Maleimide resin, curable resin composition and cured product thereof

Through the maleimide resin and hardenable resin composition with a specific structure, the problem of insufficient heat resistance and dielectric characteristics of existing materials in high-frequency electrical and electronic parts and 3D printing is solved, and the high heat resistance of the materials is achieved , low dielectric properties, suitable for a wide range of high-performance applications.

CN117279962BActive Publication Date: 2024-11-01NIPPON KAYAKU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280033186.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-05-06
Filing Date
2022-04-28
Publication Date
2024-11-01
Estimated Expiration
2042-04-28

AI Technical Summary

Technical Problem

Existing resin materials are difficult to have heat resistance, low dielectric properties and good hardening in high-frequency electrical and electronic parts, and lack heat resistance, mechanical properties and electrical properties in 3D printing applications. Traditional materials such as acrylates and Epoxy resin is insufficiently hygroscopic.

Method used

Developing maleimide resins with specific structures and their hardened resin compositions, through the reaction of styrene/maleic acid copolymer and diamine compound, combined with free radical polymerization initiator and polyphenylene ether compound, to form a Hardened substance with excellent heat resistance and low dielectric properties.

Benefits of technology

It realizes high heat resistance, low dielectric properties and good hardening of resin materials used in electrical and electronic parts and 3D printing, improves the mechanical and electrical characteristics of the materials, and is suitable for semiconductor sealing, printed circuit substrates and carbon fiber composites. Materials and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117279962B_ABST
    Figure CN117279962B_ABST
Patent Text Reader

Abstract

The present invention provides a maleimide resin having excellent heat resistance and electrical properties and good curability, a curable resin composition and a cured product thereof. The maleimide resin is obtained by reacting a styrene / maleic acid copolymer, a compound containing two or more amino groups in the molecule and maleic anhydride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a maleimide resin having a specific structure, a curable resin composition and a cured product thereof, which are suitable for use in semiconductor sealing materials, printed circuit boards, electrical and electronic parts such as build-up laminates, light-weight and high-strength materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics, and 3D printing applications. Background Art

[0002] In recent years, as the application fields of laminated boards equipped with electrical and electronic components have expanded, the required characteristics have also become wider and more advanced. In the past, semiconductor chips were mainly mounted on metal lead frames, but semiconductor chips with higher processing power such as central processing units (hereinafter referred to as CPUs) are often mounted on laminated boards made of polymer materials.

[0003] In particular, semiconductor packages (hereinafter referred to as PKG) used in smart phones are required to have thinner PKG substrates in order to meet the requirements of miniaturization, thinness and high density. However, if the PKG substrate is thinner, the rigidity will decrease, so the heating when the PKG is soldered and mounted on the motherboard (PCB) will cause large warping and other undesirable situations. In order to reduce this situation, a PKG substrate material with a high Tg above the soldering mounting temperature is required.

[0004] In addition, the fifth-generation communication system "5G", which is now being developed at an accelerated pace, is expected to further develop large-capacity and high-speed communications. The frequency used by 5G will be higher, so to achieve high-speed communication using high frequencies, it is required to further improve the performance of substrate materials. For example, it is very important to have low dielectric properties in order to reduce transmission losses, and the loss tangent is required to be at least 0.005 or less at 10GHz. The transmission loss generated on the printed circuit board is derived from conductor loss and dielectric loss (Non-patent Document 1). Conductor loss is caused by the resistance component of conductors such as wiring on the substrate, and is divided into losses caused by the high-frequency skin effect and scattering losses caused by the roughness of the copper foil surface. The higher the frequency, the more electronic signals will flow near the copper foil surface (the distance from the copper foil surface is 1GHz: 2.1μm, 10GHz: 0.66μm). In order to reduce the skin effect, the low roughness of copper foil has been developed in recent years. The problem then becomes to ensure the adhesion to the low roughness copper foil, which is one of the requirements of the resin material. However, low dielectric materials such as PTFE (polytetrafluoroethylene) or LCP (liquid crystal polymer) lack adhesion. In addition, these materials are thermoplastic materials and therefore lack formability. In view of this, it is expected to develop a thermosetting resin with excellent adhesion, low dielectric properties, and formability.

[0005] In addition, in the automotive field, with the development of electronics, precision electronic equipment is also installed near the engine drive unit, which requires a higher level of heat resistance and moisture resistance. Electric cars and air conditioners are beginning to use SiC semiconductors, which requires extremely high heat resistance for the sealing materials of semiconductor elements, so the previous epoxy resin sealing materials have become unable to cope with it.

[0006] In view of the above background, polymer materials that have both heat resistance and low loss tangent properties are being explored. For example, Patent Document 1 proposes a composition containing a maleimide resin and a phenolic resin having an acrylic group. However, on the other hand, phenolic hydroxyl groups that do not contribute to the reaction during the curing reaction will remain, so it is difficult to say that the electrical properties are sufficient. In addition, Patent Document 2 discloses an allyl ether resin in which the hydroxyl group is replaced by an allyl group. However, it is shown that Claisen rearrangement will occur at 190°C, and phenolic hydroxyl groups that do not contribute to the curing reaction will be generated at 200°C, which is the molding temperature of a general substrate, so the electrical properties cannot be satisfied.

[0007] In addition, in recent years, 3D printing has attracted much attention as a three-dimensional shaping technique, and has begun to be used in fields that require reliability, such as aerospace, automobiles, and connectors of electronic parts used in these fields. In particular, light-curing and heat-curing resins are being explored for uses represented by stereolithography (SLA) or digital light processing (DLP). Therefore, although the stability and accuracy of the shape are mainly required in the previous method of transferring from the mold, various properties such as heat resistance, mechanical properties, toughness, flame retardancy, and electrical properties are required in 3D printing applications, and their materials are being developed. In addition, when used for structural components, there will be issues such as changes in properties due to moisture absorption. Currently, acrylate resins or epoxy resins are used for this purpose, but both hardened materials contain a large number of ester bonds, ether bonds, and even hydroxyl groups, and the hygroscopic properties are not sufficient.

[0008] [Prior art literature]

[0009] [Non-patent literature]

[0010] Non-patent document 1: Factors of signal loss in high-speed signal transmission on printed circuit boards (Mitsui Mining and Smelting Co., Ltd.) 29th The Japan Institute of Electronics Packaging Spring Performance Conference 16P1-17.

[0011] [Patent Document]

[0012] Patent Document 1: Japanese Patent Application Laid-Open No. 04-359911

[0013] Patent document 2: International Publication No. 2016 / 002704. Summary of the invention

[0014] [Problems that the invention aims to solve]

[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a maleimide resin having excellent heat resistance and electrical properties and good curability, a curable resin composition, and a cured product thereof.

[0016] [Methods used to solve the problem]

[0017] The present inventors have conducted intensive studies to solve the above problems and have found that a maleimide resin having a specific structure and a curable resin composition thereof have excellent heat resistance and low dielectric properties when cured, thereby completing the present invention.

[0018] That is, the present invention relates to the following [1] to

[10] . In addition, in the present application, "(value 1) to (value 2)" include the upper and lower limits.

[0019] [1] A maleimide resin obtained by reacting a styrene / maleic acid copolymer, a compound having two or more amino groups in the molecule, and maleic anhydride.

[0020] [2] The maleimide resin according to [1], which has repeating units of the following formulae (a) and (b).

[0021]

[0022] (In the above formula, X represents an arbitrary organic group. m and n are the average values ​​of the number of repetitions, 1≤m≤1000, 1≤n≤1000. (a) and (b) are bonded with * and the repetition positions may be random.)

[0023] [3] The maleimide resin according to [2], wherein in the formula (b), X is any one or more of the following formulas (A) to (P).

[0024]

[0025] (In the above formula, R represents a hydrocarbon group having 1 to 10 carbon atoms, a represents an integer from 0 to 4, p represents a number from 1 to 20, and * represents a bonding position.)

[0026] [4] The maleimide resin according to [3], wherein in the formula (b), X is any one or more of the formulas (A) to (F).

[0027] [5] The maleimide resin according to [1], wherein the compound containing two or more amino groups in the molecule is at least one selected from the group consisting of amine compounds represented by the following formulae (1) to (5) and dimer diamines.

[0028]

[0029] (In formula (1), n ​​is the average value of the number of repetitions, 1≤n<5.)

[0030]

[0031] (In formula (2), R each independently represents a hydrocarbon group having 1 to 3 carbon atoms, p is the average value of the number of repetitions, and 0≤p≤20.)

[0032]

[0033] (In formula (3), R each independently represents a hydrocarbon group having 1 to 3 carbon atoms)

[0034]

[0035] (In formula (4), n is the average value of the number of repetitions, 1 <n<5。)

[0036]

[0037] (In formula (5), n is the average value of the number of repetitions, 1≤n<5.)

[0038] [6] A curable resin composition comprising the maleimide resin according to any one of [1] to [5].

[0039] [7] The curable resin composition according to [6], further comprising a radical polymerization initiator.

[0040] [8] The curable resin composition according to [6] or [7], further comprising a polyphenylene ether compound.

[0041] [9] The curable resin composition according to any one of [6] to [8], further comprising a styrene / butadiene copolymer.

[0042]

[10] A cured product obtained by curing the maleimide resin described in any one of [1] to [5] or the curable resin composition described in any one of [6] to [9].

[0043] [Effects of the invention]

[0044] The maleimide resin of the present invention has excellent curability, and its cured product has excellent properties in terms of high heat resistance and low dielectric properties, and is therefore a material that can be used in sealing of electrical and electronic parts, circuit substrates, carbon fiber composites, and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The GPC chart of Synthesis Example 1 is shown.

[0046] Figure 2 The HPLC chart of Synthesis Example 1 is shown.

[0047] Figure 3 The synthesis example 1 1 H-NMR chart.

[0048] Figure 4 The GPC chart of Example 1 is shown.

[0049] Figure 5 Example 1 1 H-NMR chart.

[0050] Figure 6 The GPC chart of Example 2 is shown.

[0051] Figure 7 Example 2 1 H-NMR chart.

[0052] Figure 8 The GPC chart of Example 3 is shown.

[0053] Fig. 9 The GPC chart of Example 4 is shown.

[0054] Fig.10 The GPC chart of Example 5 is shown.

[0055] Fig.11 Example 5 1 H-NMR chart.

[0056] Fig.12 The GPC chart of Example 6 is shown.

[0057] Fig.13 The synthesis example 6 1 H-NMR chart.

