A submerged arc welding method for Q500ME steel plate for high-strength wind tower
By optimizing the submerged arc welding wire composition and welding parameters, combined with no preheating and slow cooling heat treatment, the problem of matching the weld metal strength and -40°C impact toughness in Q500ME steel plate welding was solved, reducing cold crack sensitivity and achieving high efficiency and safety. The excellent welding effect meets the usage requirements of high-strength wind towers.
Patent Information
- Application Number
- CN202311426645.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-10-31
AI Technical Summary
The existing welding method of Q500ME steel plate cannot effectively match the strength and -40°C impact toughness of the weld metal. Improper welding heat input affects the welding thermal cycle process, resulting in increased crack sensitivity of the welded joint, and fails to take into account different thicknesses of the steel plate. The groove processing affects the welding performance and efficiency.
The chemical composition of submerged arc welding wire is C: 0.06~0.10%, Mn: 1.40~1.90%, Si: ≤0.35%, S: ≤0.010%, P: ≤0.012%, Ni: 0.50~0.80%, Mo: 0.20 -0.40%, Ti: ≤0.15%, the balance is Fe and unavoidable impurities, submerged arc flux with alkalinity ≥1.8, welding heat input ≤36KJ/cm, the groove processing method is determined according to the thickness of the steel plate, and the ambient temperature is not lower than 25℃ There is no preheating for welding, and slow cooling heat treatment is performed after welding to reduce cold crack sensitivity.
It achieves excellent comprehensive mechanical properties and impact properties of welded joints, reduces cold crack sensitivity, takes into account welding performance and efficiency, and meets the use requirements of high-strength wind towers. The tensile strength of welded joints is ≥620MPa, and the impact energy at -40℃ ≥31J, the surface and cross-section crack rates are basically zero.
Smart Images

Figure CN117324732B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of steel plate material welding, and particularly relates to a submerged arc welding method for a Q500ME steel plate for a high-strength wind tower. Background Art
[0002] With the rapid development of my country's wind power industry and cost constraints, steel used in wind towers has gradually become lighter, and the strength of steel plates has gradually developed towards high strength. At present, Q420-level high-strength steel plates have been successfully used on wind towers. Q500ME, as a low-alloy high-strength steel plate with thermomechanical rolling as its delivery state, has better comprehensive performance and welding performance than Q420 according to GB / T 1591-2018 standard. Therefore, the research and development of welding methods for Q500ME steel plates is of great significance to improving the high strength of wind power towers.
[0003] The existing submerged arc welding method of Q500 grade steel plate is concentrated on Q500qE steel for bridges, while the welding of Q500ME steel plate is still relatively blank. The existing welding materials fail to match its weld metal strength and -40℃ impact toughness. Improper welding heat input affects the welding thermal cycle process, and affects the microstructure and mechanical properties of the weld metal and heat-affected zone of the weld joint, which will lead to increased weld crack sensitivity and decreased mechanical properties such as strength and toughness and impact properties. Secondly, improper preheating temperature and post-weld heat treatment will further increase the cold crack sensitivity of the weld joint, thereby affecting the safety and reliability of the tower longitudinal seam, circumferential seam and door frame welding. In addition, the thickness of the Q500ME steel plate used in the entire tower is generally 12 to 60 mm. Failure to coordinate reasonable groove processing according to different thicknesses of the steel plate results in a failure to balance performance and efficiency, thereby failing to meet application requirements. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a submerged arc welding method for Q500ME steel plate for high-strength wind towers. The welded joint has excellent comprehensive mechanical properties, sufficient safety margin of mechanical properties and impact properties, effectively reduces the sensitivity of cold cracks, can take into account both performance and efficiency, and meet the use requirements of high-strength wind towers.
