A piezoelectric ceramic material with high piezoelectric coefficient and its preparation method and application

Through component design and quasi-similar phase boundary construction of PNN-PST-PT ternary piezoelectric ceramic material, the shortcomings of existing piezoelectric ceramic materials in piezoelectric performance are solved, and high voltage electrical coefficient and high electromechanical coupling coefficient are achieved. Suitable for high-performance piezoelectric devices.

CN117303899BActive Publication Date: 2024-11-19XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311293963.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-08
Publication Date
2024-11-19
Estimated Expiration
2043-10-08

AI Technical Summary

Technical Problem

The piezoelectric ceramic materials of existing ternary and multivariate systems have poor piezoelectric properties, especially the unmodified materials lack piezoelectric properties below 700pC/N, making it difficult to meet the needs of high-precision electromechanical devices.

Method used

Through component design combined with quasi-isotype phase boundary (MPB), PNN-PST-PT ternary piezoelectric ceramic material is constructed, and B-position elements of different radii and valence states are regulated to form multiphase coexistence, reduce polarization anisotropy, and achieve polarization , and improve piezoelectric performance.

Benefits of technology

It significantly improves the piezoelectric coefficient, plane electromechanical coupling coefficient and room temperature dielectric constant of piezoelectric ceramic materials, which is suitable for high-performance piezoelectric devices. The piezoelectric coefficient is 390~1028pC/N, and the plane electromechanical coupling coefficient is 0.43~0.71. The room temperature dielectric constant is 2956~6663.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117303899B_ABST
    Figure CN117303899B_ABST
Patent Text Reader

Abstract

The present invention discloses a piezoelectric ceramic material with a high piezoelectric coefficient, a preparation method and an application thereof. The chemical composition of the piezoelectric ceramic material is xPb(Nb 2 / 3 Ni 1 / 3 )O3‑yPb(Sc 1 / 2 Ta 1 / 2 )O3‑(1‑x‑y)PbTiO3(PNN‑PST‑PT), 0.2≤x≤0.5, 0.332≤y≤0.405. The piezoelectric ceramic material is prepared by a solid-state reaction method, and the main steps include: weighing of raw materials, ball milling, calcination, granulation, molding, debinding and sintering process. The PNN‑PST‑PT piezoelectric ceramics prepared by the present invention have excellent piezoelectric properties and improve the problem of high sintering temperature containing Sc and Ta elements. Therefore, the PNN‑PST‑PT piezoelectric ceramics of the present invention are a very promising new high-performance piezoelectric material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of piezoelectric ceramic preparation, and in particular relates to a piezoelectric ceramic material with a high piezoelectric coefficient, a preparation method and an application thereof. Background Art

[0002] As a widely used functional material, piezoelectric ceramics can realize the conversion of electrical energy into mechanical energy. Among them, perovskite relaxor ferroelectrics have the best piezoelectric properties and show great application potential in high-precision electromechanical devices. For example, the Sm-doped PMN-PT relaxor system has achieved a record high piezoelectric coefficient (d 33 ). However, the piezoelectric performance of most unmodified ternary and multi-element systems is still poor (e.g., below 700 pC / N).

[0003] Excellent piezoelectricity is usually determined by the intrinsic crystal structure of the piezoelectric body. At present, the widely accepted method to obtain high-performance piezoelectric ceramics is to construct a quasi-modular phase boundary (MPB). However, this method shows certain limitations in order to further improve the piezoelectricity and achieve a smoother energy distribution. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to construct a new type of piezoelectric ceramic material with a high piezoelectric coefficient through component design combined with MPB, and at the same time disclose its preparation method and application. The present invention provides a new way to improve the piezoelectric properties of piezoelectric ceramic materials.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention discloses a piezoelectric ceramic material with a high piezoelectric coefficient. The piezoelectric ceramic material is a PNN-PST-PT ternary piezoelectric ceramic, and its chemical composition is xPb(Nb 2 / 3 Ni 1 / 3 )O3-yPb(Sc 1 / 2 Ta 1 / 2 )O3-(1-xy)PbTiO3, where 0.2≤x≤0.5, 0.332≤y≤0.405.

[0007] Preferably, the piezoelectric coefficient of the piezoelectric ceramic material is 390-1028 pC / N, the plane electromechanical coupling coefficient is 0.43-0.71, the Curie temperature is 96-168°C, the room temperature dielectric constant is 2956-6663, and the residual polarization strength is 16-31 μC / cm 2 , the coercive field is 0.29~0.52kV / mm.