[0058] Fig.14 The GPC chart of Example 7 is shown.

[0059] Fig.15 The GPC chart of Example 8 is shown.

[0060] Fig.16 The GPC chart of Example 9 is shown.

[0061] Fig.17 The GPC chart of Example 10 is shown.

[0062] Fig.18 Example 10 1 H-NMR chart.

[0063] Fig.19The GPC chart of Example 11 is shown.

[0064] Fig. 20 Example 11 1 H-NMR chart.

[0065] Fig.21 The GPC chart of Example 12 is shown.

[0066] Fig. 22 Example 12 1 H-NMR chart.

[0067] Fig.23 The GPC chart of Example 13 is shown.

[0068] Fig.24 Example 13 1 H-NMR chart.

[0069] Fig.25 The GPC chart of Example 14 is shown.

[0070] Fig.26 Example 14 1 H-NMR chart.

[0071] Fig. 27 The GPC chart of Example 15 is shown.

[0072] Fig.28 Example 15 1 H-NMR chart. DETAILED DESCRIPTION

[0073] The maleimide resin of the present invention is obtained by reacting a styrene / maleic acid copolymer, a compound having two or more amino groups in the molecule, and maleic anhydride.

[0074] The maleimide resin of the present invention preferably has repeating units of the following formulae (a) and (b).

[0075]

[0076] In the above formula, X represents an arbitrary organic group. m and n are respectively the average values ​​of the number of repetitions, 1≤m≤1000, 1≤n≤1000. (a) and (b) are respectively bonded with * and the repetition positions may be random.

[0077] m is usually 1≤m≤1000, preferably 2≤m≤750, and more preferably 3≤m≤500. n is usually 1≤n≤1000, preferably 1≤n≤500, more preferably 1.1≤n≤100, and even more preferably 1.1≤n≤20. The values ​​of m and n are derived from the styrene / maleic acid copolymer as a raw material, and can be obtained by its acid value. The preferred range of the molecular weight (weight average molecular weight (Mw) measured by colloid permeation chromatography (hereinafter referred to as GPC)) of the styrene / maleic acid copolymer as a raw material is preferably 200 or more and less than 50,000, more preferably 300 or more and less than 30,000, and even more preferably 400 or more and less than 20,000. If the weight average molecular weight is less than 20,000, water washing and purification becomes easier, and if it is 200 or more, the target compound will not volatilize in the solvent removal step.

[0078] In the aforementioned formula (b), X is preferably any one or more of the following formulae (A) to (P), more preferably any one of the following formulae (A) to (F), and even more preferably the following formula (B).

[0079]

[0080] In the above formulae (A) to (P), R represents a hydrocarbon group having 1 to 10 carbon atoms. a represents an integer from 0 to 4. p represents the average value of the number of repetitions, 0≤p≤20. * represents a bonding position. In addition, the average value p of the number of repetitions of formula (E) can be calculated from the number average molecular weight (Mn) value obtained by GPC measurement of the compound represented by formula (E) or the area % of the stratified data of each peak (detector: differential refractive index detector), etc.

[0081] In the above formulas (A) to (P), R is usually a hydrocarbon group having 1 to 10 carbon atoms, preferably a hydrocarbon group having 1 to 5 carbon atoms, and more preferably a hydrocarbon group having 1 to 3 carbon atoms. When R is a hydrocarbon having 10 or less carbon atoms, molecular vibration is not easily generated when exposed to high frequencies, and thus the electrical properties are excellent.

[0082] The styrene / maleic acid copolymer, which is the raw material of the maleimide resin of the present invention, can be obtained by copolymerizing styrene and maleic anhydride. The polymerization method can use free radical polymerization or coordination polymerization, various living polymerizations, and any publicly known method, but for example, it can be obtained by reacting styrene and maleic anhydride in toluene in the presence of a free radical polymerization initiator. At this time, the obtained polymer can be a random polymer or a periodic copolymer, or a block polymer or an alternating copolymer. In addition, the stereoregularity of the polystyrene segment can be any of syndiotactic, heterotactic, or homotactic. The molecular weight is preferably 500 to 50000, more preferably 750 to 40000, more preferably 1000 to 30000, and particularly preferably 1500 to 20000 in terms of weight average molecular weight (Mw). When the molecular weight is less than 500, the obtained target is easy to volatilize, and the weight of the resin component will decrease when heated, so it is difficult to be applied to the manufacturing process of the substrate material. In addition, when the molecular weight is greater than 30000, it is difficult to stir during manufacturing and difficult to wash and purify.

[0083] As the compound having two or more amine groups in the molecule of the raw material of the maleimide resin of the present invention, any publicly known amine compound can be used. Examples thereof include amine compounds represented by the following formulas (A') to (P'), methylenediamine, ethylenediamine, propylenediamine, butylenediamine, pentamethylenediamine, hexamethylenediamine, trimethylhexamethylenediamine, dimer diamine, 1,3-bisaminomethylcyclohexane, norbornanediamine, isophoronediamine, bisaminomethyltricyclodecane and other aliphatic diamine compounds.

[0084] The dimer diamine is a diamine in which the two terminal carboxylic acid groups (-COOH) of the dimer acid are substituted with primary aminomethyl groups (-CH2-NH2) or amine groups (-NH2). The dimer diamine can be a publicly known commercial product. Examples of commercial products include Priamine (registered trademark) manufactured by CRODA JAPAN.

[0085] The compounds having two or more amine groups in the above-mentioned molecules are preferably dimer diamines, or any one or more of the following formulas (A') to (P'), more preferably any one of the following formulas (A') to (F'), and more preferably the following formula (B'). This is because by using an amine compound having a molecular weight distribution, heat resistance or solvent solubility can be improved. In addition, these can be used alone or in combination.

[0086]

[0087] In the above formulae (A') to (P'), R represents a hydrocarbon group having 1 to 10 carbon atoms. a represents an integer from 0 to 4. p represents the average value of the number of repetitions, 0≤p≤20. n represents the average value of the number of repetitions, 1≤n<5.

[0088] In addition, the average value p of the number of repetitions of formula (E') and the average value n of the number of repetitions of formulas (A'), (B'), (C'), (D'), and (F') can be calculated from the number average molecular weight (Mn) value obtained by GPC measurement of the compounds represented by formulas (A') to (F') or the area % of the stratified data of each peak (detector: differential refractive index detector), etc.

[0089] In the above formulas (A') to (P'), R is usually a hydrocarbon group with 1 to 10 carbon atoms, preferably 1 to 5 carbon atoms, and more preferably 1 to 3 carbon atoms. When R is a hydrocarbon group with 10 carbon atoms or less, it is not easy to produce molecular vibration when exposed to high frequencies, so the electrical properties are excellent. In addition, it is more preferred that p is 1≤p≤20 and n is 1 <n<5。

[0090] In the above formula (B'), it is particularly preferred that a is 0, that is, the following formula (1).

[0091]

[0092] In formula (1), n ​​is the average value of the number of repetitions, and 1≤n<5. The average value of the number of repetitions n in formula (1) can be calculated from the number average molecular weight (Mn) value obtained by GPC measurement of the compound represented by formula (1) or the area % of the stratified data of each peak (detector: differential refractive index detector), etc.

[0093] The above formula (E') is particularly preferably the following formula (2).

[0094]

[0095] In formula (2), R is independently a hydrocarbon group having 1 to 3 carbon atoms, p is an average value of the number of repetitions, and 0≤p≤20. The average value of the number of repetitions p in formula (2) can be calculated from the number average molecular weight (Mn) value obtained by GPC measurement of the compound represented by formula (2) or the area % of the stratified data of each peak (detector: differential refractive index detector), etc.

[0096] In the above formula (F'), a is particularly preferably 2 and n is 0, that is, the following formula (3), or a is particularly preferably 0, that is, the following formula (4).

[0097]

[0098] In formula (3), R each independently represents a hydrocarbon group having 1 to 3 carbon atoms.

[0099]

[0100] In formula (4), n is the average value of the number of repetitions, and 1 < n < 5. The average value n of the number of repetitions in formula (4) can be calculated from the number average molecular weight (Mn) value obtained by GPC measurement of the compound represented by formula (4) or the area percentage of the layered data of each peak (detector: differential refractive index detector), etc.

[0101] The above formula (C’) is particularly preferably a = 0, that is, the following formula (5).

[0102]

[0103] In formula (5), n is the average value of the number of repetitions, and 1 ≤ n < 5. The average value n of the number of repetitions in formula (5) can be calculated from the number average molecular weight (Mn) value obtained by GPC measurement of the compound represented by formula (5) or the area percentage of the layered data of each peak (detector: differential refractive index detector), etc.

[0104] The method for producing the maleimide resin of the present invention is not particularly limited, and it can be produced from a styrene / maleic acid copolymer, a compound having two or more amino groups in the molecule, and maleic anhydride.

[0105] Specifically, it can be obtained by the following method: through the first step of imidizing a styrene / maleic acid copolymer with a compound having two or more amine groups in the molecule in a solvent in the presence of a catalyst, and as a second step, maleic anhydride is added and maleimidized. In the imidization of the first step, the amine group of the amine compound is added in excess of 1 mole of anhydride contained in the styrene / maleic acid copolymer, thereby preventing the gelation caused by the three-dimensional crosslinking in the reaction step. At this time, the preferred range of the value (α / β) of the mole number (α) of the amine group of the raw material amine divided by the mole number (β) of the anhydride of the styrene / maleic acid copolymer is preferably 1.1 to 20, more preferably 1.1 to 15, and more preferably 1.1 to 10. Amines will produce gelation when they do not reach the above range, so it is difficult to manufacture. In addition, when the above range is exceeded, the amount of polystyrene introduced will be reduced, and the electrical properties cannot be fully improved. The solvent used may include aromatic solvents such as toluene and xylene, aliphatic solvents such as cyclohexane and n-hexane, ethers such as diethyl ether and diisopropyl ether, ester solvents such as ethyl acetate and butyl acetate, ketone solvents such as methyl isobutyl ketone and cyclopentanone, etc., but it is not limited to these, and two or more kinds may be used in combination. In addition, in addition to the aforementioned non-water-soluble solvent, aprotic polar solvents may also be used in combination. For example, dimethyl sulfone, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, N-methylpyrrolidone (Methyl pyrrolidone), etc. may be mentioned, and two or more kinds may also be used in combination. When using aprotic polar solvents, it is more preferred to use a boiling point higher than the non-water-soluble solvent used in combination. During the reaction, hydrochloric acid, phosphoric acid, sulfuric acid, formic acid, p-toluenesulfonic acid, methanesulfonic acid, Lewis acids such as aluminum chloride and zinc chloride, activated clay, acid clay, white carbon, zeolite, solid acids such as silica alumina, acidic ion exchange resins, etc. can be used as catalysts. These can be used alone or in combination of two or more. The amount of the catalyst used is usually 0.1 to 0.8 moles, preferably 0.2 to 0.7 moles, relative to 1 mole of the amino group of the amine compound used. If the amount of the catalyst used is too much, the viscosity of the reaction solution will be too high, and there is a concern that it is difficult to stir. If it is too little, there is a concern that the reaction will slow down. In addition, as a co-catalyst for imidization, a basic co-catalyst such as triethylamine can be used alone or in combination. When sulfonic acid or the like is used as a catalyst, it can be neutralized with an alkali metal such as sodium hydroxide or potassium hydroxide before the extraction step. In the extraction step, an aromatic hydrocarbon solvent such as toluene or xylene can be used alone, or a non-aromatic hydrocarbon such as cyclohexane or toluene can be used in combination. After the extraction, the organic layer is washed with water until the drainage becomes neutral, and the solvent is distilled off using an evaporator or the like, thereby obtaining the target maleimide resin having a polystyrene structure in the molecule.