[0005] The technical solution adopted by the present invention to solve its technical problem is:
[0006] A submerged arc welding method for a Q500ME steel plate for a high-strength wind tower, the method comprising:
[0007] Selection of welding materials: The chemical composition of submerged arc welding wire includes by weight percentage: C: 0.06-0.10%, Mn: 1.40-1.90%, Si: ≤0.35%, S: ≤0.010%, P: ≤0.012%, Ni: 0.50-0.80%, Mo: 0.20-0.40%, Ti: ≤0.15%, the balance is Fe and unavoidable impurities; the basicity of submerged arc welding flux is ≥1.8;
[0008] The butt joint of the steel plate made of Q500ME material is not grooved or grooved, and the butt joint of the steel plate is subjected to multi-layer and multi-pass submerged arc welding with welding materials, and the welding heat input is ≤36KJ / cm.
[0009] The selection basis of the above welding materials is:
[0010] For Q500ME steel, the composition of submerged arc welding wire is designed by comprehensively considering the strength of weld metal, -40℃ impact toughness matching with steel plate and crack sensitivity of high-strength steel: (1) In order to reduce the crack sensitivity of high-strength steel in weld, the low C / P / S composition matching principle is adopted; (2) In order to ensure the safety margin of mechanical properties and impact properties of weld joint, the "slightly higher equal strength" matching principle is adopted, that is, the mechanical properties of weld joint are not lower than those of Q500ME steel plate, Mo / Ni alloy is used to ensure high strength and high toughness of weld, and fine grain strengthening is achieved by adding microalloy Ti; at the same time, in order to obtain a better combination of strength, plasticity and toughness, the submerged arc welding flux is selected with basicity ≥1.8, which has good arc stability and slag removal properties.
[0011] The above welding heat input is determined based on:
[0012] Since changes in welding heat input affect the welding thermal cycle process, and thus affect the microstructure and mechanical properties of the weld metal and heat-affected zone of the weld joint, in order to ensure sufficient safety margin for the performance of the weld joint, the welding heat input is ≤36KJ / cm, which can avoid excessive welding heat input and reduce tensile properties, especially the -40℃ Charpy V-notch impact energy of various parts of the weld joint.
[0013] Furthermore, the thickness of the steel plate is ≤60 mm, and the diameter of the submerged arc welding wire is 4.0 mm.
[0014] Furthermore, the submerged arc welding flux is SJ102G, which is a fluorine-alkali type welding flux. The sintered welding flux has high basicity and good metallurgical effect. The submerged arc welding flux is baked at 350° C. for 2 to 3 hours before use to prevent moisture from increasing the risk of hydrogen-induced cracking.
[0015] Furthermore, the groove processing is determined according to the thickness h of the steel plate:
[0016] When 12mm≤h<20mm, no groove is made at the butt joint of the steel plate, which can reduce welding residual deformation and achieve high efficiency and energy saving;
[0017] When 20mm≤h<40mm, V-shaped groove is used at the butt joint of steel plates to take into account both weld penetration and efficiency;
[0018] When 40mm≤h≤60mm, an asymmetric X-shaped groove is used at the steel plate butt joint to reduce welding workload, improve work efficiency, and obtain better weld formation.
[0019] Furthermore, the V-shaped groove angle and the front and back groove angles of the asymmetric X-shaped groove are both 50° to 70°, which can fully penetrate the weld, the root blunt edge is 3 to 4 mm, the angular deformation is reduced, the groove assembly gap is 0 to 2 mm, and the weld quality is comprehensively improved.
[0020] Furthermore, when submerged arc welding is performed without preheating before welding at an ambient temperature of not less than 25°C, according to the GB / T 4675.1 standard test, the surface crack rate and cross-sectional crack rate of the joint are basically zero when welding without preheating, which is highly efficient and energy-saving and can effectively prevent the occurrence of welding cold cracks.
[0021] Furthermore, taking into account the composition of steel and welding materials, the interpass temperature of the multi-layer and multi-pass submerged arc welding is controlled at ≤200°C, which can avoid the degradation of mechanical properties due to coarse grains caused by excessively high temperature.
