A highly conductive and corrosion-resistant coating for bipolar plates of PEM electrolyzers and its preparation method

By preparing titanium nitride nanocrystalline thin films on the surface of bipolar plates in a PEM electrolytic cell and sputtering metal nitride nanocrystalline coatings, the problem of easy coating peeling was solved, the adhesion and conductivity of the coating were improved, the contact resistance was reduced, and high-efficiency corrosion resistance and conductivity were achieved.

CN117305878BActive Publication Date: 2026-11-17XI AN JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311345827.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-17
Publication Date
2026-11-17
Estimated Expiration
2043-10-17

AI Technical Summary

Technical Problem

The coating on the bipolar plates of existing PEM electrolyzers is prone to peeling off, and the adhesion between the coating and the plate surface is weak, affecting corrosion resistance and conductivity.

Method used

Titanium nitride nanocrystalline films were prepared on the surface of a titanium-based bipolar plate by nitriding, and a metal nitride nanocrystalline coating was sputtered onto it. By combining ion nitriding and magnetron sputtering techniques, a dense nanocrystalline coating structure was formed.

Benefits of technology

It improves the adhesion between the coating and the substrate, enhances corrosion resistance and conductivity, reduces contact resistance, and lowers costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117305878B_ABST
    Figure CN117305878B_ABST
Patent Text Reader

Abstract

This invention discloses a highly conductive and corrosion-resistant coating for PEM electrolytic cell bipolar plates and its preparation method. This method addresses the surface characteristics of the flow channels in PEM electrolytic cell bipolar plates and the features of magnetron sputtering technology. First, surface pretreatment is performed using ion nitriding to form a uniformly distributed first protective layer, reconstructing the surface morphology and structure of the titanium-based bipolar plate. Then, a fine-grained and dense second protective layer is prepared using magnetron sputtering technology, solving the problem of poor coating quality in PEM electrolytic cell bipolar plate preparations using magnetron sputtering. The nanocrystalline coating prepared by this method has a dense structure, preventing corrosive media from penetrating the coating and corroding the substrate. The low lattice mismatch of the nanocrystalline coating improves the adhesion between the coating and the substrate. Furthermore, the composite-prepared nanocrystalline coating has good conductivity, further reducing the contact resistance of the bipolar plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of PEM electrolysis for hydrogen production, specifically relating to a highly conductive and corrosion-resistant coating for bipolar plates of a PEM electrolyzer and its preparation method. Background Technology

[0002] Hydrogen energy is a crucial component of the future energy system, with hydrogen production from renewable energy sources being a primary development direction. Proton exchange membrane electrolyzers (PEMECs) effectively address the volatility and intermittency issues of renewable energy sources like wind and solar power, making them the most promising green hydrogen production devices. The working environment of PEM electrolyzer bipolar plates is characterized by strong acidity (pH 2–4), high potential (1.5–2V), and strong oxidation (O2 production at the anode). Therefore, the bipolar plate materials must possess excellent corrosion resistance, high conductivity, and long lifespan. Currently, research and commercial applications mainly focus on titanium-based bipolar plates. However, titanium materials easily form a passivation film on the oxygen side, increasing contact resistance and consequently raising overpotential and reducing water electrolysis efficiency. Coating the bipolar plate surface with precious metals such as Pt and It can significantly improve the corrosion resistance and conductivity of titanium-based bipolar plates, but their high cost and scarcity make it difficult to meet the future demand for large-scale hydrogen energy production and application. Therefore, developing bipolar plate coating modification technology that combines high conductivity, strong corrosion resistance, and significantly reduced cost is one of the key issues that must be addressed for the large-scale application of PEM electrolyzers.

[0003] Titanium nitride (TiN) possesses both corrosion resistance and high electrical conductivity, making it a promising candidate material for bipolar plate coatings in PEM electrolytic cells. The most common method for preparing TiN coatings on titanium-based bipolar plates is magnetron sputtering. This method works by colliding electrons with argon atoms under an electric field, ionizing them to produce positively charged Ar ions and negatively charged electrons. The Ar ions are accelerated towards the cathode target under the electric field, bombarding the target surface with high energy, resulting in sputtering. The sputtered target components are then deposited onto the substrate surface under the influence of the electric field, gradually growing to form a thin film / coating. However, magnetron sputtering coatings exhibit poor coating wrapping properties, and the coating quality, film-substrate adhesion strength, and electrochemical characteristics are directly related to the substrate surface morphology. Therefore, fine optimization of surface pretreatment processes such as cleaning, grinding, and polishing is necessary to improve the quality of magnetron sputtering coatings.