[0106] The maleimide resin having the repeating units of the formulae (a) and (b) can be represented by the following formula (6).

[0107]

[0108] In the above formula (6), X represents an arbitrary organic group. m and n are respectively the average values ​​of the number of repetitions, 1≤m≤1000, 1≤n≤1000. The values ​​of m and n are derived from the styrene / maleic acid copolymer as a raw material, and can be obtained from its acid value. Although each repeating unit is represented in a specific order for the convenience of recording, each repeating position can be random.

[0109] In the above formula (6), the more preferred ranges of X, m and n are the same as those in the above formulas (a) and (b).

[0110] The curable resin composition of the present invention may contain a polymerization inhibitor. By containing a polymerization inhibitor, the storage stability can be improved and the reaction starting temperature can be controlled. By controlling the reaction starting temperature, it is easy to ensure fluidity, and the impregnation property into glass cloth etc. will not be impaired, and B-stage formation such as prepreg is easier. During prepreg, if the polymerization reaction is excessive, it is easy to cause unfavorable situations such as difficulty in lamination in the lamination step.

[0111] The polymerization inhibitors that can be used include phenolic, sulfuric, phosphorus, hindered amine, nitroso, nitroxide free radicals and the like. The polymerization inhibitor can be added during the synthesis of the maleimide resin of the present invention, or can be added after the synthesis. In addition, the polymerization inhibitor can be used alone or in combination of two or more. The amount of the polymerization inhibitor used is usually 0.008 to 1 part by weight relative to 100 parts by weight of the resin component, and more preferably 0.01 to 0.5 parts by weight. These polymerization inhibitors can be used alone or in combination of two or more. In the present invention, phenolic, hindered amine, nitroso, and nitroxide free radicals are more preferred.

[0112] Specific examples of phenolic polymerization inhibitors include 2,6-di-tert-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-tert-butyl-p-ethylphenol, stearyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, isooctyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylanilino)-1,3,5-tris(2-hydroxy-3,5-di-tert-butylphenyl) propionate, Monophenols such as 2,4-bis[(octylthio)methyl]-o-cresol; 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylenebis(3-methyl-6-tert-butylphenol), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxy phenyl) propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid), 2,2-thio-divinylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 3,5-di-tert-butyl-4-hydroxybenzyl diethyl phosphate, 3,9-bis[1, 1-dimethyl-2-{β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]2,4,8,10-tetraoxaspiro[5,5]undecane, bis(3,5-di-tert-butyl-4-hydroxybenzylsulfonate) calcium and other bisphenols; 1,1,3-tri(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tri(3,5- di-tert-butyl-4-hydroxybenzyl)benzene, tetra-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] methane, bis[3,3'-bis-(4'-hydroxy-3'-tert-butylphenyl) butyrate] diol, tri-(3,5-di-tert-butyl-4-hydroxybenzyl)-triisocyanate, 1,3,5-tris(3',5'-di-tert-butyl-4'-hydroxybenzyl)-S-tri -2,4,6-(1H,3H,5H)trione, tocopherol and other high molecular weight phenols.

[0113] Specific examples of the sulfur-based polymerization inhibitor include dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, and distearyl-3,3'-thiodipropionate.

[0114] Specific examples of the phosphorus-based polymerization inhibitor include triphenyl phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, tris(nonylphenyl) phosphite, diisodecyl pentaerythritol phosphite, tris(2,4-di-tert-butylphenyl) phosphite, cyclic neopentanetetraylbis(octadecyl)phosphite, cyclic neopentanetetraylbis(2,4-di-tert-butylphenyl)phosphite, cyclic neopentanetetraylbis(2,4-di-tert-butyl-4-methylphenyl)phosphite, bis[2 -tert-butyl-6-methyl-4-{2-(octadecyloxycarbonyl)ethyl}phenyl] hydrogen phosphite and other phosphites; 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(3,5-di-tert-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and other oxaphosphaphenanthrene oxides, etc.

[0115] Specific examples of hindered amine polymerization inhibitors include ADK STAB LA-40MP, ADK STAB LA-40Si, ADK STAB LA-402AF, ADK STAB LA-87, ADK STAB LA-82, ADK STAB LA-81, ADK STAB LA-77Y, ADK STAB LA-77G, ADK STAB LA-72, ADK STAB LA-68, ADK STAB LA-63P, ADK STAB LA-57, ADK STAB LA-52, Chimassorb2020FDL, Chimassorb944FDL, Chimassorb944LD, Tinuvin622SF, TinuvinPA144, Tinuvin765, Tinuvin770DF, TinuvinXT55FB, Tinuvin111FDL, Tinuvin783FDL, Tinuvin791FB, etc., but not limited to these.

[0116] Specific examples of the nitroso-based polymerization inhibitor include p-nitrosophenol, N-nitrosodiphenylamine, and ammonium salts of N-nitrosophenylhydroxylamine (cupferroalin), and ammonium salts of N-nitrosophenylhydroxylamine (cupferroalin) are more preferred.

[0117] Specific examples of the nitroxide-based polymerization inhibitor include di-tert-butyl nitroxide, 2,2,6,6-tetramethylpiperidine-1-oxide, 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxide, 4-oxo-2,2,6,6-tetramethylpiperidine-1-oxide, 4-amino-2,2,6,6-tetramethylpiperidine-1-oxide, 4-methoxy-2,2,6,6-tetramethylpiperidine-1-oxide, 4-acetoxy-2,2,6,6-tetramethylpiperidine-1-oxide, and 4-benzoyloxy-2,2,6,6-tetramethylpiperidine-1-oxide, but are not limited to these.

[0118] The curable resin composition of the present invention may also use any publicly known material as the curable resin other than the maleimide resin of the present invention. Specifically, phenol resin, epoxy resin, amine resin, resin containing active olefin, isocyanate resin, polyamide resin, polyimide resin, cyanate resin, acrylic resin, methallyl resin, active ester resin, etc. can be cited. One type can be used, or multiple types can be used in combination. In addition, from the perspective of heat resistance, adhesion, and balance of dielectric properties, epoxy resin, resin containing active olefin, and cyanate resin are more preferably contained. By containing these curable resins, the brittleness of the cured product can be improved and the metal adhesion can be improved, and the rupture of the package during solder reflow or reliability tests such as hot and cold cycles can be suppressed.

[0119] The amount of the curable resin used is preferably 10 times or less, more preferably 5 times or less, and particularly preferably 3 times or less relative to the maleimide resin of the present invention. In addition, the lower limit is preferably 0.5 times or more, and more preferably 1 times or more. If it is 10 times or less, the heat resistance or dielectric properties of the maleimide resin of the present invention can be utilized.

[0120] As phenol resin, epoxy resin, amine resin, active olefin-containing resin, isocyanate resin, polyamide resin, polyimide resin, cyanate resin, active ester resin, the following can be used as examples.

[0121] Phenolic resins: polycondensates of phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, hydroquinone, resorcinol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, o-phthalaldehyde, crotonaldehyde, cinnamaldehyde, furfural, etc.), phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl Polymers of phenols and ketones (such as acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, diphenyl ketone, etc.), phenol resins obtained by polycondensation of phenols and substituted biphenyls (such as 4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl) or substituted phenyls (such as 1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene and 1,4-bis(hydroxymethyl)benzene), polycondensates of bisphenols and various aldehydes, and polyphenylene ether compounds.

[0122] The polyphenylene ether compound can be any publicly known one, but from the viewpoint of heat resistance and electrical properties, a polyphenylene ether compound having an ethylenically unsaturated double bond is more preferred, and a polyphenylene ether compound having an acryloyl group, a methacryloyl group, or a styrene structure is more preferred. Commercially available products include SA-9000-111 (manufactured by SABIC, a polyphenylene ether compound having a methacryloyl group) or OPE-2St 1200 (manufactured by Mitsubishi Gas Chemical Co., Ltd., a polyphenylene ether compound having a styrene structure).

[0123] The number average molecular weight (Mn) of the polyphenylene ether compound is preferably 500 to 5000, more preferably 2000 to 5000, and even more preferably 2000 to 4000. If the molecular weight is less than 500, the heat resistance of the cured product may not be sufficiently obtained. In addition, if the molecular weight exceeds 5000, the melt viscosity will increase, and sufficient fluidity may not be obtained, so there is a tendency for poor molding. In addition, the reactivity will also decrease, the curing reaction will take a long time, and the unreacted compounds will increase due to the inability to enter the curing system, and the glass transition temperature of the cured product will decrease, and there is a tendency for the heat resistance of the cured product to decrease.

[0124] When the number average molecular weight of the polyphenylene ether compound is 500 to 5000, it can exhibit excellent heat resistance and moldability while maintaining excellent dielectric properties. Specifically, the number average molecular weight can be measured using colloid permeation chromatography or the like.

