Heterojunction solar cell and method for preparing the same
During the preparation process of heterojunction solar cells, RPD equipment is used to deposit a thin indium-containing TCO seed layer and combined with PVD equipment to deposit an indium-free TCO film, which solves the problems of low RPD equipment productivity and high target material cost, and achieves The effect of reducing manufacturing costs and improving efficiency has promoted the industrial development of heterojunction solar cells.
Patent Information
- Application Number
- CN202311619461.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-11-30
AI Technical Summary
During the preparation process of heterojunction solar cells, the RPD equipment production capacity is too low, and dust is easily generated during the process, resulting in a short PM cycle, low overall equipment utilization, and high cost of coating targets, which affects industrial development.
RPD equipment is used to prepare a thin indium-containing TCO seed layer on the back, and PVD equipment is used to deposit an indium-free TCO film on it. Combined with indium-free materials, the cost of the TCO film is reduced and the conversion efficiency is improved.
It extends the normal operation time of RPD equipment, increases production capacity, reduces TCO film manufacturing costs, ensures battery efficiency to the maximum extent, and is conducive to large-scale manufacturing and industrial development.
Smart Images

Figure CN117423781B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of photovoltaic technology, and in particular to a heterojunction solar cell and a preparation method thereof. Background Art
[0002] The conversion efficiency of heterojunction (Silicon Hetero-Junction; SHJ) solar cell technology has reached 25.6%. The conversion efficiency of heterojunction back contact (HBC) cells developed based on heterojunction cells has reached 26.67%. At present, the conversion efficiency of heterojunction solar cells has reached the world efficiency record of 26.81%. Heterojunction solar cells are a kind of double-sided cells, which have many advantages such as simple process flow, high conversion efficiency, low temperature coefficient, energy saving in low-temperature manufacturing throughout the process, suitable for thin-film, natural double-sided power generation, good weak light response, etc., and have developed rapidly in the photovoltaic field. How to improve the efficiency of heterojunction solar cells, reduce their manufacturing costs, and ultimately convert them into power generation benefits is the focus of heterojunction industrialization today.
[0003] It should be noted that in the world efficiency record of 26.81% for heterojunction solar cells, its TCO (Transparent Conductive Oxide) film was deposited using reactive ion deposition (RPD) equipment. The TCO film of mass-produced heterojunction solar cells is basically deposited using physical vapor deposition (PVD) equipment. Nowadays, there are also very few heterojunction cells that use RPD and PVD equipment to co-deposit TCO films, deriving corresponding PAR equipment (PVD and RPD). In the PAR equipment, RPD equipment is used for coating the bottom of the cell (TCO film on the back), and PVD equipment is used for coating the top of the cell (TCO film on the front). Although heterojunction cells have appeared that use PAR equipment in combination with co-deposition of TCO films, when RPD equipment is used to prepare the back TCO film, in order to ensure the conductivity and back reflection of the TCO film, the thickness of the back TCO film is generally 100nm-120nm, which results in too low RPD production capacity. The RPD equipment itself is prone to generate dust during the process, resulting in a very short PM cycle, which greatly shortens the overall equipment utilization rate. At the same time, the target material required for RPD coating is much more expensive than the PVD target material, and the target material utilization rate of RPD equipment is low, generally less than 40%. This results in the heterojunction solar cells prepared by the combination of RPD and PVD having certain efficiency advantages, but the cost is relatively high, which is not conducive to industrial development. Summary of the invention
[0004] Based on this, it is necessary to provide a method for preparing a heterojunction solar cell. The method for preparing a heterojunction solar cell of the present invention can reduce the coating thickness of the RPD device, shorten its PM cycle, and improve its production capacity. At the same time, the combination of indium-free materials can further reduce the TCO film cost of the heterojunction solar cell, maximize the battery conversion efficiency, and facilitate industrial development.
[0005] An embodiment of the present application provides a method for preparing a heterojunction solar cell.
[0006] A method for preparing a heterojunction solar cell comprises the following steps:
[0007] Cleaning and texturing the silicon substrate;
[0008] Intrinsic amorphous silicon layers are respectively prepared on two surfaces of a silicon substrate;
[0009] Preparing an N-type doped layer on the front intrinsic amorphous silicon layer of the silicon substrate;
[0010] Preparing a P-type doped layer on the back intrinsic amorphous silicon layer of the silicon substrate;
[0011] Using an RPD device to prepare a back-side indium-containing TCO seed layer on the P-type doped layer, and using a PVD device to prepare a back-side indium-free TCO film on the back-side indium-containing TCO seed layer;
[0012] Using a PVD device to prepare a front indium-containing TCO seed layer on the N-type doped layer, and preparing a front indium-free TCO film on the front indium-containing TCO seed layer; and
[0013] A back electrode is prepared on the back indium-free TCO film, and a front electrode is prepared on the front indium-free TCO film.