[0004] Typically, the surface of a bipolar plate in a PEM electrolytic cell features a ridge-groove channel structure with a depth of approximately 0.3–1.5 mm and a width of approximately 0.5–2 mm. During magnetron sputtering coating preparation, the sidewalls of the channel structure are perpendicular to the target material, often resulting in uneven coating growth or even no coating deposition, which significantly impacts the corrosion resistance of the bipolar plate. Furthermore, numerous surface defects on the substrate after bipolar plate channel processing also negatively affect coating density and film-substrate adhesion. To address these issues, researchers have prepared coatings of noble metals such as Pt and Ir on the surface of bipolar plates using electroplating. While electroplated coatings exhibit good uniformity, they suffer from defects such as pinholes and impurities, leading to easy detachment and reduced durability during long-term service. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a highly conductive and corrosion-resistant coating for PEM electrolytic cell bipolar plates and its preparation method, so as to solve the problems of easy peeling of PEM electrolytic cell bipolar plate coatings and weak coating adhesion and electrode surface adhesion in the prior art.

[0006] To achieve the above objectives, the present invention employs the following technical solution:

[0007] A method for preparing a highly conductive and corrosion-resistant coating for a PEM electrolytic cell bipolar plate involves preparing a titanium nitride nanocrystalline film on the surface of a titanium-based bipolar plate by nitriding; sputtering a metal nitride nanocrystalline coating, wherein the metal nitride nanocrystalline is a transition metal nitride nanocrystalline; and preparing a highly conductive and corrosion-resistant coating on the surface of the titanium-based bipolar plate.

[0008] The titanium nitride nanocrystalline film has a grain size of 5–20 nm; the metal nitride nanocrystalline coating has a grain size of 5–40 nm.

[0009] A further improvement of the present invention is that:

[0010] Preferably, during the nitriding process, the side with the flow channels faces the anode plate, and the distance between the side with the flow channels and the anode plate is ≤100mm.

[0011] Preferably, the nitriding time is 2-6 hours, the nitriding pressure is 1-30 Pa, and the nitriding substrate temperature is 400-800℃.

[0012] Preferably, when the nitriding pressure is <15Pa, the nitriding temperature is ≤550℃ and the nitriding time is ≥3h; when the pressure is ≥15Pa, the nitriding temperature is 550-800℃ and the nitriding time is ≥2h.

[0013] Preferably, the sputtered metal nitride nanocrystalline coating is titanium nitride, tantalum nitride, or niobium nitride.

[0014] Preferably, during the sputtering process, the sputtering temperature is 200-550℃ and the bias voltage is 100-300V.

[0015] Preferably, an annealing operation is performed after sputtering a metal nitride nanocrystalline coating.

[0016] Preferably, the annealing temperature is 400-600℃ and the annealing time is 1-4h.

[0017] Preferably, when the annealing temperature is ≤500℃, the annealing time is ≥3h; when the annealing temperature is >500℃, the annealing time is <3h.

[0018] A highly conductive and corrosion-resistant coating for a PEM electrolytic cell bipolar plate prepared by any of the above methods comprises a titanium nitride nanocrystalline film and a metal nitride nanocrystalline coating on the surface of a titanium-based bipolar plate, wherein the metal nitride nanocrystalline coating is located outside the titanium nitride nanocrystalline film; the thickness of the titanium nitride nanocrystalline film is 50–200 nm; the grain size of the metal nitride nanocrystalline coating is 5–40 nm, and the thickness is ≥100 nm.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] This invention discloses a method for preparing a highly conductive and corrosion-resistant coating for a PEM electrolytic cell bipolar plate. This method, taking into account the surface characteristics of the flow channel of the PEM electrolytic cell bipolar plate and the advantages of magnetron sputtering technology, firstly, uses ion nitriding for surface pretreatment to form a uniformly distributed first protective layer, reconstructing the surface morphology and structure of the titanium-based bipolar plate. Then, magnetron sputtering technology is used to prepare a fine-grained and dense second protective layer, solving the problem of poor coating quality in PEM electrolytic cell bipolar plates prepared by magnetron sputtering. This invention combines the high uniformity and density of ion-nitrided films with the controllable thickness of the coating prepared by magnetron sputtering technology, and the ability of annealing to further optimize the crystallinity and density of the coating. The nanocrystalline coating prepared by this method has a dense structure, preventing corrosive media from penetrating the coating and corroding the substrate. The low lattice mismatch of the nanocrystalline coating improves the adhesion between the coating and the substrate. In addition, the composite nanocrystalline coating has good conductivity, further reducing the contact resistance of the bipolar plate.

