sizing agent with deionized water to a certain solid content, and then performing sizing modification on the surface of the carbon fiber; 2) Dry the sizing carbon fiber at 110°C~170°C.