[0014] In some of the embodiments, the silicon substrate is an N-type single crystal silicon wafer, the thickness of the silicon substrate is 60 μm to 180 μm, and the resistivity is 0.2 Ω.cm to 5 Ω.cm.
[0015] In some embodiments, the cleaning and texturing process for the silicon substrate includes the following steps:
[0016] The silicon substrate is treated with gettering equipment using a high-temperature tubular phosphorus diffusion or chain gettering equipment. The square resistance of the silicon substrate after gettering is 20Ω / □~40Ω / □;
[0017] A trough-type wet acid solution is used to remove the PSG layer on the surface of the silicon substrate after doping, and an alkaline solution is used to texture the surface of the silicon substrate so that both sides of the silicon substrate have a pyramid-shaped surface light-trapping structure. The silicon substrate is cleaned to remove the surface oxide layer.
[0018] In some embodiments, the cleaning of the silicon substrate includes the following steps: performing RCA cleaning on the silicon substrate, then using HF solution to clean the silicon substrate to remove the surface oxide layer, and finally cleaning with deionized water and drying the surface.
[0019] In some embodiments, when the intrinsic amorphous silicon layers are respectively prepared on two surfaces of the silicon substrate, the steps specifically include:
[0020] The intrinsic amorphous silicon layer is deposited by RF-PECVD; wherein, in the RF-PECVD process, the equipment power supply adopts 13.56MHz~40MHz, the process gas contains one or more of SiH4, H2, CO2, CH4, N2O, the deposition temperature is 160℃~220℃, and the deposition pressure is 0.2mbar~2mbar.
[0021] In some embodiments, the intrinsic amorphous silicon layer has a thickness of 2 nm to 10 nm.
[0022] In some embodiments, the N-type doped layer is an N-type doped amorphous silicon layer, a nanocrystalline silicon layer, or a microcrystalline silicon layer;
[0023] And / or, the thickness of the N-type doping layer is 5 nm to 20 nm.
[0024] In some embodiments, when preparing an N-type doped layer on the front intrinsic amorphous silicon layer of a silicon substrate, the steps include:
[0025] An N-type doped layer is deposited on the front intrinsic amorphous silicon layer of the silicon substrate by RF-CVD equipment or VHF-CVD equipment; the power supply of the RF-CVD equipment or VHF-CVD equipment adopts 13.56MHz, 26MHz or 40MHz, and the process gas contains one or more of SiH4, H2, CO2, CH4, N2O, PH3; the deposition temperature is 160℃~200℃, and the deposition pressure is 0.5mbar~5mbar.
[0026] In some embodiments, the P-type doped layer is a P-type doped amorphous silicon layer, a nanocrystalline silicon layer, or a microcrystalline silicon layer;
[0027] And / or, the thickness of the P-type doping layer is 5 nm to 30 nm.
[0028] In some embodiments, when preparing a P-type doped layer on the back intrinsic amorphous silicon layer of a silicon substrate, the steps include:
[0029] A p-type doped layer is deposited on the intrinsic amorphous silicon layer on the back side of the silicon substrate by an RF-CVD device or a VHF-CVD device; the power supply of the RF-CVD device or the VHF-CVD device adopts 13.56MHz to 40MHz, the process gas includes one or more of SiH4, H2, CO2, CH4, N2O, B2H6, TMB, the deposition temperature is 160℃ to 200℃, and the deposition pressure is 0.5mbar to 5mbar.
[0030] In some of the embodiments, the back indium-containing TCO seed layer is an ITO film, a VTTO film, a SCOT film, an IWO film, an ICO film or an IMO film;
[0031] And / or, the thickness of the back indium-containing TCO seed layer is 1 nm to 20 nm.
[0032] In some of the embodiments, when the RPD equipment is used to prepare the back indium-containing TCO seed layer on the P-type doped layer, the process temperature is 0-200°C, the process pressure is 0.3Pa-0.8Pa, and the process gas is Ar / O2 and Ar / H2 or H2O, wherein Ar / O2 is a necessary process gas and the rest are non-necessary process gases.
[0033] In some of the embodiments, the back-side indium-free TCO film has a thickness of 80 nm to 120 nm;
[0034] And / or, the back indium-free TCO film is a SnO2 film, a ZnO film, an AZO film, a GZO film or a GAZO film.