[0021] Plasma nitriding is a chemical vapor phase method with good coating properties. It has excellent coating properties for complex surfaces such as polyhedral structures, gaps, and deep holes. It can generate titanium nitride nanocrystals in situ, achieving the first level of corrosion protection for the substrate surface and defects. Moreover, the titanium nitride nanocrystals formed by plasma nitriding provide effective nucleation sites for the subsequent preparation of magnetron sputtering metal nitride nanocrystal coatings. This is beneficial for forming a fine and dense metal nitride second protective layer during magnetron sputtering, thus solving the problem of poor coating quality of bipolar plates in PEM electrolytic cells.

[0022] Furthermore, the coating preparation and heat treatment are completed sequentially within the cavity of the magnetron sputtering equipment, avoiding the problem of coating oxidation caused by repeated loading and unloading, and simplifying the process. Temperature control can prevent grain growth and improve coating adhesion. In addition, plasma nitriding can sputter away oxides on the substrate surface, improving production efficiency. The metal nitride coating prepared by this invention avoids the use of precious metals such as Pt and Ir, significantly reducing the cost of PEM electrolytic cells. Attached Figure Description

[0023] Figure 1 This is a surface morphology diagram of the coating of the present invention;

[0024] Figure (a) shows the coating prepared by direct magnetron sputtering; Figure (b) shows the coating prepared by the composite preparation method.

[0025] Figure 2 The diagram shows the contact resistance of the coatings prepared by different methods according to the present invention.

[0026] Figure 3 The diagram shows the corrosion performance of coatings prepared by different methods according to the present invention. Detailed Implementation

[0027] One embodiment of the present invention discloses a composite preparation method for a highly conductive and corrosion-resistant metal nitride coating on a bipolar plate of a PEM electrolytic cell, comprising the following steps:

[0028] Step 1: Place the titanium-based bipolar plate in the plasma nitriding equipment, on the parallel plate capacitor plasma cathode plate, with the side with the flow channels facing the parallel plate anode plate, at a distance of no more than 100mm from the anode plate. The parallel placement of the anode plates makes nitriding more uniform, and the flow channels can be nitrided uniformly. The bipolar plate is completely surrounded by plasma and is in a stable glow plasma. The plasma-activated nitrogen element collides, diffuses, and reacts uniformly with the surface of the bipolar plate flow channels to generate titanium nitride.

[0029] Specifically, the nitriding time is controlled at 2-6 hours, the nitriding pressure at 1-30 Pa, and the nitriding substrate temperature at 400-800℃. By nitriding at these temperatures, pressures, and times, nanocrystals of the target size can be obtained. Preferably, when the nitriding pressure is less than 15 Pa, the nitriding temperature does not exceed 550℃, and the nitriding time is not less than 3 hours; when the pressure is greater than or equal to 15 Pa, the nitriding temperature is 550-800℃, and the nitriding time is not less than 2 hours. The lower the pressure, the better the nitriding effect; therefore, the nitriding temperature and time are carefully controlled. At high pressures, the nitriding effect is generally poor; therefore, the nitriding temperature and time are increased to ensure the desired nitriding effect.

[0030] The voltage between the plasma plates of the parallel-plate capacitor is 0.8-2KV, the current is 0.2-0.8A, and the self-bias voltage is less than 0.8KV (the operating voltage and current of the parallel-plate capacitor will be adjusted as the equipment is modified). The surface of the bipolar flow channel structure is simultaneously acted upon by plasma, forming a dense titanium nitride nanocrystalline film in situ on the titanium substrate surface. The grain size is 5-20nm, the film thickness is 50-200nm, and the grain orientation is anisotropic. This invention utilizes nitriding to enable in-situ growth of titanium nitride grains, resulting in good adhesion between the film and the substrate.