[0125] The polyphenylene ether compound can be obtained by polymerization reaction, or it can be obtained by redistribution reaction of a high molecular weight polyphenylene ether compound with a number average molecular weight of about 10,000 to 30,000. In addition, these are reacted as raw materials with compounds having ethylenic unsaturated double bonds such as methacrylic acid chloride, acrylic acid chloride, chloromethyl styrene, etc., thereby free radical polymerizability can be imparted. The polyphenylene ether compound obtained by the redistribution reaction can be obtained by, for example, heating a high molecular weight polyphenylene ether compound in a solvent such as toluene in the presence of a phenolic compound and a free radical initiator and performing a redistribution reaction. As described above, the polyphenylene ether compound obtained by the redistribution reaction has a hydroxyl group derived from a phenolic compound at both ends of the molecular chain that contributes to hardening, so high heat resistance can be further maintained, and the compound having ethylenic unsaturated double bonds can also introduce functional groups at both ends of the molecular chain after modification, which is more preferred from this point of view. In addition, the polyphenylene ether compound obtained by the polymerization reaction shows excellent fluidity, which is more preferred from this point of view.

[0126] When a polyphenylene ether compound is obtained by a polymerization reaction, the molecular weight of the polyphenylene ether compound can be adjusted by adjusting the polymerization conditions, etc. In addition, in the case of a polyphenylene ether compound obtained by a redistribution reaction, the molecular weight of the obtained polyphenylene ether compound can be adjusted by adjusting the conditions of the redistribution reaction, etc. More specifically, it can be considered to adjust the amount of the phenolic compound used in the redistribution reaction. That is, the more the amount of the phenolic compound is blended, the lower the molecular weight of the obtained polyphenylene ether compound will be. At this time, a high molecular weight polyphenylene ether compound for redistribution reaction can use poly(2,6-dimethyl-1,4-phenylene ether) and the like. In addition, the phenolic compound used in the aforementioned redistribution reaction is not particularly limited. For example, it is more preferred to use a multifunctional phenolic compound having two or more phenolic hydroxyl groups in the molecule such as bisphenol A, phenol novolac, cresol novolac, etc. These can be used alone or in combination of two or more.

[0127] The content of the polyphenylene ether compound is not particularly limited, but is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, relative to the total mass of the curable resin component. When the content of the polyphenylene ether compound is 10 to 90% by mass, it is preferred because heat resistance and the like are excellent, and a cured product that fully exhibits the excellent dielectric properties of the polyphenylene ether compound can be obtained.

[0128] Epoxy resin: a glycidyl ether epoxy resin obtained by glycidylating the above-mentioned phenol resins, alcohols, etc., an alicyclic epoxy resin represented by 4-vinyl-1-cyclohexene diepoxide or 3,4-epoxycyclohexylmethyl-3,4'-epoxycyclohexanecarboxylic acid radical, a glycidylamine epoxy resin represented by tetraglycidyldiaminodiphenylmethane (TGDDM) or triglycidylparaaminophenol, and a glycidyl ester epoxy resin.

[0129] Amine resin: diaminodiphenylmethane, diaminodiphenyl sulfone, isophoronediamine, naphthalene diamine, aniline novolac, o-ethylaniline novolac, aniline resin obtained by reaction of aniline with chlorinated xylene, aniline and substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) described in Japanese Patent No. 6429862, or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene and 1,4-bis(hydroxymethyl)benzene, etc.).

[0130] Resins containing active olefins: polycondensates of the above-mentioned phenol resins and halogen compounds containing active olefins (chloromethylstyrene, allyl chloride, methallyl chloride, acrylic acid chloride, allyl chloride, etc.), phenols containing active olefins (2-allylphenol, 2-propenylphenol, 4-allylphenol, 4-propenylphenol, eugenol, isoeugenol, etc.) and halogen compounds (4,4'-bis(methoxymethyl)-1,1'-biphenyl, 1,4-bis(chloromethyl)benzene, 4,4'-difluorodiphenyl ketone, 4,4'-dichlorodiphenyl ketone, 4,4'-dibromodiphenyl ketone, cyanuric chloride, etc.) Polycondensates of bis(maleimide) and bis(maleimide) of poly(chloro) esters, etc.), polycondensates of epoxy resins or alcohols and substituted or unsubstituted acrylates (acrylates, methacrylates, etc.), maleimide resins (4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, m-phenylene bismaleimide, 2,2'-bis[4-(4-maleimidephenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimidephenoxy)benzene, 1,3-bis(4-maleimidephenoxy)benzene), phenol aralkyl type maleimide resins (ANILIX-MI, MITSUI FINE CHEMICALS Co., Ltd.), biphenyl aralkyl type maleimide resin (a resin solution containing the maleimide resin (M2) described in Example 4 of JP-A-2009-001783 is solidified by distilling off the solvent under reduced pressure), and bisamino isopropylphenylbenzene type maleimide (maleimide resin described in International Publication No. 2020 / 054601).

[0131] Isocyanate resin: aromatic diisocyanates such as p-phenylene diisocyanate, m-phenylene diisocyanate, p-xylene diisocyanate, m-xylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, and naphthalene diisocyanate; diisocyanates with aliphatic or alicyclic structures such as isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, hydrogenated xylene diisocyanate, norbornene diisocyanate, and lysine diisocyanate; polyisocyanates such as biuret forms of one or more isocyanate monomers, or isocyanate forms of the above diisocyanate compounds in a quantity of 3; polyisocyanates obtained by urea esterification of the above isocyanate compounds with polyol compounds.

[0132] Polyamide resin: a polymer with one or more selected from amino acids (6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, p-aminomethylbenzoic acid, etc.) and lactams (ε-caprolactam, ω-undecanealactam, ω-laurolactam) as main raw materials; or a polymer with one or more diamines and one or more dicarboxylic acids as main raw materials.

[0133] Diamines: aliphatic diamines such as ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decanediamine, undecanediamine, dodecanediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,5-diaminopentane, 2-methyl-1,8-diaminooctane; alicyclic diamines such as cyclohexanediamine, bis-(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane; aromatic diamines such as xylenediamine, etc.

[0134] Dicarboxylic acids: aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; dialkyl esters and dichlorides of these dicarboxylic acids.

[0135] Polyimide resin: a polycondensate of the aforementioned diamine and tetracarboxylic dianhydride.

[0136] Tetracarboxylic dianhydride: 4,4'-(hexafluoroisopropylidene) diphthalic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-cyclohexene-1,2-dicarboxylic anhydride, pyromelite dianhydride, 1,2,3,4-benzene tetracarboxylic anhydride, 3,3',4,4'-diphenyl ketone tetracarboxylic anhydride, 2,2',3,3'-diphenyl ketone tetracarboxylic anhydride, 3,3',4,4'-biphenyl tetracarboxylic anhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic anhydride, 2,2',3,3'-biphenyl tetracarboxylic anhydride, methylene-4,4'-diphthalic anhydride, 1,1-ethylene-4,4'-diphthalic anhydride, 2,2'-propylene-4,4'-diphthalic anhydride, 1 ,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride, thio-4,4'-diphthalic dianhydride, sulfonyl-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)phthalic dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic dianhydride, 1,4-bis[2-(3,4-dicarboxyphenyl) 2-propyl]phthalic anhydride, bis[3-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, 2,2-bis[3-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, bis(3,4-dicarboxyphenoxy)dimethylsilane dianhydride, 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic anhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride, 1,2,5,6-naphthalenetetracarboxylic anhydride, 3,4,9,10-perylenetetracarboxylic anhydride, 2,3,6,7-anthracenetetracarboxylic anhydride, 1,2, 7,8-phenanthrenetetracarboxylic dianhydride, ethylenetetracarboxylic dianhydride, 1,2,3,4-butanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, cyclohexane-1,2,3,4-tetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride, 3,3',4,4'-dicyclohexyltetracarboxylic dianhydride, carbonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, methylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,2-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,1-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 2,2-propylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, sulfenyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, sulfonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, rel-[1S,5R,6R]-3-oxabicyclo[3,2 ,1] octane-2,4-dione-6-spiro-3'-(tetrahydrofuran-2',5'-dione), 4-(2,5-dioxo-tetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride, ethylene glycol-bis-(3,4-dicarboxylic anhydride phenyl) ether, 4,4'-biphenyl bis(trimellitic acid monoester anhydride), 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride. ,

[0137] Cyanate resin: a cyanate compound obtained by reacting a phenol resin with a halogenated cyanine, and specific examples thereof include dicyanate benzene, tricyanate benzene, dicyanate naphthalene, dicyanate biphenyl, 2,2'-bis(4-cyanate phenyl)propane, bis(4-cyanate phenyl)methane, bis(3,5-dimethyl-4-cyanate phenyl)methane, 2,2'-bis(3,5-dimethyl-4-cyanate phenyl)propane, 2,2'-bis(4-cyanate phenyl)ethane, 2,2'-bis(4-cyanate phenyl)hexafluoropropane, bis(4-cyanate phenyl)sulfone, bis(4-cyanate phenyl)sulfide, phenol novolac cyanate, and a hydroxyl group of a phenol / dicyclopentadiene co-condensate converted to a cyanate group, but are not limited thereto.

[0138] In addition, the cyanate compound described in the synthesis method of Japanese Patent Application Laid-Open No. 2005-264154 is particularly preferred as the cyanate compound because of its low hygroscopicity, flame retardancy, and excellent dielectric properties.

[0139] Cyanate resins are used to tri-quantify the cyanate groups and form sym-tri The curable resin composition may contain a catalyst such as zinc naphthenate, cobalt naphthenate, copper naphthenate, lead naphthenate, zinc octylate, tin octylate, lead acetylacetonate, dibutyltin maleate, etc. The catalyst is usually used in an amount of 0.0001 to 0.10 parts by mass, preferably 0.00015 to 0.0015 parts by mass, based on 100 parts by mass of the total mass of the curable resin composition.

[0140] Active ester resin: A compound having one or more active ester groups in one molecule can be optionally used as a hardener for curable resins other than the maleimide resin of the present invention such as epoxy resin. The active ester hardener is preferably a compound having two or more highly reactive ester groups in one molecule such as phenol esters, thiophenol esters, N-hydroxylamine esters, and esters of heterocyclic hydroxyl compounds. The active ester hardener is preferably obtained by a condensation reaction of at least one of a carboxylic acid compound and a thiocarboxylic acid compound with at least one of a hydroxyl compound and a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester hardener obtained from a carboxylic acid compound and a hydroxyl compound is more preferred, and an active ester hardener obtained from a carboxylic acid compound and at least one of a phenol compound and a naphthol compound is more preferred.

[0141] Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyrophyllic acid.