[0008] The present invention also discloses a method for preparing a piezoelectric ceramic material with a high piezoelectric coefficient, comprising the following steps:

[0009] 1) According to xPb(Nb 2 / 3 Ni 1 / 3 )O3-yPb(Sc 1 / 2 Ta 1 / 2 )O3-(1-xy)PbTiO3, 0.2≤x≤0.5, 0.332≤y≤0.405 are used for the stoichiometric proportion of the materials, ScTaO4, NiNb2O6, PbO and TiO2 are weighed, and the mixture is fully ball-milled to obtain a mixture, which is then dried and ground for later use;

[0010] 2) pre-calcining the mixture treated in step 1) to obtain a pure perovskite phase PNN-PST-PT pre-calcined powder, and then fully ball-milling and drying the pre-calcined powder for a second time;

[0011] 3) The pre-burned powder after the secondary ball milling is granulated, then sieved and pressed into green sheets, and the green sheets are debinded and sintered to obtain PNN-PST-PT ternary piezoelectric ceramics.

[0012] Preferably, in step 1), the preparation method of the precursor ScTaO4 is as follows: weigh the raw materials Sc2O3 and Ta2O5 according to ScTaO4, ball mill them evenly, dry and grind them, and then calcine them at 1300-1400° C. for 2-4 hours to obtain a ScTaO4 precursor;

[0013] The preparation method of the precursor NiNb2O6 used is as follows: according to the chemical formula of NiNb2O6, the raw materials Ni(Ac)2·4H2O and Nb2O5 are weighed, ball-milled evenly, dried, and ground, and then calcined at 1000-1100°C for 4-6 hours to obtain a NiNb2O6 precursor.

[0014] Preferably, in step 1), the ball milling speed is 250-280 rpm, the ball milling time is 24 h, and the drying temperature is 70-90°C.

[0015] Preferably, in step 2), the pre-calcination temperature is 800-850°C, the pre-calcination treatment time is 2-4h, the secondary ball milling speed is 250-280 rpm, the secondary ball milling time is 12h, and the drying temperature is 70-90°C.

[0016] Preferably, in step 3), the pre-calcined powder is granulated with a polyvinyl alcohol aqueous solution having a mass concentration of 5%, the amount of the polyvinyl alcohol aqueous solution added is 5% to 10% of the mass of the pre-calcined powder, and the sieve used has an aperture of 80 to 100 meshes.

[0017] Preferably, in step 3), the debinding treatment temperature is 550° C., the debinding treatment time is 2 hours, and the heating rate during the debinding process is 1° C. / min.

[0018] Preferably, in step 3), the sintering temperature is 1000-1200° C., the heating rate during the sintering process is 3° C. / min, and the holding time is 2 hours.

[0019] The invention also discloses the application of the piezoelectric ceramic material with a high piezoelectric coefficient in the preparation of high-precision electromechanical devices.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The piezoelectric ceramic material with a high piezoelectric coefficient disclosed in the present invention forms a new ternary piezoelectric ceramic material system, namely, a PNN-PST-PT ternary piezoelectric ceramic, through component design and MPB construction. The PNN-PST-PT piezoelectric ceramic prepared by the present invention has excellent piezoelectric properties and improves the problem of high sintering temperature of Sc and Ta elements. By regulating the B-site elements with different radii and valence states in the relaxation system, multi-phase coexistence is formed on the nanoscale, and then the polarization anisotropy is reduced on the local scale to achieve a "quasi-isotropic" distribution of polarization, reduce the energy barrier, smooth the energy distribution curve, and finally significantly improve the piezoelectric performance. The PNN-PST-PT piezoelectric ceramic prepared by the present invention has the following characteristics: the piezoelectric coefficient (d 33 ) is 390~1028pC / N, the plane electromechanical coupling coefficient is 0.43~0.71, the room temperature dielectric constant is 2956~6663, and the residual polarization strength is 16~31μC / cm 2 Therefore, the PNN-PST-PT piezoelectric ceramic is very suitable for the application of high-performance piezoelectric devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a ternary phase diagram of the piezoelectric ceramic material of the present invention;

[0023] Figure 2 is an X-ray diffraction pattern of the piezoelectric ceramic material of the present invention;