[0031] Since both the cathode and anode of the titanium-based bipolar plate have flow channels, after nitriding one side of the anode plate, the titanium-based bipolar plate is flipped over, and the above process is repeated on the cathode plate of the other layer for nitriding.

[0032] Step 2: Place the nitrided titanium-based bipolar plate in the magnetron sputtering chamber, control the sputtering temperature to 200-550℃ and the bias voltage to 100-300V, and sputter a metal nitride nanocrystalline coating on the titanium nitride surface formed by plasma nitriding. The coating material system is a corrosion-resistant and highly conductive transition metal nitride, which is titanium nitride, tantalum nitride or niobium nitride. The coating thickness is greater than 100nm, the coating grain size is 5-40nm, and the adhesion between the coating prepared by magnetron sputtering and the titanium-based bipolar plate is greater than 30N.

[0033] Step 3: After preparing the metal nitride coating using magnetron sputtering, annealing is performed at a temperature of 400-600℃ for 1-4 hours. Preferably, when the annealing temperature is not higher than 500℃, the annealing time is not less than 3 hours; when the annealing temperature is higher than 500℃, the annealing time is less than 3 hours. This process allows the two phases on both sides of the interface to diffuse into each other, reducing lattice distortion and improving the bonding force between the two phases. Annealing also releases and reduces the internal stress between grains. Subsequently, the furnace is cooled at a rate not exceeding 5℃ / min. By limiting the cooling rate, slow diffusion between grains is allowed, further improving the grain bonding force. The goal is to maintain a grain size of less than 50nm in the internal titanium nitride film and an adhesion force greater than 40N between the coating and the bipolar plate substrate.

[0034] Example 1

[0035] A bipolar titanium substrate was placed in a plasma nitriding apparatus. The bipolar substrate was positioned on a parallel-plate capacitor plasma cathode, with the side containing the flow channels facing the parallel-plate anode, at a distance of 80 mm. The nitriding time was controlled at 4 hours, the nitriding pressure at 10 Pa, and the substrate temperature at 500 °C. The voltage between the parallel-plate capacitor plasma electrodes was 0.8 kV, the current at 0.4 A, and the self-bias voltage at 0.65 kV. The bipolar substrate was completely encapsulated by plasma, resulting in uniform and dense titanium nitride with a grain size of approximately 8 nm and anisotropic grain orientation. The nitrided bipolar substrate was then placed in a magnetron sputtering chamber, with the sputtering temperature controlled at 300 °C and the bias voltage at 150 V. A nano-titanium nitride coating was sputtered onto the surface of the plasma-nitrided titanium nitride, with a coating thickness of 100 nm and a grain size of approximately 15 nm. The adhesion between the magnetron-sputtered coating and the bipolar substrate was approximately 35 N. After magnetron sputtering, annealing was performed at a controlled temperature of 420℃ for 3.5 hours with a furnace cooling rate of 5℃ / min. The resulting coating had a grain size of approximately 20 nm and an adhesion strength of 42 N to the bipolar substrate. The composite coating exhibited a contact resistance of 7.5 mΩcm. 2 The self-corrosion current density is 0.93 μA / cm. 2 The contact resistance and self-corrosion current density tested in this invention were performed using methods in accordance with the national standard GB / T 20042.6-2011 "Proton Exchange Membrane Fuel Cells Part 6: Test Methods for Bipolar Plate Characteristics". The bonding strength test was performed in accordance with GB / T 30707-2014 "Test Method for Bond Strength of Fine Ceramic Coatings - Scratch Method". The methods used in the following embodiments are the same and will not be described in detail.

[0036] SEM characterization results are as follows Figure 1 As shown, the titanium nitride coating prepared by direct magnetron sputtering in the comparative scheme has spherical grains with a grain size of about 35 nm. In contrast, the titanium nitride composite coating prepared by the composite preparation method described in Example 1 has a significantly reduced grain size of about 20 nm. The grooved structure on the substrate surface is uniformly covered by the coating, exhibiting good coverage and uniformity.