[0142] Examples of phenolic compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, acid phenolphthalin, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxydiphenyl ketone, trihydroxydiphenyl ketone, tetrahydroxydiphenyl ketone, phloroglucinol, benzenetriol, dicyclopentadiene-type diphenolic compounds, phenol novolac, etc. Here, the "dicyclopentadiene-type diphenolic compound" refers to a diphenolic compound obtained by condensing two molecules of phenol with one molecule of dicyclopentadiene.

[0143] Preferred specific examples of active ester curing agents include active ester compounds containing a dicyclopentadiene diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of a phenol novolac, and active ester compounds containing a benzoylated product of a phenol novolac. Among them, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene diphenol structure are more preferred. "Dicyclopentadiene diphenol structure" means a divalent structural unit composed of phenylene-dicyclopentylene-phenylene.

[0144] Examples of commercially available active ester hardeners include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", "EXB-8000L-65TM", and "EXB-8150-65T" (manufactured by DIC Corporation) as active ester compounds containing a dicyclopentadiene-type diphenol structure; and "EXB9416-70BK" (manufactured by DIC Corporation) as an active ester compound containing a naphthalene structure. ; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester compound containing an acetylated product of phenol novolac; "YLH1026", "YLH1030", "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester compounds containing benzoylated products of phenol novolac; "DC808" (manufactured by Mitsubishi Chemical Corporation) as active ester hardeners of acetylated products of phenol novolac; "EXB-9050L-62M" manufactured by DIC Corporation and the like as active ester hardeners containing phosphorus atoms.

[0145] The curable resin composition of the present invention may be used in combination with a curing accelerator (curing catalyst) to improve curability. For the purpose of promoting the self-polymerization of a curable resin that can be free radically polymerized, such as an olefin compound or a maleimide resin, or promoting free radical polymerization with other components, a specific example of a curing accelerator that can be used is preferably a free radical polymerization initiator. Examples of the free radical polymerization initiator include ketone peroxides such as methyl ethyl ketone peroxide and acetylacetone peroxide, diacyl peroxides such as benzoyl peroxide, diisopropylbenzene peroxide, dialkyl peroxides such as 1,3-bis-(tert-butyl isopropyl peroxide)-benzene, peroxyketals such as tert-butyl peroxide of benzoic acid and 1,1-diperoxytert-butylcyclohexane, α-isopropyl peroxide of neodecanoate, tert-butyl peroxide of neodecanoate, tert-butyl peroxide of neopentanoate, 1,1,3,3-tetramethylbutyl peroxide of 2-ethylhexanoate, tert-amyl peroxide of 2-ethylhexanoate, tert-butyl peroxide of 2-ethylhexanoate, 3,5,5-trimethylhexanoate peroxide The hardening accelerators include tert-amyl ester, tert-butyl peroxide 3,5,5-trimethylhexanoate, tert-amyl peroxide benzoate and other alkyl peroxyesters, di-2-ethylhexyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, tert-butyl peroxyisopropyl carbonate, 1,6-bis(tert-butylperoxycarbonyloxy)hexane and other peroxycarbonates, tert-butyl hydroperoxide, isopropyl hydroperoxide, tert-butyl peroxide octanoate, lauroyl peroxide and other organic peroxides, or azo compounds such as azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile) and the like, but are not limited thereto. Ketone peroxides, diacyl peroxides, hydroperoxides, dialkyl peroxides, peroxyketals, alkyl peroxyesters, peroxycarbonates and the like are more preferred, and dialkyl peroxides are more preferred. The amount of the radical polymerization initiator added is preferably 0.01 to 5 parts by mass, more preferably 0.01 to 3 parts by mass, relative to 100 parts by mass of the curable resin composition. If the amount of the radical polymerization initiator used is too large, the molecular weight cannot be sufficiently increased during the polymerization reaction.

[0146] In addition, a curing accelerator other than the radical polymerization initiator may be optionally added or used in combination. Specific examples of the curing accelerator that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo(5,4,0)undecene-7, phosphines such as triphenylphosphine, quaternary ammonium salts such as tetrabutylammonium salts, triisopropylmethylammonium salts, trimethyldecylammonium salts, cetyltrimethylammonium salts, and hexadecyltrimethylammonium hydroxide, and triphenylbenzylphosphonium salts. , triphenylethylphosphonium salt, tetrabutylphosphonium salt and other quaternary phosphonium salts (the counter ions of the quaternary salts are halogen, organic acid ions, hydroxide ions, etc., and are not particularly specified, but organic acid ions and hydroxide ions are particularly preferred), tin octoate, zinc carboxylates (zinc 2-ethylhexanoate, zinc stearate, zinc behenate, zinc myristate) or zinc phosphates (octyl zinc phosphate, stearyl zinc phosphate, etc.) and other zinc compounds (transition metal salts), etc. The blending amount of the hardening accelerator is 0.01 to 5.0 parts by weight relative to 100 parts of the epoxy resin.

[0147] The curable resin composition of the present invention may contain a phosphorus-containing compound as a flame retardancy imparting component. The phosphorus-containing compound may be a reactive type or an additive type. Specific examples of the phosphorus-containing compound include trimethyl phosphate, triethyl phosphate, tricresyl phosphate, tris(thio)phosphate, cresyl diphenyl phosphate, cresyl-2,6-di(xylylene) phosphate, Phosphates such as phosphate, 1,3-phenylenebis(di(xylyl)phosphate), 1,4-phenylenebis(di(xylyl)phosphate), 4,4'-biphenyl(di(xylyl)phosphate); phosphanes such as 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide; phosphorus-containing epoxy compounds obtained by the reaction of epoxy resin with active hydrogen of the aforementioned phosphanes, red phosphorus, etc., preferably phosphates, phosphanes or phosphorus-containing epoxy compounds, more preferably 1,3-phenylenebis(di(xylyl)phosphate), 1,4-phenylenebis(di(xylyl)phosphate), 4,4'-biphenyl(di(xylyl)phosphate) or phosphorus-containing epoxy compounds. The phosphorus-containing compound content is preferably in the range of (phosphorus-containing compound) / (full epoxy resin) from 0.1 to 0.6 (weight ratio). If it is less than 0.1, the flame retardancy is insufficient, and if it exceeds 0.6, there is a concern that the hygroscopicity and dielectric properties of the cured product may be adversely affected.

[0148] In addition, the curable resin composition of the present invention may optionally contain a light stabilizer. The light stabilizer is preferably a hindered amine light stabilizer (HALS). HALS is not particularly limited, and a representative example is dibutylamine / 1,3,5-tributylamine. / N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidinyl)butylamine polycondensate, dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, poly〔{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-tri bis(1,2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, 2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-n-butylmalonate bis(1,2,2,6,6-pentamethyl-4-piperidinyl), and the like. Only one type of HALS may be used, or two or more types may be used in combination.

[0149] In addition, the curable resin composition of the present invention may be optionally blended with a binder resin. Examples of the binder resin include butyral resins, acetal resins, acrylic resins, epoxy-nylon resins, NBR-phenol resins, epoxy-NBR resins, polyamide resins, polyimide resins, and silicone resins, but are not limited thereto. The amount of the binder resin blended is preferably within a range that does not impair the flame retardancy and heat resistance of the cured product, and is preferably 0.05 to 50 parts by mass, more preferably 0.05 to 20 parts by mass, relative to 100 parts by mass of the resin component.

[0150] In addition, the curable resin composition of the present invention may optionally contain fused silica, crystalline silica, porous silica, alumina, zircon, calcium silicate, calcium carbonate, quartz powder, silicon carbide, silicon nitride, boron nitride, zirconium dioxide, aluminum nitride, graphite, forsterite, steatite, spinel, mullite, titanium dioxide, talc, clay, iron oxide asbestos, glass powder and other powders, or inorganic fillers formed into spherical or crushed forms thereof. In addition, in particular, when obtaining a curable resin composition for semiconductor sealing, the amount of the above-mentioned inorganic filler used is generally 80 to 92% by mass in the curable resin composition, and more preferably 83 to 90% by mass.

[0151] The curable resin composition of the present invention may be optionally blended with publicly known additives. Specific examples of usable additives include polybutadiene and its modified products, modified products of acrylonitrile copolymers, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, silicone gel, silicone oil, silane coupling agent and other filler surface treatment agents, mold release agents, carbon black, phthalocyanine blue, phthalocyanine green and other colorants. The amount of these additives blended is preferably 1,000 parts by mass or less, and more preferably 700 parts by mass or less, relative to 100 parts by mass of the curable resin composition. From the viewpoint of low water absorption and electrical properties, polybutadiene and its modified products, polyphenylene ether, polystyrene, polyethylene, fluororesin and the like are more preferred. From the viewpoint of electrical properties, adhesion and low water absorption, polybutadiene and its modified products are more preferred. Specifically, examples include butadiene-based thermoplastic elastomers such as styrene butadiene copolymers (SBR: RICON-100, RICON-181, RICON-184, all manufactured by Cray Valley Co., Ltd.), acrylonitrile butadiene copolymers, and styrene-based thermoplastic elastomers such as styrene butadiene styrene copolymers (SBS), hydrogenated styrene butadiene styrene copolymers, styrene isoprene styrene copolymers (SIS), hydrogenated styrene isoprene styrene copolymers, and hydrogenated styrene (butadiene / isoprene) styrene copolymers. These styrene-based thermoplastic elastomers may be used alone or in combination of two or more. Among these high molecular weight bodies, styrene-based thermoplastic elastomers such as styrene-butadiene-styrene copolymers, hydrogenated styrene-butadiene-styrene copolymers, styrene-isoprene-styrene copolymers, hydrogenated styrene-isoprene-styrene copolymers, and hydrogenated styrene-(butadiene / isoprene)-styrene copolymers are more preferred. In particular, styrene-isoprene-styrene copolymers, hydrogenated styrene-butadiene-styrene copolymers, hydrogenated styrene-isoprene-styrene copolymers, and hydrogenated styrene-(butadiene / isoprene)-styrene copolymers are more preferred because they have high heat resistance and are not easily degraded by oxidation.Specifically, there are SEPTON 1020, SEPTON 2002, SEPTON 2004F, SEPTON 2005, SEPTON 2006, SEPTON 2063, SEPTON 2104, SEPTON 4003, SEPTON 4044, SEPTON 4055, SEPTON 4077, SEPTON 4099, SEPTON 8004, SEPTON 8006, SEPTON 8007L, SEPTON HG252, SEPTON V9827, HYBRAR 7125 (hydrogenation), HYBRAR 7215F, HYBRAR 7311F (all manufactured by Kuraray Co., Ltd.). In addition, the weight average molecular weight of the styrene-based thermoplastic elastomer is not particularly limited if it is 10,000 or more. However, if it is too large, the compatibility with low molecular weight components other than the polyphenylene ether compound having a weight average molecular weight of about 50 to 1,000 and oligomer components having a weight average molecular weight of about 1,000 to 5,000 will be poor, and it will be difficult to ensure mixing and solvent stability, so it is more preferably about 10,000 to 300,000. In general, in the case of compounds containing heteroatoms such as oxygen or nitrogen such as bismaleimide or polymaleimide, it is difficult to ensure compatibility with low polar compounds such as compounds mainly composed of hydrocarbons or compounds composed only of hydrocarbons in the above-mentioned additives or the above-mentioned curing resin components due to their polarity. On the other hand, the maleimide resin of the present invention itself does not have a skeleton design that actively introduces heteroatoms such as oxygen and nitrogen (few polar groups), and therefore has excellent compatibility with materials having low polarity and low dielectric properties or compounds consisting only of hydrocarbons.