[0024] Figure 3 is the room temperature piezoelectric coefficient (d 33 ) and the planar electromechanical coupling coefficient (k p )picture;

[0025] Figure 4 is a hysteresis loop diagram of the piezoelectric ceramic material of the present invention;

[0026] Figure 5 It is the dielectric temperature spectrum of the piezoelectric ceramic material of the present invention. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0028] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0029] The present invention discloses a new type of piezoelectric ceramic material with a high piezoelectric coefficient, the chemical composition of which is: xPb(Nb 2 / 3 Ni 1 / 3 )O3-yPb(Sc 1 / 2 Ta 1 / 2 )O3-(1-xy)PbTiO3, 0.2≤x≤0.5, 0.332≤y≤0.405.

[0030] The method for preparing the above-mentioned PNN-PST-PT piezoelectric ceramic material with high piezoelectric coefficient disclosed in the present invention comprises the following steps:

[0031] 1) According to the chemical formula of NiNb2O6 and ScTaO4, the raw materials of Nb2O5 and Ni(Ac)2·4H2O as well as Sc2O3 and Ta2O5 are accurately weighed and mixed by ball milling, and then dried and ground, and then put into a corundum crucible for compaction and calcination to obtain NiNb2O6 and ScTaO4 precursors.

[0032] 2) According to xPb(Nb 2 / 3 Ni 1 / 3 )O3-yPb(Sc 1 / 2 Ta 1 / 2)O3-(1-xy)PbTiO3, 0.2≤x≤0.5, 0.332≤y≤0.405. Weigh NiNb2O6, ScTaO4, TiO2, and PbO into a nylon ball mill and add anhydrous ethanol as the ball milling medium for a ball milling.

[0033] 3) The ball-milled mixture in 2) is dried in an oven and then ground, and then placed in a crucible for pre-calcination to obtain a PNN-PST-PT pre-calcined powder with a pure perovskite phase structure.

[0034] 4) The pre-calcined powder obtained in step 3 is ball-milled for a second time and then dried in an oven.

[0035] 5) Weigh a certain amount of the pre-sintered powder after secondary ball milling, add polyvinyl alcohol (PVA) aqueous solution to granulate, sieve, and press into green sheets with a certain shape and size.

[0036] 6) The green sheet is subjected to a debinding treatment, and then the green sheet after debinding is sintered and densified to obtain a PNN-PST-PT ceramic sheet.

[0037] After sintering, the PNN-PST-PT ceramic sheet undergoes subsequent sample preparation and electrical performance testing, including:

[0038] The ceramic sheet is ground to a certain thickness with sandpaper, and the upper and lower surfaces are sprayed with gold to make electrodes.

[0039] After the gold spraying, the excess gold layer on the edge of the ceramic piece was polished off with sandpaper, and then the ceramic piece was polarized and then the electrical performance was tested. The polarization was carried out at room temperature for 10 minutes, and the polarization electric field was 2kV / mm.

[0040] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0041] See also Figure 1 Through the analysis of the PNN-PST-PT ternary phase diagram, five different components were selected for the experiment, namely, Example 1—0.2PNN-0.395PST-0.405PT (A0), Example 2—0.3PNN-0.315PST-0.385PT (B0), Example 3—0.4PNN-0.235PST-0.365PT (C0), Example 4—0.45PNN-0.195PST-0.355PT (D0), and Example 5—0.5PNN-0.345PST-0.155PT (E0).

[0042] Example 1

[0043] 10.3252 g of Nb2O5 (99.99%), 9.6748 g of Ni(Ac)2·4H2O (99.9%), 4.7604 g of Sc2O3 (99.9%) and 15.2396 g of Ta2O5 (99.99%) were weighed respectively and put into a ball mill, and ball-milled at 280 rpm on a planetary ball mill (QM-3SP2, Instrument Factory, Nanjing University) for 24 hours, then dried in an oven at 80°C, and then calcined in a muffle furnace at 1000-1100°C and 1300-1400°C for 4-6 hours and 2-4 hours, respectively, to obtain NiNb2O6 and ScTaO4 precursors.