[0037] The contact resistance test results of the coating are as follows: Figure 2 As shown, the contact resistance gradually decreases with increasing contact pressure. Under 1.5 MPa conditions, the contact resistance of the commercial pure titanium substrate in the comparative scheme is approximately 20 mΩcm. 2 The contact resistance of the titanium nitride coating prepared by direct magnetron sputtering is approximately 10 mΩcm. 2 The contact resistance of the titanium nitride composite coating prepared by the composite preparation method described in Example 1 is approximately 7.5 mΩcm. 2 The contact resistance is significantly reduced.

[0038] Corrosion performance test results are as follows Figure 3 As shown, the corrosion test solution used was 0.5 mol / L H2SO4 + 2 ppmF. - The test temperature was 80℃. In the comparison, the self-corrosion current density of the commercially available pure titanium substrate was approximately 87 μA / cm². 2 The self-corrosion current density of the titanium nitride coating prepared by direct magnetron sputtering is approximately 35 μA / cm. 2 The self-corrosion current density of the titanium nitride composite coating prepared by the composite preparation method described in Example 1 is approximately 0.93 μA / cm. 2 The self-corrosion current density is significantly reduced.

[0039] Example 2

[0040] A bipolar titanium substrate was placed in a plasma nitriding apparatus, positioned on a parallel-plate capacitor plasma cathode, with the side containing the flow channels facing the parallel-plate anode, 50 mm away. The nitriding time was controlled at 4 hours, the nitriding pressure at 10 Pa, and the substrate temperature at 400 °C. The voltage between the parallel-plate capacitor plasma electrodes was 0.8 kV, the current at 0.6 A, and the self-bias voltage at 0.75 kV. The bipolar substrate was completely encapsulated by plasma, resulting in uniform and dense titanium nitride with a grain size of approximately 5 nm and anisotropic grain orientation. The nitrided bipolar substrate was then placed in a magnetron sputtering chamber, with the sputtering temperature controlled at 300 °C and the bias voltage at 150 V. A nano-titanium nitride coating was sputtered onto the surface of the plasma-nitrided titanium nitride, with a coating thickness of 100 nm and a grain size of approximately 10 nm. The adhesion between the magnetron-sputtered coating and the bipolar substrate was approximately 32 N. After magnetron sputtering, annealing was performed at a controlled temperature of 400℃ for 4 hours, with a furnace cooling rate of 5℃ / min. The resulting coating had a grain size of approximately 13 nm and an adhesion strength of 45 N to the bipolar substrate. The composite coating exhibited a contact resistance of 6.3 mΩcm. 2 The self-corrosion current density is 0.95 μA / cm. 2 .

[0041] The contact resistance test results of the coating are as follows: Figure 2 As shown, the contact resistance gradually decreases with increasing contact pressure. Under 1.5 MPa conditions, the contact resistance of the commercial pure titanium substrate in the comparative scheme is approximately 20 mΩcm. 2 The contact resistance of the titanium nitride coating prepared by direct magnetron sputtering is approximately 10 mΩcm. 2 The contact resistance of the titanium nitride composite coating prepared by the composite preparation method described in Example 2 is approximately 6.3 mΩcm. 2 The contact resistance is significantly reduced.

[0042] Corrosion performance test results are as follows Figure 3As shown, the corrosion test solution used was 0.5 mol / L H2SO4 + 2 ppmF. - The test temperature was 80℃. In the comparison, the self-corrosion current density of the commercially available pure titanium substrate was approximately 87 μA / cm². 2 The self-corrosion current density of the titanium nitride coating prepared by direct magnetron sputtering is approximately 35 μA / cm. 2 The self-corrosion current density of the titanium nitride composite coating prepared by the composite preparation method described in Example 2 is approximately 0.95 μA / cm. 2 The self-corrosion current density is significantly reduced.