[0152] The curable resin composition of the present invention can be obtained by uniformly mixing the above-mentioned components at a specific ratio, and generally performing preliminary curing at 130 to 180° C. for 30 to 500 seconds, and further performing post-curing at 150 to 200° C. for 2 to 15 hours, thereby fully performing the curing reaction and obtaining the cured product of the present invention. Alternatively, the components of the curable resin composition may be uniformly dispersed or dissolved in a solvent, etc., and cured after removing the solvent.

[0153] The curable resin composition of the present invention thus obtained has moisture resistance, heat resistance, and high adhesion. Therefore, the curable resin composition of the present invention can be used in a wide range of fields requiring moisture resistance, heat resistance, and high adhesion. Specifically, it can be used as a material for various electrical and electronic parts such as insulating materials, laminated boards (printed wiring boards, BGA substrates, build-up substrates, etc.), sealing materials, and resists. In addition, it can also be used in the fields of molding materials, composite materials, coating materials, adhesives, 3D printing, etc. In particular, it helps to improve solder reflow resistance in semiconductor sealing.

[0154] The semiconductor device has a seal with the curable resin composition of the present invention. Examples of the semiconductor device include DIP (dual in-line package), QFP (quad flat package), BGA (ball grid array), CSP (chip size package), SOP (small outline package), TSOP (thin small outline package), TQFP (thin quad flat package), etc.

[0155] The preparation method of the curable resin composition of the present invention is not particularly limited, and the components may be simply mixed uniformly or prepolymerized. For example, the maleimide resin of the present invention may be heated in the presence or absence of a catalyst and in the presence or absence of a solvent to be prepolymerized. Similarly, in addition to the maleimide resin of the present invention, a curing agent such as an epoxy resin, an amine compound, a maleimide compound, a cyanate compound, a phenol resin, an acid anhydride compound, and other additives may be added to prepolymerize. The mixing or prepolymerization of the components may be performed in the absence of a solvent, for example, using an extruder, a kneader, a roller, etc., or in the presence of a solvent, using a reaction vessel equipped with a stirring device.

[0156] The uniform mixing method can form a uniform resin composition by kneading at a temperature in the range of 50 to 100°C using a kneader, a roller, a planetary mixer, etc. The obtained resin composition can be crushed and molded into a cylindrical flat plate, a granular powder, or a powdery molded body by a molding machine such as a flat bed, or melted on a surface support and molded into a sheet with a thickness of 0.05 mm to 10 mm to form a curable resin composition molded body. The obtained molded body is a molded body that does not feel sticky at 0 to 20°C, and the fluidity and curability are hardly reduced even if stored at -25 to 0°C for more than 1 week.

[0157] The obtained molded body can be molded into a hardened product using a transfer molding machine or a compression molding machine.

[0158] An organic solvent may be added to the curable resin composition of the present invention to form a varnish-like composition (hereinafter referred to as varnish). The curable resin composition of the present invention may be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc. to form a varnish, and then impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, paper, etc. and heated and dried to obtain a prepreg, and the prepreg is hot-pressed to form a cured product of the curable resin composition of the present invention. The solvent in this case is generally used in an amount of 10 to 70% by weight, preferably 15 to 70% by weight, in the mixture of the curable resin composition of the present invention and the solvent. In addition, if it is a liquid composition, a cured resin containing carbon fibers can be directly obtained, for example, by RTM (Resin Transfer Molding).

[0159] In addition, the curable resin composition of the present invention can be used as a modifier for film-type compositions. Specifically, it can be used in cases where flexibility in the B-stage is to be improved. The film-type resin composition can be obtained by applying the curable resin composition of the present invention as the curable resin composition varnish on a release film, removing the solvent under heating, and then B-staging to obtain a sheet-like adhesive. The sheet-like adhesive can be used as an interlayer insulating layer in a multilayer substrate, etc.

[0160] The curable resin composition of the present invention can be obtained by heating and melting, reducing viscosity and impregnating with reinforcing fibers such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, and alumina fiber to obtain a prepreg. Specific examples thereof include glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, as well as fibers of inorganic substances other than glass or poly(p-phenylene terephthalamide) (Kevlar (registered trademark), manufactured by DuPont Co., Ltd.), wholly aromatic polyamide, polyester; and organic fibers such as poly(p-phenylene benzoxazole), polyimide and carbon fiber, but are not limited to these. The shape of the substrate is not particularly limited, and examples thereof include woven fabrics, non-woven fabrics, rovings, chopped strands, and the like. In addition, the weaving methods of the woven fabrics are known to include plain weave, roe weave, twill weave, etc., which can be appropriately selected from these publicly known methods according to the intended use or performance. In addition, it is also suitable to use glass woven fabrics that are subjected to fiberization treatment or surface treatment with silane coupling agents, etc. The thickness of the substrate is not particularly limited, but is preferably about 0.01 to 0.4 mm. Alternatively, a prepreg may be obtained by impregnating the reinforcing fibers with the varnish and heating and drying the impregnated fibers.

[0161] The laminate of the present embodiment has one or more prepregs. As long as the laminate has one or more prepregs, there is no particular limitation, and it may have any other layers. The manufacturing method of the laminate can appropriately use generally known methods, and there is no particular limitation. For example, when forming a metal foil clad laminate, a multi-stage press, a multi-stage vacuum press, a continuous molding machine, an autoclave molding machine, etc. can be used, and the prepregs can be stacked on each other and heated and pressurized to obtain a laminate. At this time, the heating temperature is not particularly limited, and is preferably 65 to 300°C, and more preferably 120 to 270°C. In addition, the pressurization pressure is not particularly limited, but if the pressure is too large, it is difficult to adjust the solid content of the resin of the laminate, and the quality is unstable. In addition, if the pressure is too small, there will be bubbles or the adhesion between the layers will be deteriorated, so it is more preferably 2.0 to 5.0MPa, and more preferably 2.5 to 4.0MPa. The laminated plate of the present embodiment includes a layer composed of a metal foil, and thus can be suitably used as a metal foil clad laminated plate described later.

[0162] The above-mentioned prepreg is cut into a desired shape, and after being optionally laminated with copper foil or the like, a curable resin composition is heated and cured while applying pressure to the laminate by a press molding method, an autoclave molding method, a sheet winding molding method, or the like, thereby obtaining an electrical and electronic laminate (printed wiring board) or a carbon fiber reinforced material.

[0163] The cured product of the present invention can be used in various applications such as molding materials, adhesives, composite materials, coatings, etc. The cured product of the curable resin composition described in the present invention exhibits excellent heat resistance and dielectric properties, and is therefore suitable for use in semiconductor element sealing materials, liquid crystal display element sealing materials, organic EL element sealing materials, printed circuit boards, build-up laminates and other electrical and electronic parts, or composite materials for lightweight and high-strength structural materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics.

[0164] (Example)

[0165] The present invention will be further described in detail by way of examples. Unless otherwise specified, "parts" are parts by mass. In addition, the present invention is not limited to these examples.

[0166] Various analytical methods used in the examples are described below.

[0167] <Colloid Permeation Chromatography (GPC)>

[0168] The weight average molecular weight (Mw) and the number average molecular weight (Mn) were calculated in terms of polystyrene using a polystyrene standard solution.

[0169] GPC: DGU-20A3R, LC-20AD, SIL-20AHT, RID-20A, SPD-20A, CTO-20A, CBM-20A (all manufactured by Shimadzu Corporation).

[0170] Column:ShodexKF-603, KF-602x2, KF-601x2.

[0171] Connecting solvent: tetrahydrofuran.

[0172] Flow rate: 0.5ml / min.

[0173] Column temperature: 40°C.

[0174] Detection: RI (differential refractometer).

[0175] <High-speed liquid chromatography (HPLC)>

[0176] Column: Inertsil ODS-2 (GL Sciences).

[0177] Detector: UV274nm.

[0178] Temperature: 40℃.

[0179] Solvent: acetonitrile / water.

[0180] Flow rate: 1.0ml / min.

[0181] Injection volume: 5 μl (concentration: about 10 mg / 6 ml).

[0182] Gradient Program:

[0183] Acetonitrile / water;

[0184] Start with a 30 / 70 gradient → 100 / 0 after 28 minutes and keep it as is.

[0185] [Synthesis example 1]

[0186] In a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 559 parts of aniline, 291 parts of α,α,α',α'-tetramethylbenzenedimethanol (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), and 360 parts of toluene were added while nitrogen flushing was performed. Then, 63 parts of a 35% aqueous hydrochloric acid solution were added and stirring was started. While the water and toluene generated by dehydration were extracted, the internal temperature was raised to 160°C and the reaction was carried out for 15 hours. The mixture was cooled to room temperature, the extracted toluene and water were returned to the system, and 88 parts of a 30% aqueous sodium hydroxide solution were added to neutralize the mixture. Thereafter, the organic layer was washed with water until the waste liquid became neutral, and then concentrated to obtain 458 parts of an aromatic amine resin (A1) represented by the following formula (1-a). The amine equivalent of the aromatic amine resin (A1) was 185 g / eq, and the softening point was 58.7°C. According to GPC analysis (RI), the n=1 isomer is 61%, and the 4,4'-(1,3-phenylenediisopropylidene) dianiline in the n=1 isomer according to HPLC analysis is 16.7%, so the 4,4'-(1,3-phenylenediisopropylidene) dianiline in the aromatic amine resin is 10.2%. The GPC chart of the obtained aromatic amine resin (A1) is shown in Figure 1 , HPLC chart is shown in Figure 2 .in addition, 1 H-NMR chart (heavy chloroform) is shown in Figure 3 . 1 In the H-NMR chart, a signal derived from an amine group was observed at 3.05 to 3.65 ppm.