[0044] According to the stoichiometric ratio of 0.2PNN-0.395PST-0.405PT, 1.3534g of NiNb2O6, 3.4106g of ScTaO4, 1.9285g of TiO2 (99.99%) and 13.5737g of PbO (99.9%) were weighed into a nylon ball mill and 25mL of anhydrous ethanol was added. The mixture was milled at 280 rpm on a planetary ball mill for 24 hours, and then the milled slurry was dried in an oven at 80°C.

[0045] The dried mixed powder is ground and then compacted in a corundum crucible. The crucible is placed in a muffle furnace and heated to 850°C at a rate of 3°C / min. After two hours of heat preservation, 0.2PNN-0.395PST-0.405PT pre-burned powder is obtained. The pre-burned powder is then crushed and ground and placed in a ball mill for 12 hours, and finally dried in an oven.

[0046] Weigh 6 g of 0.2PNN-0.395PST-0.405PT ceramic powder into a mortar, add about 0.6 g of PVA solution several times for granulation, and grind and sieve (80 mesh) repeatedly to ensure that powder particles of uniform size and sufficient granulation are obtained.

[0047] 0.75 g of granulated powder was weighed and poured into a mold with a diameter of 10 mm for tableting. The green tablets obtained by pressing were placed in a muffle furnace and slowly heated to 550° C. at a heating rate of 1° C. / min and kept for 2 hours for debinding.

[0048] The green sheet after debinding was placed in a 30 mL small crucible and buried with the second ball-milled powder of the same component. It was placed in a high-temperature furnace and heated to 1000-1200°C at a heating rate of 3°C / min and kept warm for 2 hours to obtain a dense 0.2PNN-0.395PST-0.405PT ceramic sheet.

[0049] The dense sintered 0.2PNN-0.395PST-0.405PT ceramic sheet was then sanded to a thickness of 0.7 mm, and the electrode was plated by gold spraying. The excess gold layer on the edge was then polished off, and finally the electrical performance test was carried out after polarization at room temperature for 10 minutes.

[0050] The 0.2PNN-0.395PST-0.405PT piezoelectric ceramics prepared in this embodiment have the following characteristics: piezoelectric coefficient is 390pC / N, planar electromechanical coupling coefficient is 0.43, Curie temperature is 168°C, relative dielectric constant at room temperature is 2956, and remanent polarization is 21μC / cm 2 , the coercive field is 0.52kV / mm.

[0051] Example 2

[0052] According to the stoichiometric ratio of 0.3PNN-0.315PST-0.385PT, 2.0413g of NiNb2O6, 2.7348g of ScTaO4, 1.8433g of TiO2 (99.99%) and 13.6482g of PbO (99.9%) were weighed into a nylon ball mill jar and 25mL of anhydrous ethanol was added. The mixture was ball-milled at 280 rpm on a planetary ball mill for 24 hours, and the ball-milled slurry was then dried in an oven at 80°C.

[0053] The dried mixed powder is ground and then compacted in a corundum crucible. The crucible is placed in a muffle furnace and heated to 850°C at a rate of 3°C / min. After two hours of insulation, 0.3PNN-0.315PST-0.385PT pre-burned powder is obtained. The pre-burned powder is then crushed and ground and placed in a ball mill for 12 hours, and finally dried in an oven.

[0054] Weigh 6 g of 0.3PNN-0.315PST-0.385PT ceramic powder into a mortar, add about 0.6 g of PVA solution several times for granulation, and grind and sieve (80 mesh) repeatedly to ensure that powder particles of uniform size and sufficient granulation are obtained.

[0055] 0.75 g of granulated powder was weighed and poured into a mold with a diameter of 10 mm for tableting. The green tablets obtained by pressing were placed in a muffle furnace and slowly heated to 550° C. at a heating rate of 1° C. / min and kept for 2 hours for debinding.

[0056] The green sheet after debinding was placed in a 30 mL small crucible and buried with the second ball-milled powder of the same component. It was placed in a high-temperature furnace and heated to 1000-1200°C at a heating rate of 3°C / min and kept warm for 2 hours to obtain a dense 0.3PNN-0.315PST-0.385PT ceramic sheet.

[0057] The dense sintered 0.3PNN-0.315PST-0.385PT ceramic sheet was then sanded to a thickness of 0.7 mm, and the electrode was plated by gold spraying. The excess gold layer on the edge was then polished off, and finally the electrical performance test was carried out after polarization at room temperature for 10 minutes.