[0035] In some embodiments, when a back-side indium-free TCO film is prepared on the back-side indium-containing TCO seed layer using a magnetron sputtering device PVD device, the power density is 2KW / m 2 ~8KW / m 2 The process gases are Ar / O2 and Ar / H2 or H2O, among which Ar / O2 is a necessary process gas and the rest are non-essential process gases. The process pressure is 0.3Pa~0.8Pa and the process temperature is 0-100℃.
[0036] In some of the embodiments, the front indium-containing TCO seed layer is an ITO film, a VTTO film, a SCOT film, an IWO film, an ICO film or an IMO film;
[0037] And / or, the thickness of the front indium-containing TCO seed layer is 5 nm to 50 nm.
[0038] In some embodiments, when a front indium-containing TCO seed layer is prepared on the N-type doped layer using a PVD device, and a front indium-free TCO film is prepared on the front indium-containing TCO seed layer, the power density is 2KW / m 2 ~8KW / m 2 The process gases are Ar / O2 and Ar / H2 or H2O, among which Ar / O2 is a necessary process gas and the rest are non-essential process gases. The process pressure is 0.3Pa~0.8Pa and the process temperature is 0-100℃.
[0039] In some of the embodiments, the thickness of the front indium-free TCO film is 40 nm to 100 nm;
[0040] And / or, the front indium-free TCO film is a SnO2 film, a ZnO film, an AZO film, a GZO film or a GAZO film.
[0041] In some embodiments, preparing the back electrode on the back indium-free TCO film and preparing the front electrode on the front indium-free TCO film are independently selected from one or more of the following methods:
[0042] (1) preparing the back electrode or the front electrode by screen printing or laser transfer of one or more of low-temperature silver paste, low-temperature copper paste and silver-coated copper paste;
[0043] (2) The back electrode or the front electrode is prepared by forming a patterned metal grid line by electroplating one or more alloys of Al, Ti, Ni, Co, Ag, Cu and Sn.
[0044] An embodiment of the present application also provides a heterojunction solar cell.
[0045] A heterojunction solar cell is prepared by adopting the preparation method.
[0046] The above-mentioned preparation method of heterojunction solar cells can reduce the coating thickness of RPD equipment, shorten its PM cycle, and improve its production capacity. At the same time, the combination of indium-free materials can further reduce the TCO film cost of heterojunction solar cells, maximize the battery conversion efficiency, and facilitate industrial development. This application can effectively increase the normal operation time and effective operation time of RPD and PVD combined equipment, increase the effective production capacity of the equipment, reduce the TCO film manufacturing cost and raw material cost, maximize the technical advantages of the coating of the RPD equipment itself, ensure the battery efficiency, reduce the manufacturing cost of heterojunction solar cells, and facilitate its large-scale manufacturing production. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0048] In order to more completely understand the present application and its beneficial effects, the following description will be made in conjunction with the accompanying drawings. In the following description, the same reference numerals represent the same parts.
[0049] Figure 1 A schematic diagram of a method for preparing a heterojunction solar cell according to an embodiment of the present invention;
[0050] Figure 2 A schematic diagram of the structure of a heterojunction solar cell prepared by the method for preparing a heterojunction solar cell according to an embodiment of the present invention.
[0051] Description of Reference Numerals
[0052] 10. Heterojunction solar cell; 100. Silicon substrate; 201, 202. Intrinsic amorphous silicon layer; 301. N-type doped layer; 302. P-type doped layer; 401. Front indium-containing TCO seed layer; 501. Front indium-free TCO film; 402. Back indium-containing TCO seed layer; 502. Back indium-free TCO film; 601. Front electrode; 602. Back electrode. DETAILED DESCRIPTION
[0053] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0054] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0055] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0056] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0057] In the description of the present invention, "several" means more than one, "many" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number itself, and "above", "below", "within", etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing the technical features, and cannot be understood as indicating or implying the relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0058] In this article, unless otherwise stated, each reaction step may be carried out in the order described herein or may not be carried out in the order described herein. For example, other steps may be included between each reaction step, and the order of the reaction steps may also be appropriately swapped. This can be determined by the technician based on common knowledge and experience. Preferably, the reaction method herein is carried out sequentially.