[0187]

[0188] [Example 1]

[0189] In a flask equipped with a thermometer, a cooling tube and a stirrer, 75 parts of toluene, 11.2 parts of a styrene / maleic acid copolymer (RK-69, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 50, Mw: 3000), 14.8 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1 and 0.6 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 4 hours. After cooling, 10.3 parts of maleic anhydride were added, and the reaction was continued under reflux for 16 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure to obtain the target compound (M-1) (Mn: 1460, Mw: 3239) as a brown solid resin. The GPC chart of the obtained compound during the reaction is shown in Figure 4 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Figure 5 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 7.08 ppm(s).

[0190] [Example 2]

[0191] In a flask equipped with a thermometer, a cooling tube and a stirrer, 75 parts of toluene, 11.2 parts of a styrene / maleic acid copolymer (SMAEF80, manufactured by Cray Valley, acid value: 120, Mw: 14400), 14.8 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1 and 0.6 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 4 hours. After cooling, 8.8 parts of maleic anhydride were added, and the reaction was continued under reflux for 16 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure to obtain the target compound (M-2) (Mn: 1556, Mw: 14314) as a brown solid resin. The GPC chart of the obtained compound during the reaction is shown in Figure 6 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Figure 7 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 7.08 ppm(s).

[0192] [Example 3]

[0193] In a flask equipped with a thermometer, a cooling tube and a stirrer, 75 parts of toluene, 11.2 parts of a styrene / maleic acid copolymer (RK-69, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 50, Mw: 3000), 11.2 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1, and 0.6 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 3 hours. After cooling, 7.4 parts of maleic anhydride were added, and the reaction was continued under reflux for 16 hours. After cooling, 50 parts of toluene were added, and the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 26.3 parts of the target compound (M-3) as a brown solid resin (Mn: 1378, Mw: 2875). The GPC chart of the obtained compound during the reaction is shown in Figure 8 .

[0194] [Example 4]

[0195] In a flask equipped with a thermometer, a cooling tube and a stirrer, 75 parts of toluene, 9.4 parts of a styrene / maleic acid copolymer (SMAEF80, manufactured by Cray Valley, acid value: 120, Mw: 14400), 7.4 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1 and 0.3 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 2 hours. After cooling, 2.9 parts of maleic anhydride were added, and the reaction was continued under reflux for 16 hours. After cooling, 100 parts of toluene were added, and the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining the target compound (M-4) (Mn: 2186, Mw: 14502) as a brown solid resin. The GPC chart of the obtained compound during the reaction is shown in Fig. 9 .

[0196] [Example 5]

[0197] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 75 parts of toluene, 11.2 parts of a styrene / maleic acid copolymer (RK-69, manufactured by Gifu Shellac Manufacturing, acid value: 50, Mw: 3000), 11.8 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1, 5.1 parts of dimer diamine (Priamine: manufactured by CRODA JAPAN), and 0.68 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 4 hours. After cooling, 10.3 parts of maleic anhydride were added, and the reaction was continued under reflux for 16 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 26.1 parts of the target compound (M-5) (Mn: 1444, Mw: 2998) as a brown solid resin. The GPC chart of the obtained compound during the reaction is shown in Fig.10 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig.11 . 1 In the H-NMR chart, signals derived from the maleimide group were observed at 6.82 (s) and 6.85 ppm (s).

[0198] [Example 6]

[0199] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 75 parts of toluene, 11.2 parts of a styrene / maleic acid copolymer (RK-69, manufactured by Gifu Shellac Manufacturing, acid value: 50, Mw: 3000), 5.4 parts of a dimer diamine (Priamine: manufactured by CRODA JAPAN), and 0.2 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 3 hours. After cooling, 1.5 parts of maleic anhydride were added, and the reaction was continued under reflux for 6 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 14.1 parts of the target compound (M-6) as a yellow solid resin (Mn: 3194, Mw: 4677). The GPC chart of the obtained compound during the reaction is shown in Fig.12 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig.13 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 6.82 ppm(s).

[0200] [Example 7]

[0201] In a flask equipped with a thermometer, a cooling tube and a stirrer, 75 parts of toluene, 9.4 parts of a styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 60, Mw: 10140), 11.2 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1 and 0.5 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 4 hours. After cooling, 7.4 parts of maleic anhydride were added, and the reaction was continued under reflux for 16 hours. After cooling, 100 parts of toluene were added, and the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 21.6 parts of the target compound (M-7) as a brown solid resin (Mn: 1834, Mw: 12628). The GPC chart of the obtained compound during the reaction is shown in Fig.14 .

[0202] [Example 8]

[0203] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 101 parts of toluene, 18.7 parts of a styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 60, Mw: 10140), 14.9 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1, and 0.6 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 4 hours. After cooling, 8.8 parts of maleic anhydride were added, and the reaction was continued under reflux for 16 hours. After cooling, 50 parts of toluene were added, and the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 35.2 parts of the target compound (M-8) as a brown solid resin (Mn: 2493, Mw: 19879). The GPC chart of the obtained compound is shown in Fig.15 .

[0204] [Example 9]

[0205] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 75 parts of toluene, 11.2 parts of a styrene / maleic acid copolymer (RK-69, manufactured by Gifu Shellac Manufacturing, acid value: 50, Mw: 3000), 14.8 parts of the aromatic amine resin (A1) obtained in Synthesis Example 1, and 0.6 parts of methanesulfonic acid were added, and the mixture was reacted at 110°C for 4 hours. After cooling, 10.3 parts of maleic anhydride were added, and the reaction was continued under reflux for 28 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The obtained organic layer was returned to the reaction vessel and azeotropically dehydrated under reflux for 30 minutes. 0.6 parts of methanesulfonic acid was added and reacted for 4 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 27.3 parts of the target compound (M-9) (Mn: 1619, Mw: 3395) as a brown solid resin. The GPC chart of the obtained compound during the reaction is shown in Fig.16 .

[0206] [Comparative Synthesis Example 1]

[0207] In a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation trap, and a stirrer, 147 parts of maleic anhydride, 300 parts of toluene, and 4 parts of methanesulfonic acid were added and heated to reflux. Then, a resin solution prepared by dissolving 197 parts of an aromatic amine resin (A1) in 95 parts of N-methyl-2-pyrrolidone and 100 parts of toluene was dripped in for 3 hours while maintaining a reflux state. During this time, the condensed water and toluene that were azeotropically distilled under reflux conditions were cooled and separated in the Dean-Stark azeotropic distillation trap, and then the toluene in the organic layer was returned to the system, and the water was discharged to the outside of the system. After the resin solution was dripped in, the reaction was carried out for 6 hours while maintaining a reflux state and performing a dehydration operation.

[0208] After the reaction, water washing was repeated 4 times to remove methanesulfonic acid and excess maleic anhydride, and water was removed from the system by azeotropy of toluene and water under heating and reduced pressure below 70°C. Then, 2 parts of methanesulfonic acid were added and reacted under heating and reflux for 2 hours. After the reaction, water washing was repeated 4 times until the washing water became neutral, and water was removed from the system by azeotropy of toluene and water under heating and reduced pressure below 70°C. Toluene was completely distilled off under heating and reduced pressure to obtain maleimide resin (M-16). The softening point of the obtained maleimide resin (M-16) was 100°C and the acid value was 9 mgKOH / g.

[0209] [Synthesis example 2]

[0210] In a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation trap, and a stirrer, 70.9 parts of 2,6-diisopropylaniline, 272 parts of α,α,α',α'-tetramethyl-1,3-benzenedimethanol, 280 parts of xylene, and 70 parts of activated clay were added, and the temperature was raised to 210°C while removing xylene and generated water, and the reaction was carried out for 3 hours. After the internal temperature was cooled to 140°C, 212.7 parts of 2,6-diisopropylaniline was added, and the temperature was raised to 220°C and the reaction was carried out for 3 hours. After cooling to room temperature, the extracted xylene was returned, and the activated clay was removed by filtration. The mixture was concentrated under heating and reduced pressure to obtain 330 parts of an aromatic amine resin (A2) represented by the following formula (2-a) as a light yellow solid. The amine equivalent of the aromatic amine resin (A2) is 372.5 g / eq.

[0211]

[0212] [Example 10]

[0213] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 75 parts of toluene, 25 parts of NMP, 9.4 parts of styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 60, Mw: 10140), 14.9 parts of the aromatic amine resin (A2) obtained in Synthesis Example 2, and 0.3 parts of methanesulfonic acid were added, and the mixture was reacted at 115°C for 2 hours. After cooling, 4.4 parts of maleic anhydride were added, and the reaction was continued under reflux for 2 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 25.4 parts of the target compound (M-10) as a brown solid resin (Mn: 2928, Mw: 11540). The GPC chart of the obtained compound is shown in Fig.17 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig.18 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 6.85 ppm(s).

[0214] [Synthesis example 3]

[0215] In a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation trap, and a stirrer, 48.5 parts of 2,6-dimethylaniline, 272 parts of α,α,,α',α'-tetramethyl-1,3-benzenedimethanol, 200 parts of toluene, and 70 parts of activated clay were added, and the temperature was raised to 210°C while removing toluene and generated water, and the reaction was carried out for 3 hours. After the internal temperature was cooled to 140°C, 145.4 parts of 2,6-dimethylaniline was added, and the temperature was raised to 220°C, and the reaction was carried out for 3 hours. After cooling to room temperature, the extracted toluene was returned, and the activated clay was removed by filtration. The mixture was concentrated under heating and reduced pressure to obtain 281.4 parts of an aromatic amine resin (A3) represented by the following formula (2-b) as a brown solid. The amine equivalent of the aromatic amine resin (A3) is 316.9 g / eq.

[0216]

[0217] [Example 11]

[0218] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 75 parts of toluene, 25 parts of NMP, 9.4 parts of styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 60, Mw: 10140), 9.4 parts of the aromatic amine resin (A3) obtained in Synthesis Example 3, and 0.25 parts of methanesulfonic acid were added, and the mixture was reacted at 115°C for 2 hours. After cooling, 4.4 parts of maleic anhydride were added, and the reaction was continued under reflux for 2 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 24.0 parts of the target compound (M-11) as a brown solid resin (Mn: 2127, Mw: 8411). The GPC chart of the obtained compound during the reaction is shown in Fig.19 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig. 20 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 6.85 ppm(s).