[0058] The 0.2PNN-0.395PST-0.405PT piezoelectric ceramic prepared in this embodiment has the following characteristics: piezoelectric coefficient is 893pC / N, planar electromechanical coupling coefficient is 0.71, Curie temperature is 141°C, relative dielectric constant at room temperature is 3768, and remanent polarization is 26μC / cm 2 , the coercive field is 0.4kV / mm.

[0059] Example 3

[0060] According to the stoichiometric ratio of 0.4PNN-0.235PST-0.365PT, 2.7367g of NiNb2O6, 2.0515g of ScTaO4, 1.7572g of TiO2 (99.99%) and 13.7236g of PbO (99.9%) were weighed into a nylon ball mill and 25mL of anhydrous ethanol was added. The mixture was ball-milled at 280 rpm on a planetary ball mill for 24 hours, and the ball-milled slurry was then dried in an oven at 80°C.

[0061] The dried mixed powder is ground and then compacted in a corundum crucible. The crucible is placed in a muffle furnace and heated to 850°C at a rate of 3°C / min. After two hours of insulation, 0.4PNN-0.235PST-0.365PT pre-burned powder is obtained. The pre-burned powder is then crushed and ground and placed in a ball mill for 12 hours, and finally dried in an oven.

[0062] Weigh 6 g of 0.4PNN-0.235PST-0.365PT ceramic powder into a mortar, add about 0.6 g of PVA solution several times for granulation, and grind and sieve (80 mesh) repeatedly to ensure that powder particles of uniform size and sufficient granulation are obtained.

[0063] 0.75 g of granulated powder was weighed and poured into a mold with a diameter of 10 mm for tableting. The green tablets obtained by pressing were placed in a muffle furnace and slowly heated to 550° C. at a heating rate of 1° C. / min and kept for 2 hours for debinding.

[0064] The green sheet after debinding was placed in a 30 mL small crucible and buried with the second ball-milled powder of the same component. It was placed in a high-temperature furnace and heated to 1000-1200°C at a heating rate of 3°C / min and kept warm for 2 hours to obtain a dense 0.4PNN-0.235PST-0.365PT ceramic sheet.

[0065] The dense sintered 0.3PNN-0.315PST-0.385PT ceramic sheet was then sanded to a thickness of 0.7 mm, and the electrode was plated by gold spraying. The excess gold layer on the edge was then polished off, and finally the electrical performance test was carried out after polarization at room temperature for 10 minutes.

[0066] The 0.4PNN-0.235PST-0.365PT piezoelectric ceramic prepared in this embodiment has the following characteristics: piezoelectric coefficient is 1028pC / N, planar electromechanical coupling coefficient is 0.69, Curie temperature is 116°C, relative dielectric constant at room temperature is 5085, and residual polarization is 31μC / cm 2 , the coercive field is 0.33kV / mm.

[0067] Example 4

[0068] According to the stoichiometric ratio of 0.45PNN-0.195PST-0.355PT, 3.0874g of NiNb2O6, 1.7086g of ScTaO4, 1.7122g of TiO2 (99.99%) and 13.7616g of PbO (99.9%) were weighed into a nylon ball mill jar and 25mL of anhydrous ethanol was added. The mixture was ball-milled at 280 rpm on a planetary ball mill for 24 hours, and the ball-milled slurry was then dried in an oven at 80°C.

[0069] The dried mixed powder is ground and then compacted in a corundum crucible. The crucible is placed in a muffle furnace and heated to 850°C at a rate of 3°C / min. After two hours of insulation, 0.45PNN-0.195PST-0.355PT pre-burned powder is obtained. The pre-burned powder is then crushed and ground and placed in a ball mill for 12 hours, and finally dried in an oven.

[0070] Weigh 6 g of 0.45PNN-0.195PST-0.355PT ceramic powder into a mortar, add about 0.6 g of PVA solution several times for granulation, and grind and sieve (80 mesh) repeatedly to ensure that powder particles of uniform size and sufficient granulation are obtained.

[0071] 0.75 g of granulated powder was weighed and poured into a mold with a diameter of 10 mm for tableting. The green tablets obtained by pressing were placed in a muffle furnace and slowly heated to 550° C. at a heating rate of 1° C. / min and kept for 2 hours for debinding.