[0059] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0060] The embodiment of the present application provides a method for preparing a heterojunction solar cell 10 to solve the problem in the traditional technology that, when preparing heterojunction solar cells, the RPD equipment has too low production capacity, and the RPD equipment itself is prone to generate dust during the process, resulting in a short PM cycle, which greatly shortens the overall equipment utilization rate. At the same time, the target material required for RPD coating is much more expensive than the PVD target material, and the RPD equipment target material utilization rate is low, resulting in a high cost of heterojunction solar cells prepared by the combination of RPD and PVD, which is not conducive to industrial development. The preparation method of the heterojunction solar cell 10 will be described below in conjunction with the accompanying drawings.
[0061] The method for preparing the heterojunction solar cell 10 provided in the embodiment of the present application is exemplary, see Figure 1 As shown, Figure 1 A schematic diagram of the process flow of the method for preparing the heterojunction solar cell 10 provided in the embodiment of the present application. The method for preparing the heterojunction solar cell 10 of the present application can reduce the production cost of the cell, achieve cost reduction and efficiency improvement, and facilitate industrial development.
[0062] In order to more clearly illustrate the structure of the method for preparing the heterojunction solar cell 10 , the method for preparing the heterojunction solar cell 10 will be introduced below with reference to the accompanying drawings.
[0063] For example, see Figure 1 As shown, Figure 1 A schematic diagram of the process flow of a method for preparing a heterojunction solar cell 10 provided in an embodiment of the present application.
[0064] A method for preparing a heterojunction solar cell 10 comprises the following steps:
[0065] (1) The silicon substrate 101 is cleaned and textured.
[0066] (2) Intrinsic amorphous silicon layers 201 and 202 are respectively prepared on two surfaces of the silicon substrate 101 .
[0067] (3) An N-type doped layer 301 is formed on the front intrinsic amorphous silicon layer 201 of the silicon substrate 101 .
[0068] (4) A P-type doped layer 302 is prepared on the intrinsic amorphous silicon layer 202 on the back side of the silicon substrate 101 .
[0069] (5) A back-side indium-containing TCO seed layer 402 is prepared on the P-type doped layer 302 using an RPD (Reactive Plasma Deposition) device, and a back-side indium-free TCO film 502 is prepared on the back-side indium-containing TCO seed layer 402 using a PVD (Physical Vapour Deposition) device.
[0070] (5) A front indium-containing TCO seed layer 401 is prepared on the N-type doped layer 301 by using a PVD device, and a front indium-free TCO film 501 is prepared on the front indium-containing TCO seed layer 401 .
[0071] (7) A back electrode 602 is prepared on the back indium-free TCO film 502 , and a front electrode 601 is prepared on the front indium-free TCO film 501 .
[0072] In the present application, a TCO film is deposited on the front side of the silicon substrate 101 using conventional PVD equipment, and the front TCO film adopts a combination of a front indium-containing TCO seed layer 401 and a front indium-free TCO film 501. The front side is deposited with a PVD device on the front side. The front indium-containing TCO seed layer 401 is mainly matched with the p-side doped semiconductor, and the front indium-free TCO film 501 is mainly to reduce the overall TCO cost.
[0073] The back side first uses the RPD device to deposit a thin back side indium-containing TCO seed layer 402, and then uses the PVD device to deposit the back side indium-free TCO film 502. The back side RPD device and the PVD device chamber are connected, that is, after the RPD coating, there is no need to break the vacuum, and it directly enters the PVD chamber for subsequent coating. The back side indium-containing TCO seed layer 402 is first formed by using the RPD. On the one hand, the deposited film has good density and no ion damage to the back side passivation structure. On the other hand, the indium-containing seed layer can have a better band gap and work function match with the P-type doped conductive layer, and can also promote the crystallization of the back side indium-free TCO film 502, improve the carrier mobility of the back side indium-free TCO film 502, and improve its electrical properties. Since the RPD only deposits the back side indium-containing TCO seed layer 402, it can effectively increase the RPD equipment capacity, increase its utilization rate, and reduce its PM cycle, while reducing the use of expensive RPD targets and reducing processing costs.
[0074] In the present application, Physical Vapor Deposition (PVD) works as follows: in a vacuum environment, through the combined action of voltage and magnetic field, the target material is bombarded with ionized inert gas ions, causing the target material to be ejected in the form of ions, atoms or molecules and deposited on the substrate to form a thin film.