[0022] Furthermore, the interpass temperature is 150-180°C, which can avoid the increase of temperature internal stress of the weld due to too low temperature.
[0023] Furthermore, the welding current is 630-680A, the welding voltage is 32-35V, and the welding speed is 36-42cm / min. The welding operation is simple, efficient and energy-saving. It can avoid defects such as welding leakage, burn-through, cracks, large deformation, spatter, etc. caused by excessive welding current, and avoid defects such as incomplete penetration, incomplete fusion, slag inclusion, and poor seam formation caused by too small welding current; the welding voltage and welding current are coordinated, and under certain conditions of welding current and welding submerged arc voltage, the appropriate welding speed is combined to make the weld width and penetration depth appropriate, and the mechanical properties meet the requirements.
[0024] Furthermore, after welding, dehydrogenation treatment is carried out by keeping the temperature at 250℃ for 2 to 3 hours and then performing slow cooling and heat treatment. The dehydrogenation treatment accelerates the escape of hydrogen in the weld and heat-affected zone, which can effectively reduce the cold crack sensitivity of the welded joint, thereby ensuring the safety and reliability of the tower longitudinal seam, circumferential seam and door frame welding.
[0025] Furthermore, using heat-insulating cotton to cover the butted steel plates for slow cooling can make the stress distribution smoother.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The present invention is directed to Q500ME steel for high-strength wind towers. The composition of the submerged arc welding wire is designed according to the matching principles of "low C / P / S" and "slightly higher than equal strength". By adding low C / P / S, Mo / Ni alloy and Ti, combined with a submerged arc welding flux with a basicity of ≥1.8 and a welding heat input of ≤36KJ / cm, the tensile strength of the submerged arc welding butt joint and the impact energy of each zone at -40°C of the joint reach a relatively high level. The invention has excellent low-temperature impact toughness and safety reserve, and solves the problem of poor comprehensive mechanical properties caused by improper welding materials and welding heat input. The mechanical properties and impact properties have sufficient safety margins, the tensile strength is ≥620MPa, the impact energy at -40°C is ≥31J, and the joint side bending d=4a, 180°.
[0028] (2) The butt joint manufacturing process of the present invention adopts no preheating before welding and slow cooling and dehydrogenation treatment after welding, which solves the existing problem of weld crack sensitivity caused by improper welding preheating and post-weld heat treatment. The surface crack rate and cross-sectional crack rate of the joint are basically zero, ensuring the safety and reliability of the tower longitudinal seam, circumferential seam and door frame welding.
[0029] (3) The present invention determines different groove processing systems according to the thickness of the steel plate, and realizes the manufacture of Q500ME butt joints with steel plates ≤60mm thick for high-strength wind towers, which basically covers the thickness of the entire tower. The welded joints after multi-layer and multi-pass welding have excellent comprehensive mechanical properties, strong practicality, simple welding operation, high efficiency and energy saving, and are suitable for the manufacture, promotion and application of high-strength wind towers. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0031] Figure 1 is a welding schematic diagram of Example 1 of the present invention;
[0032] Figure 2 : is a diagram showing the weld crack condition of Example 1 of the present invention, Figure 2 (a) indicates the crack situation of weld section. Figure 2 (b) Indicates the crack situation on the weld surface.
[0033] Figure 3 is a welding schematic diagram of embodiment 2 of the present invention;
[0034] Figure 4 is a diagram showing the weld crack condition of Example 2 of the present invention, Figure 4 (a) indicates the crack situation of weld section. Figure 4 (b) Indicates the crack situation on the weld surface.
[0035] Figure 5 is a welding schematic diagram of embodiment 3 of the present invention;
[0036] Figure 6 is a diagram showing the weld crack condition of Example 3 of the present invention, Figure 6 (a) indicates the crack situation of weld section. Figure 6 (b) Indicates the crack situation on the weld surface.