[0072] The green sheet after debinding was placed in a 30 mL small crucible and buried with the second ball-milled powder of the same component. It was placed in a high-temperature furnace and heated to 1000-1200°C at a heating rate of 3°C / min and kept warm for 2 hours to obtain a dense 0.45PNN-0.195PST-0.355PT ceramic sheet.

[0073] The dense sintered 0.45PNN-0.195PST-0.355PT ceramic sheet is then sanded to a thickness of 0.7 mm, and the electrode is plated by gold spraying. The excess gold layer on the edge is then polished off, and finally the electrical performance test can be carried out after polarization at room temperature for 10 minutes.

[0074] The 0.45PNN-0.195PST-0.355PT piezoelectric ceramics prepared in this embodiment have the following characteristics: piezoelectric coefficient is 735pC / N, planar electromechanical coupling coefficient is 0.58, Curie temperature is 104°C, relative dielectric constant at room temperature is 5961, and remanent polarization is 22μC / cm 2 , the coercive field is 0.29kV / mm.

[0075] Example 5

[0076] According to the stoichiometric ratio of 0.5PNN-0.345PST-0.155PT, 3.4400g of NiNb2O6, 1.3619g of ScTaO4, 1.6687g of TiO2 (99.99%) and 13.8000g of PbO (99.9%) were weighed into a nylon ball mill jar and 25mL of anhydrous ethanol was added. The mixture was ball-milled at 280 rpm on a planetary ball mill for 24 hours, and the ball-milled slurry was then dried in an oven at 80°C.

[0077] The dried mixed powder is ground and then compacted in a corundum crucible. The crucible is placed in a muffle furnace and heated to 850°C at a rate of 3°C / min. After two hours of insulation, 0.5PNN-0.345PST-0.155PT pre-burned powder is obtained. The pre-burned powder is then crushed and ground and placed in a ball mill for 12 hours, and finally dried in an oven.

[0078] Weigh 6 g of 0.5PNN-0.345PST-0.155PT ceramic powder into a mortar, add about 0.6 g of PVA solution several times for granulation, and grind and sieve (80 mesh) repeatedly to ensure that powder particles of uniform size and sufficient granulation are obtained.

[0079] 0.75 g of granulated powder was weighed and poured into a mold with a diameter of 10 mm for tableting. The green tablets obtained by pressing were placed in a muffle furnace and slowly heated to 550° C. at a heating rate of 1° C. / min and kept for 2 hours for debinding.

[0080] The green sheet after debinding was placed in a 30 mL small crucible and buried with the second ball-milled powder of the same component. It was placed in a high-temperature furnace and heated to 1000-1200°C at a heating rate of 3°C / min and kept warm for 2 hours to obtain a dense 0.5PNN-0.345PST-0.155PT ceramic sheet.

[0081] The dense sintered 0.5PNN-0.345PST-0.155PT ceramic sheet was then sanded to a thickness of 0.7 mm, and the electrode was plated with gold by spraying. The excess gold layer on the edge was then polished off, and finally the electrical performance test was carried out after polarization at room temperature for 10 minutes.

[0082] The 0.5PNN-0.345PST-0.155PT piezoelectric ceramic prepared in this embodiment has the following characteristics: piezoelectric coefficient is 673pC / N, planar electromechanical coupling coefficient is 0.48, Curie temperature is 96°C, relative dielectric constant at room temperature is 6663, and remanent polarization is 16μC / cm 2 , the coercive field is 0.32kV / mm.

[0083] The phase structures of the piezoelectric ceramics prepared in the above-mentioned embodiments 1-5 were characterized by X-ray diffraction. Figure 2 , it can be seen from the figure that the piezoelectric ceramic prepared in the embodiment of the present invention is a pure perovskite structure.

[0084] according to Figure 3 According to the resonance and anti-resonance spectrum test diagram in the figure, it is calculated that the planar electromechanical coupling coefficient of the piezoelectric ceramic prepared in Example 3 of the present invention is 0.69.

[0085] from Figure 4 It can be seen from the dielectric temperature spectrum that the Curie temperature of the piezoelectric ceramic prepared in Example 3 of the present invention is 116° C. and the room temperature dielectric constant is 5085.

[0086] from Figure 5 It can be seen from the hysteresis loop that the remanent polarization of the piezoelectric ceramic prepared in Example 3 of the present invention is 30.61 μC / cm 2 , the coercive field is 0.33kV / mm.