[0043] Example 3

[0044] A bipolar titanium substrate was placed in a plasma nitriding apparatus, positioned on a parallel-plate capacitor plasma cathode, with the side containing the flow channels facing the parallel-plate anode, 100 mm away. The nitriding time was controlled at 3 hours, the nitriding pressure at 15 Pa, and the substrate temperature at 650 °C. The voltage between the parallel-plate capacitor plasma electrodes was 1 kV, the current at 0.8 A, and the self-bias voltage at 0.7 kV. The bipolar substrate was completely encapsulated by plasma, resulting in uniform and dense titanium nitride with a grain size of approximately 5 nm and anisotropic grain orientation. The nitrided bipolar substrate was then placed in a magnetron sputtering chamber, with the sputtering temperature controlled at 200 °C and the bias voltage at 200 V. A nano-niobium nitride coating was sputtered onto the surface of the plasma-nitrided titanium nitride, with a coating thickness of 150 nm and a grain size of approximately 8 nm. The adhesion between the magnetron-sputtered coating and the bipolar substrate was approximately 32 N. After magnetron sputtering, annealing was performed at a controlled temperature of 500℃ for 3 hours, with a furnace cooling rate of 5℃ / min. The resulting coating had a grain size of approximately 18 nm and an adhesion strength of 32 N to the bipolar substrate. The composite coating had a contact resistance of 4.3 mΩcm. 2 The self-corrosion current density is 0.77 μA / cm. 2 .

[0045] Example 4

[0046] A bipolar titanium substrate was placed in a plasma nitriding apparatus, positioned on a parallel-plate capacitor plasma cathode, with the side containing the flow channels facing the parallel-plate anode, 100 mm away. The nitriding time was controlled at 5 hours, the nitriding pressure at 15 Pa, and the substrate temperature at 650 °C. The voltage between the parallel-plate capacitor plasma electrodes was 1.2 kV, the current at 0.8 A, and the self-bias voltage at 0.7 kV. The bipolar substrate was completely encapsulated by plasma, resulting in uniform and dense titanium nitride with a grain size of approximately 15 nm and anisotropic grain orientation. The nitrided bipolar substrate was then placed in a magnetron sputtering chamber, with the sputtering temperature controlled at 300 °C and the bias voltage at 150 V. A nano-niobium nitride coating was sputtered onto the surface of the plasma-nitrided titanium nitride, with a coating thickness of 150 nm and a grain size of approximately 20 nm. The adhesion between the magnetron-sputtered coating and the bipolar substrate was approximately 32 N. After magnetron sputtering, annealing was performed at a controlled temperature of 600℃ for 2.5 hours with a furnace cooling rate of 5℃ / min. The resulting coating had a grain size of approximately 23 nm and an adhesion strength of 38 N to the bipolar substrate. The composite coating had a contact resistance of 3.2 mΩcm. 2 The self-corrosion current density is 0.86 μA / cm. 2 .

[0047] Example 5

[0048] A bipolar titanium substrate was placed in a plasma nitriding apparatus, positioned on a parallel-plate capacitor plasma cathode, with the side containing the flow channels facing the parallel-plate anode, 30 mm away. The nitriding time was controlled at 2 hours, the nitriding pressure at 20 Pa, and the substrate temperature at 650 °C. The voltage between the parallel-plate capacitor plasma electrodes was 0.8 kV, the current at 0.55 A, and the self-bias voltage at 0.8 kV. The bipolar substrate was completely encapsulated by plasma, resulting in uniform and dense titanium nitride with a grain size of approximately 18 nm and anisotropic grain orientation. The nitrided bipolar substrate was then placed in a magnetron sputtering chamber, with the sputtering temperature controlled at 550 °C and the bias voltage at 100 V. A nano-tantalum nitride coating was sputtered onto the surface of the plasma-nitrided titanium nitride, with a coating thickness of 300 nm and a grain size of approximately 30 nm. The adhesion between the magnetron-sputtered coating and the bipolar substrate was approximately 32 N. After magnetron sputtering, annealing was performed at a controlled temperature of 550℃ for 1 hour with a furnace cooling rate of 5℃ / min. The resulting coating had a grain size of approximately 32 nm and an adhesion strength of 32 N to the bipolar substrate. The composite coating had a contact resistance of 4.3 mΩcm. 2 The self-corrosion current density is 0.77 μA / cm. 2 .