[0219] [Synthesis Example 4]

[0220] In a flask equipped with a thermometer, a cooling tube, and a stirrer, add 220 parts of 2,6-diisopropylaniline and 1200 parts of water and start stirring. While controlling the internal temperature to be below 30°C, add dropwise 144 parts of 35% hydrochloric acid. After raising the internal temperature to 96°C, add dropwise 48.7 parts of a 37% formaldehyde aqueous solution over 30 minutes. After reacting at 96°C for 2 hours, cool to room temperature. Add 63.3 parts of sodium hydroxide and 200 parts of toluene, stir for 2 hours, and neutralize. Wash the organic layer with water until the waste liquid becomes neutral, concentrate under heating and reduced pressure, and obtain 215 parts of an aromatic amine resin (A4) represented by the following formula (3-a) as a brown solid.

[0221]

[0222] [Example 12]

[0223] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 75 parts of toluene, 25 parts of NMP, 18.7 parts of a styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 60, Mw: 10140), 14.7 parts of the aromatic amine resin (A4) obtained in Synthesis Example 4, and 0.29 parts of methanesulfonic acid were added, and the mixture was reacted at 111°C for 8 hours. After cooling, 8.8 parts of maleic anhydride were added, and the reaction was continued at 111°C for 2 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under reduced pressure while heating to obtain 20.2 parts of the target compound (M-12) as a brown solid resin (Mn: 2126, Mw: 11527). The GPC chart of the obtained compound during the reaction is shown in Fig.21 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig. 22 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 6.87 ppm(s).

[0224] [Synthesis Example 5]

[0225] In a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation trap, and a stirrer, 47.3 parts of aniline and 25.3 parts of a 35% hydrochloric acid aqueous solution were added, and the temperature was raised to 60°C. A 37% formaldehyde aqueous solution was added dropwise over 30 minutes, and the mixture was reacted at 80°C for 1 hour. The mixture was heated to 128°C while water was extracted over 1 hour, and the mixture was reacted for 30 minutes. After cooling to room temperature, 30.7 parts of a 30% sodium hydroxide aqueous solution was added dropwise and neutralized. After adding 100 parts of toluene, the organic layer was washed three times with 100 parts of water. The mixture was concentrated under reduced pressure with heating to obtain 15.6 parts of an aromatic amine resin (A5) represented by the following formula (4-a) as a black liquid. The amine equivalent of the aromatic amine resin (A5) was 100.6 g / eq. The content of the compound with the structure represented by n=1 was 81.5% in terms of GPC area % (RI).

[0226]

[0227] [Example 13]

[0228] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 75 parts of toluene, 25 parts of NMP, 18.7 parts of a styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 60, Mw: 10140), 8.0 parts of the aromatic amine resin (A5) obtained in Synthesis Example 5, and 0.16 parts of methanesulfonic acid were added, and the mixture was reacted at 120°C for 2 hours. After cooling, 8.8 parts of maleic anhydride were added, and the reaction was continued at 120°C for 6 hours. After cooling, 400 parts of toluene were added, and the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under reduced pressure while heating, thereby obtaining 35.3 parts of the target compound (M-13) as a brown solid resin (Mn: 2011, Mw: 22708). The GPC chart of the obtained compound during the reaction is shown in Fig.23 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig.24 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 6.85 ppm(s).

[0229] [Example 14]

[0230] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 71.6 parts of toluene, 75 parts of NMP, 13.9 parts of a styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing Co., Ltd., acid value: 60, Mw: 10140), 11.8 parts of an amine resin represented by the following formula (5-a) synthesized according to Synthesis Example 2 of Japanese Patent Gazette No. 2009-001783, and 0.25 parts of methanesulfonic acid were added, and the mixture was reacted at 100°C for 8 hours. After cooling, 6.6 parts of maleic anhydride were added, and the reaction was continued at 100°C for 2 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under heating and reduced pressure, thereby obtaining 20.2 parts of the target compound (M-14) as a brown solid resin (Mn: 3973, Mw: 146462). The GPC chart of the obtained compound is shown in Fig.25 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig.26 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 6.85 ppm(s).

[0231]

[0232] [Example 15]

[0233] In a flask equipped with a thermometer, a cooling tube and a stirrer, 75 parts of toluene, 25 parts of NMP, 18.7 parts of styrene / maleic acid copolymer (RK-42, manufactured by Gifu Shellac Manufacturing, acid value: 60, Mw: 10140), 11.3 parts of 4,4'-methylenebis(2-ethyl-6-methylaniline) (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.2 parts of methanesulfonic acid were added, and the mixture was reacted at 120°C for 2 hours. After cooling, 8.8 parts of maleic anhydride were added, and the reaction was continued at 120°C for 6 hours. After cooling, the organic layer was washed 5 times with 100 parts of water. The solvent was distilled off under reduced pressure while heating to obtain 35.3 parts of the target compound (M-15) as a brown solid resin (Mn: 1829, Mw: 11101). The GPC chart of the obtained compound during the reaction is shown in Fig. 27 In addition, the obtained compound 1 H-NMR chart (heavy chloroform) is shown in Fig.28 . 1 In the H-NMR chart, a signal derived from a maleimide group was observed at 6.87 ppm(s).

[0234] [Examples 16 to 17, Comparative Examples 1 to 2]

[0235] The materials were mixed in the proportions shown in Table 1, kneaded in a mortar, poured into a mold, cured at 220°C for 1 hour, and various tests were performed. In addition, in Comparative Example 1, the materials were mixed in the proportions shown in Table 1, heated and melted in a metal container, and directly poured into a mold, and after transfer molding at 175°C, cured at 160°C for 2 hours, and cured at 180°C for 6 hours.

[0236] <Dielectric constant test, loss tangent test>

[0237] The test was conducted by the cavity resonator perturbation method using a 10 GHz cavity resonator manufactured by AET Co., Ltd. The test was conducted with a sample size of 1.7 mm in width x 100 mm in length and 1.7 mm in thickness.

[0238] <Heat resistance (DMA)>

[0239] Dynamic viscoelasticity tester: TA-instruments, DMA-2980.

[0240] Measuring temperature range: -30 to 280°C.

[0241] Heating rate: 2℃ / min.

[0242] Frequency: 10Hz.

[0243] Test piece size: A cut piece of 5 mm × 50 mm (thickness about 800 μm) was used.

[0244] Tg: The peak point of tanδ (=loss elastic modulus / storage elastic modulus) is taken as Tg.

[0245] [Table 1]

[0246]

[0247] NC-3000-L: Biphenyl aralkyl type epoxy resin (manufactured by Nippon Kayaku Co., Ltd.).

[0248] ·GPH-65: Biphenyl aralkyl type phenol resin (manufactured by Nippon Kayaku Co., Ltd.).

[0249] · 2E4MZ: 2-ethyl-4-methylimidazole (hardening accelerator, manufactured by Shikoku Chemicals Co., Ltd.).

[0250] Examples 16 and 17 showed excellent results in terms of high heat resistance and low dielectric properties.

[0251] [Examples 18 to 31]

[0252] The materials were mixed in the proportions shown in Table 2, kneaded in a mortar, poured into a mold, cured at 220° C. for 1 hour, and subjected to various tests.

[0253] [Table 2]

[0254]

[0255] SA-9000: polyphenylene ether compound (manufactured by SABIC).

[0256] · Ricon-100: styrene / butadiene copolymer (manufactured by Cray Valley Corporation).

[0257] Perkadox 14: thermal radical polymerization initiator (manufactured by KAYAKU NOURYON Co., Ltd.).

[0258] Examples 18 to 31 showed excellent results in terms of low dielectric properties.

[0259] Although the present invention has been described in detail with reference to specific embodiments, those skilled in the art can implement various changes and modifications without departing from the spirit and scope of the present invention.

[0260] In addition, this application is based on Japanese Patent Application (Japanese Patent Application No. 2021-078279) filed on May 6, 2021, and the entire content is cited. In addition, all cited references are incorporated into this specification.

[0261] (Industrial Applicability)

[0262] The curable resin composition of the present invention and its cured product can be used for insulating materials for electric and electronic parts (high reliability semiconductor sealing materials, etc.), laminates (printed wiring boards, BGA substrates, build-up substrates, etc.), adhesives (conductive adhesives, etc.), various composite materials including CFRP, coatings, 3D printing, and the like.

Claims

1. A maleimide resin obtained by reacting a styrene / maleic acid copolymer, a compound containing two or more amino groups in the molecule, and maleic anhydride, and having repeating units of the following formulae (a) and (b): In the above formula, X represents an arbitrary organic group, m and n are respectively the average values ​​of the repeating numbers, 1≤m≤1000, 1.1≤n≤1000, (a) and (b) are respectively bonded with * and the repeating positions may be random.

2. The maleimide resin according to claim 1, wherein in the aforementioned formula (b), X is any one or more of the following formulas (A) to (P), In the above formula, R represents a hydrocarbon group having 1 to 10 carbon atoms, a represents an integer from 0 to 4, p represents a number from 1 to 20, and * represents a bonding position. 3 . The maleimide resin according to claim 2 , wherein in the formula (b), X is any one or more of the formulas (A) to (F).

4. The maleimide resin according to claim 1, wherein the compound containing two or more amino groups in the molecule is at least one selected from the group consisting of amine compounds represented by the following formulae (1) to (5) and dimer diamines, In formula (1), n ​​is the average value of the number of repetitions, 1≤n<5; In formula (2), R is independently a hydrocarbon group having 1 to 3 carbon atoms, p is the average value of the number of repetitions, and 0≤p≤20; In formula (3), R each independently represents a hydrocarbon group having 1 to 3 carbon atoms; In formula (4), n is the average value of the number of repetitions, 1 <n<5; In formula (5), n is the average value of the number of repetitions, 1≤n<5. 5 . A curable resin composition comprising the maleimide resin according to claim 1 . The curable resin composition according to claim 5 , further comprising a radical polymerization initiator. 7 . The curable resin composition according to claim 5 , further comprising a polyphenylene ether compound. 8 . The curable resin composition according to claim 5 , further comprising a styrene / butadiene copolymer.

9. A cured product obtained by curing the maleimide resin according to claim 1.

10. A cured product obtained by curing the curable resin composition according to claim 6.