[0037] Markings in the figure: R-groove assembly gap, T-steel plate thickness, α-front groove angle, β-reverse groove angle, B-root blunt edge, the numbers at the weld in the figure represent the welding pass. DETAILED DESCRIPTION
[0038] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0039] Embodiment 1:
[0040] like Figure 1 As shown, a preferred embodiment of the submerged arc welding method of a high-strength wind tower steel plate Q500ME according to the present invention is shown, and the method comprises:
[0041] The steel plate is Q500ME produced by thermomechanical rolling, with a yield strength of ≥500MPa and dimensions of 600mm long × 300mm wide × 12mm thick. The weld is welded without preheating at an ambient temperature not lower than 25°C. The inclined Y groove test is carried out at room temperature according to GB / T 4675.1 standard. The weld crack results are as follows: Figure 2 As shown, the results show that there are no cracks in the weld section / surface, which shows that welding without preheating can effectively prevent the occurrence of welding cold cracks.
[0042] Selection of welding materials: The chemical composition of the submerged arc welding wire includes by weight percentage: C: 0.07%, Mn: 1.65%, Si: 0.21%, S: 0.006%, P: 0.005%, Ni: 0.68%, Mo: 0.34%, Ti: 0.09%, the balance is Fe and unavoidable impurities; the diameter of the submerged arc welding wire is 4.0mm; the submerged arc welding flux is SJ102G, the basicity is 1.9, and the submerged arc welding flux is baked at 350℃ for 2h before use;
[0043] The submerged arc welding groove adopts non-groove, and the groove assembly gap R is 0~1mm;
[0044] Submerged arc welding is performed on the butt joint of the steel plate with welding materials. The welding parameters are: no preheating before welding at an ambient temperature not lower than 25°C, welding current is 630A, welding voltage is 33V, welding speed is 42cm / min, welding heat input is 30KJ / cm, butt joints are welded by multi-layer multi-pass submerged arc welding, and the inter-pass temperature is controlled at 150-180°C;
[0045] After welding, the temperature is kept at 250℃ for 2h, and then the butted steel plates are covered with insulation cotton to perform slow cooling and heating treatment to room temperature to achieve hydrogen removal treatment and obtain the finished product after welding.
[0046] Embodiment 2:
[0047] like Figure 2 As shown, a preferred embodiment of the submerged arc welding method of a high-strength wind tower steel plate Q500ME according to the present invention is shown, and the method comprises:
[0048] The steel plate is Q500ME produced by thermomechanical rolling, with a yield strength of ≥500MPa and dimensions of 600mm long × 300mm wide × 20mm thick. The weld is welded without preheating at an ambient temperature not lower than 25°C. The inclined Y groove test is carried out at room temperature according to GB / T 4675.1 standard. The weld crack results are as follows: Figure 4 As shown, the results show that there are no cracks in the weld section / surface, which shows that welding without preheating can effectively prevent the occurrence of welding cold cracks.
[0049] Selection of welding materials: The chemical composition of the submerged arc welding wire includes by weight percentage: C: 0.06%, Mn: 1.65%, Si: 0.23%, S: 0.007%, P: 0.008%, Ni: 0.62%, Mo: 0.33%, Ti: 0.10%, the balance is Fe and unavoidable impurities; the diameter of the submerged arc welding wire is 4.0mm; the submerged arc welding flux is SJ102G, the basicity is 1.9, and the submerged arc welding flux is baked at 350℃ for 2h before use;
[0050] The submerged arc welding groove adopts a V-shaped groove, the V-shaped groove angle α is 60°, the root blunt edge is 4mm, and the groove assembly gap R is 1mm;
[0051] After beveling, the butt joint of the steel plate is welded with welding materials by submerged arc welding. The welding parameters are as follows: no preheating before welding at an ambient temperature not lower than 25°C, welding current of 680A, welding voltage of 32V, welding speed of 42cm / min, welding heat input of 32KJ / cm, butt joints are welded by multi-layer multi-pass submerged arc welding, and the interpass temperature is controlled at 150-180°C;
[0052] After welding, the temperature is kept at 250℃ for 2h, and then the butted steel plates are covered with insulation cotton to perform slow cooling and heating treatment to room temperature to achieve hydrogen removal treatment and obtain the finished product after welding.