[0049] Example 6

[0050] A bipolar titanium substrate was placed in a plasma nitriding apparatus. The bipolar substrate was positioned on a parallel-plate capacitor plasma cathode, with the side containing the flow channels facing the parallel-plate anode, 30 mm away from the anode. The nitriding time was controlled at 6 hours, the nitriding pressure at 30 Pa, and the substrate temperature at 800 °C. The voltage between the parallel-plate capacitor plasma electrodes was 1.2 kV, the current at 0.65 A, and the self-bias voltage at 0.6 kV. The bipolar substrate was completely encapsulated by plasma, resulting in uniform and dense titanium nitride with a grain size of approximately 20 nm and anisotropic grain orientation. The nitrided bipolar substrate was then placed in a magnetron sputtering chamber, with the sputtering temperature controlled at 200 °C and the bias voltage at 300 V. A nano-tantalum nitride coating was sputtered onto the surface of the titanium nitride formed by plasma nitriding, with a coating thickness of 200 nm and a grain size of approximately 35 nm. The adhesion between the magnetron sputtered coating and the bipolar substrate was approximately 32 N. After magnetron sputtering, annealing was performed at a controlled temperature of 600℃ for 2.5 hours with a furnace cooling rate of 5℃ / min. The resulting coating had a grain size of approximately 40 nm and an adhesion strength of 47 N to the bipolar substrate. The composite coating had a contact resistance of 7.6 mΩcm. 2 The self-corrosion current density is 1.09 μA / cm. 2 .

[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high conductive and strong corrosion resistant coating on a PEM electrolyzer bipolar plate, characterized in that, A titanium nitride nanocrystalline film was prepared on the surface of a titanium-based bipolar plate by nitriding; a metal nitride nanocrystalline coating was sputtered onto the surface of the titanium nitride nanocrystalline film to prepare a highly conductive and corrosion-resistant coating on the surface of the titanium-based bipolar plate. The nitriding is plasma nitriding. During the nitriding process, the side with the flow channels faces the anode plate, and the distance between the side with the flow channels and the anode plate is ≤100mm. The nitriding time is 2-6 h, the nitriding pressure is 1-30 Pa, and the nitriding substrate temperature is 400-800 ℃. The sputtered metal nitride nanocrystalline coating is titanium nitride, tantalum nitride, or niobium nitride. During the sputtering process, the sputtering temperature is 200-550 ℃ and the bias voltage is 100-300 V; after sputtering the metal nitride nanocrystalline coating, an annealing operation is performed. The titanium nitride nanocrystalline film has a grain size of 5~20 nm; the metal nitride nanocrystalline coating has a grain size of 5~40 nm.

2. The method for preparing a high-conductivity and high-corrosion- resistance coating for a PEM electrolyzer bipolar plate according to claim 1, characterized in that, When the nitriding pressure is <15 Pa, the nitriding temperature is ≤550 ℃ and the nitriding time is ≥3h; when the pressure is ≥15 Pa, the nitriding temperature is 550-800℃ and the nitriding time is ≥2h.

3. The method of claim 1, wherein the coating is prepared by the steps of: (a) preparing a solution of the polymer and the conductive material; (b) applying the solution to the surface of the bipolar plate; (c) drying the solution to form a coating; and (d) baking the coating to form a coating with a thickness of 1 to 100 micrometers. The annealing temperature is 400-600 ℃, and the annealing time is 1-4 h.

4. The method according to claim 3, wherein the method is characterized by, When the annealing temperature is ≤500 ℃, the annealing time is ≥3 h; when the annealing temperature is >500 ℃, the annealing time is <3 h.

5. A high conductive and strong corrosion resistant coating for PEM electrolyzer bipolar plates prepared by the method of any one of claims 1-4, characterized in that, The invention comprises a titanium nitride nanocrystalline film and a metal nitride nanocrystalline coating on the surface of a titanium-based bipolar plate, wherein the metal nitride nanocrystalline coating is located outside the titanium nitride nanocrystalline film; the thickness of the titanium nitride nanocrystalline film is 50~200 nm; the grain size of the metal nitride nanocrystalline coating is 5~40 nm and the thickness is ≥100 nm.

Citation Information

Patent Citations

  • Nano multilayer gradient composite anti-erosion coating structure and preparation method thereof

    CN107326360A

  • Method of wear-resistant coating formation on surface of articles made of structural steel

    RU2131480C1