[0087] In summary, the present invention provides a new type of lead nickel niobate-lead tantalate-lead titanate piezoelectric ceramic, abbreviated as PNN-PST-PT, and the prepared PNN-PST-PT piezoelectric ceramic can effectively solve the key technical problems in the preparation of high-performance piezoelectric devices, that is, it can simultaneously meet the requirements of high piezoelectric coefficient and high electromechanical coupling coefficient.

[0088] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A piezoelectric ceramic material having a high piezoelectric coefficient, characterized in that: The piezoelectric ceramic material is PNN-PST-PT ternary piezoelectric ceramic, and its chemical composition is x Pb(Nb 2 / 3 Ni 1 / 3 )O3- y Pb(Sc 1 / 2 Ta 1 / 2 )O3-(1 -xy )PbTiO3, wherein 0.2≤x≤0.5, 0.332≤y≤0.405; The piezoelectric coefficient of the piezoelectric ceramic material is 390-1028 pC / N, the plane electromechanical coupling coefficient is 0.43-0.71, the Curie temperature is 96-168 °C, the relative dielectric constant at room temperature is 2956-6663, and the residual polarization strength is 16-31 μC / cm 2 , the coercive field is 0.29~0.52 kV / mm.

2. The method for preparing a piezoelectric ceramic material having a high piezoelectric coefficient according to claim 1, characterized in that: The following steps are involved: 1) Follow x Pb(Nb 2 / 3 Ni 1 / 3 )O3- y Pb(Sc 1 / 2 Ta 1 / 2 )O3-(1 -xy )PbTiO3, 0.2≤x≤0.5, 0.332≤y≤0.405 are used for the stoichiometric proportion of the ingredients, ScTaO4, NiNb2O6, PbO and TiO2 are weighed, and the mixture is fully ball-milled to obtain a mixture, which is then dried and ground for later use; 2) Pre-calcining the mixture treated in step 1) to obtain a pure perovskite phase PNN-PST-PT pre-calcined powder, and then fully ball-milling and drying the pre-calcined powder for a second time; the pre-calcining temperature is 800-850°C, and the pre-calcining time is 2-4 h; 3) The pre-burned powder after the secondary ball milling is granulated, then sieved and pressed into green sheets, and the green sheets are debinded and sintered to obtain PNN-PST-PT ternary piezoelectric ceramics; The debinding treatment temperature is 550 ℃, the debinding treatment time is 2 hours, and the heating rate during the debinding process is 1 ℃ / min; the sintering treatment temperature is 1000~1200 ℃, the heating rate during the sintering process is 3 ℃ / min, and the holding time is 2 hours.

3. The method for preparing a piezoelectric ceramic material having a high piezoelectric coefficient according to claim 2, characterized in that: In step 1), the preparation method of the precursor ScTaO4 is as follows: weigh the raw materials Sc2O3 and Ta2O5 according to ScTaO4, ball mill them evenly, dry and grind them, and then calcine them at 1300-1400°C for 2-4 hours to obtain a ScTaO4 precursor; The preparation method of the precursor NiNb2O6 used is as follows: according to the chemical formula of NiNb2O6, raw materials Ni(Ac)2·4H2O and Nb2O5 are weighed, ball-milled evenly, dried, and ground, and then calcined at 1000-1100°C for 4-6 hours to obtain a NiNb2O6 precursor.

4. The method for preparing a piezoelectric ceramic material having a high piezoelectric coefficient according to claim 2, characterized in that: In step 1), the ball milling speed is 250-280 rpm, the ball milling time is 24 h, and the drying temperature is 70-90 °C.

5. The method for preparing a piezoelectric ceramic material having a high piezoelectric coefficient according to claim 2, characterized in that: In step 2), the secondary ball milling speed is 250-280 rpm, the secondary ball milling time is 12 h, and the drying temperature is 70-90 °C.

6. The method for preparing a piezoelectric ceramic material with a high piezoelectric coefficient according to claim 2, characterized in that: In step 3), the pre-calcined powder is granulated with a polyvinyl alcohol aqueous solution having a mass concentration of 5%. The amount of the polyvinyl alcohol aqueous solution added is 5% to 10% of the mass of the pre-calcined powder, and the aperture of the sieve used is 80 to 100 meshes.

7. Use of the piezoelectric ceramic material with a high piezoelectric coefficient as claimed in claim 1 in the preparation of high-precision electromechanical devices.