[0053] Embodiment 3:
[0054] like Figure 3 As shown, a preferred embodiment of the submerged arc welding method of a high-strength wind tower steel plate Q500ME according to the present invention is shown, and the method comprises:
[0055] The steel plate is Q500ME produced by thermomechanical rolling, with a yield strength of ≥500MPa and dimensions of 600mm long × 300mm wide × 40mm thick. The weld is welded without preheating at an ambient temperature not lower than 25°C. The inclined Y groove test is carried out at room temperature according to GB / T 4675.1 standard. The weld crack results are as follows: Figure 6 As shown, the results show that there are no cracks in the weld section / surface, which shows that welding without preheating can effectively prevent the occurrence of welding cold cracks.
[0056] Selection of welding materials: The chemical composition of the submerged arc welding wire includes by weight percentage: C: 0.08%, Mn: 1.67%, Si: 0.20%, S: 0.008%, P: 0.005%, Ni: 0.65%, Mo: 0.35%, Ti: 0.09%, the balance is Fe and unavoidable impurities; the diameter of the submerged arc welding wire is 4.0mm; the submerged arc welding flux is SJ102G, the basicity is 1.9, and the submerged arc welding flux is baked at 350℃ for 2h before use;
[0057] The submerged arc welding groove adopts an asymmetric X-shaped groove. The front groove angle α of the asymmetric X-shaped groove is 50°, the front groove depth accounts for 2 / 3 of the steel plate thickness, the back groove angle β is 70°, the root blunt edge B is 4mm, the sum of the back groove depth and the root blunt edge accounts for 1 / 3 of the steel plate thickness, and the groove assembly clearance R is 1mm;
[0058] After beveling, the butt joint of the steel plate is welded with welding materials by submerged arc welding. The welding parameters are as follows: no preheating before welding at an ambient temperature not lower than 25°C, welding current of 680A, welding voltage of 34V, welding speed of 38cm / min, welding heat input of 36KJ / cm, butt joints are welded by multi-layer and multi-pass submerged arc welding, and the interpass temperature is controlled at 150-180°C;
[0059] After welding, the temperature is kept at 250℃ for 2h, and then the butted steel plates are covered with insulation cotton to perform slow cooling and heating treatment to room temperature to achieve hydrogen removal treatment and obtain the finished product after welding.
[0060] Comparative Example 1:
[0061] A submerged arc welding method for a Q500ME steel plate is different from that of Example 2 in that the preheating temperature before welding is 80° C., and a finished product after welding is obtained.
[0062] Comparative Example 2:
[0063] A submerged arc welding method for a Q500ME steel plate is different from Example 3 in that the welding heat input is 38 KJ / cm and a finished product is obtained after welding.
[0064] The welded finished products obtained in the embodiments and comparative examples were subjected to tensile tests according to GB / T228.1, impact tests according to GB / T229, bending tests according to GB / T232, and welding crack tests according to GB / T 4675.1, and the mechanical properties of the welded joints were tested. The tensile properties, lateral bending properties, flaw detection grades, and impact properties of the welded joints are shown in Table 1:
[0065] Table 1. Properties of different finished welded joints
[0066] performance Example 1 Example 2 Comparative Example 1 Example 3 Comparative Example 2 Tensile strength MPa 618 693 683 671 668 Fracture location Base Material Base Material Base Material Base Material Base Material Side bend (d = 4a, 180°) qualified qualified qualified qualified qualified Flaw detection level Level I Level I Level I Level I Level I -40℃ impact energy J (weld) 70 / 90 / 82 81 / 83 / 85 88 / 92 / 76 80 / 150 / 136 56 / 37 / 44 -40℃ impact energy J (fusion line) 177 / 201 / 197 184 / 180 / 154 182 / 185 / 175 210 / 207 / 155 188 / 152 / 143
[0067] It can be seen from Table 1 above that the welded joints of Examples 1 to 3 have excellent comprehensive mechanical properties, achieve a good match between strength and toughness, and meet the requirements of welded joint tensile strength ≥620MPa, -40℃ impact energy ≥31J, joint side bending d=4a, and 180° qualified. For Example 1 and Example 2, it is further illustrated that welding without preheating has basically no effect on the performance of the welded joint, and it is feasible and less costly to adopt no preheating. For Example 2 and Example 3, it can be seen that in order to ensure sufficient safety margin for the performance of the welded joint, the performance is more suitable when the welding heat input is ≤36KJ / cm.
[0068] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A submerged arc welding method for high-strength wind tower steel plate Q500ME, characterized in that: The methods include: Selection of welding materials: The chemical composition of submerged arc welding wire includes by weight percentage: C: 0.06-0.10%, Mn: 1.40-1.90%, Si: 0.2-0.35%, S: ≤0.010%, P: ≤0.012%, Ni: 0.62-0.80%, Mo: 0.20-0.40%, Ti: ≤0.15%, the balance is Fe and unavoidable impurities; the basicity of submerged arc welding flux is ≥1.8; At the butt joint of Q500ME steel plate, there is no groove or after the groove is processed, the butt joint of the steel plate is subjected to multi-layer and multi-pass submerged arc welding with welding materials, and the welding heat input is ≤36KJ / cm; Submerged arc welding is performed without preheating before welding at an ambient temperature of not less than 25°C. The welding current is 630-680A, the welding voltage is 32-35V, and the welding speed is 36-42cm / min. After welding, the temperature is kept at 250°C for 2-3h and then slowly cooled and heated for dehydrogenation treatment.
2. The submerged arc welding method of a high-strength wind tower steel plate Q500ME according to claim 1 is characterized in that: The thickness of the steel plate is ≤60mm and the diameter of the submerged arc welding wire is 4.0mm.
3. The submerged arc welding method of a high-strength wind tower steel plate Q500ME according to claim 1 is characterized in that: The submerged arc welding flux is SJ102G, and the submerged arc welding flux is baked at 350° C. for 2 to 3 hours before use.
4. The submerged arc welding method of a high-strength wind tower steel plate Q500ME according to claim 1 is characterized in that: Determine the groove processing according to the steel plate thickness h: When 12mm≤h<20mm, no groove is made at the butt joint of the steel plate; When 20mm≤h<40mm, V-shaped groove is used at the butt joint of steel plates; When 40mm≤h≤60mm, an asymmetric X-shaped groove is used at the steel plate butt joint.
5. The submerged arc welding method of a high-strength wind tower steel plate Q500ME according to claim 4 is characterized in that: The V-shaped groove angle and the front and back groove angles of the asymmetric X-shaped groove are both 50°~70°, the blunt edge of the root is 3~4mm, and the groove assembly clearance is 0~2mm.
6. The submerged arc welding method of a high-strength wind tower steel plate Q500ME according to claim 1 is characterized in that: The interpass temperature of the multi-layer and multi-pass submerged arc welding is controlled at ≤200°C.
7. The submerged arc welding method of a high-strength wind tower steel plate Q500ME according to claim 1 is characterized in that: Use thermal insulation cotton to cover the butted steel plates for slow cooling.
Citation Information
Patent Citations
Welding method of high-strength steel for pressure steel pipe of 610MPa hydropower station
CN102101210A
High-strength Q500qE bridge steel thick plate submerged-arc welding method
CN103894710A