[0075] Reactive Plasma Deposition (RPD) is a reactive plasma deposition (RPD) device that is mainly composed of a vacuum chamber, a hollow cathode ion gun, an ion beam controller, a magnetically focused cold water crucible (source placement area), a flow controller system, a static suspended workpiece rack, a cooling water system, and other parts. Its working principle is as follows: (1) After the vacuum chamber is evacuated to the background vacuum, Ar gas is introduced into the tantalum tube of the cathode plasma gun. After the plasma power is turned on, an arc discharge is first generated in the tantalum tube. After the Ar in the tube is ionized, the Ar + The tantalum tube is bombarded by the hollow cathode effect. + The bombardment causes rapid heating, emitting high-density plasma dominated by hot electrons, and the gas discharge mode is arc discharge. (2) Ar + When the plasma reaches the vacuum chamber, it is bent and focused downward due to the action of the magnetic poles and electromagnetic coils near the crucible, and is incident on the evaporation source material in the anode crucible. The kinetic energy of the Ar plasma is converted into thermal energy, heating and evaporating the solid evaporation source material. (3) The evaporation source interacts with the plasma above the crucible during its movement toward the target substrate, resulting in partial ionization, which greatly enhances the chemical activity of the evaporated material. In particular, a few centimeters above the crucible, the upward-moving evaporation source and the downward-moving Ar plasma interact strongly, forming a strong plasma region.
[0076] In some embodiments, the silicon substrate 101 is an N-type single crystal silicon wafer, the thickness of the silicon substrate 101 is 60 μm to 180 μm, and the resistivity of the silicon substrate 101 is 0.2 Ω.cm to 5 Ω.cm.
[0077] In some embodiments, the cleaning and texturing process for the silicon substrate 101 includes the following steps:
[0078] The silicon substrate 101 is treated with a high-temperature tubular phosphorus diffusion or chain-type gettering equipment, the main purpose of which is to remove metal ion impurities in the silicon wafer and improve the quality of the silicon substrate 101. The square resistance of the silicon substrate 101 after gettering is 20Ω / □ to 40Ω / □. Then, a tank-type wet acid solution is used to remove the PSG (boron-doped silicon oxide) layer on the surface of the silicon substrate 101 after gettering, and an alkaline solution is used to texture the surface of the silicon substrate 101, so that both sides of the silicon substrate 101 have a pyramid-shaped surface light trapping structure, and the silicon substrate 101 is cleaned to remove the surface oxide layer.
[0079] In some of the embodiments, the cleaning of the silicon substrate 101 includes the following steps: performing RCA cleaning (or a solution formulation equivalent to RCA cleaning) on the silicon substrate 101, then using HF (hydrofluoric acid) solution to clean the silicon substrate 101 to remove the surface oxide layer, and finally cleaning with deionized water and drying the surface.
[0080] In some embodiments, when the intrinsic amorphous silicon layers 201 and 202 are respectively prepared on two surfaces of the silicon substrate 101, the following steps are specifically included:
[0081] The intrinsic amorphous silicon layers 201 and 202 are deposited by a radio frequency plasma enhanced chemical vapor deposition system (Radio Frequency Plasma Enhanced Chemical Vapor Deposition; RF-PECVD); wherein, in the RF-PECVD process, the equipment power supply adopts 13.56 MHz, 26 MHz or 40 MHz, preferably 13.56 MHz, the process gas comprises one or more of SiH4, H2, CO2, CH4, N2O, the deposition temperature is 160°C to 220°C, and the deposition pressure is 0.2 mbar to 2 mbar.
[0082] In some embodiments, the thickness of the intrinsic amorphous silicon layers 201 and 202 is 2 nm to 10 nm.
[0083] In some embodiments, the N-type doped layer 301 is an N-type doped amorphous silicon layer, a nanocrystalline silicon layer, or a microcrystalline silicon layer.
[0084] In some embodiments, the thickness of the N-type doped layer 301 is 5 nm to 20 nm. It should be noted that the above and subsequent thicknesses refer to the thickness of the film layer tested on the polished wafer substrate.
[0085] In some embodiments, the N-type doping layer 301 is prepared on the front intrinsic amorphous silicon layer 201 of the silicon substrate 101, including the following steps:
[0086] An N-type doped layer 301 is deposited on the front intrinsic amorphous silicon layer 201 of the silicon substrate 101 by an RF-CVD (Radio Frequency Physical Vapour Deposition) device or a VHF-CVD (Very High Frequency Physical Vapour Deposition) device; the power supply of the RF-CVD device or the VHF-CVD device adopts 13.56MHz~40MHz, for example, 13.56MHz, 26MHz or 40MHz, etc., wherein the RF-CVD device preferably adopts 13.56MHz, the VHF-CVD device preferably adopts 40MHZ, and the process gas of the RF-CVD device or the VHF-CVD device includes one or more of SiH4, H2, CO2, CH4, N2O, PH3; the deposition temperature is 160℃~200℃, and the deposition pressure is 0.5mbar~5mbar.
[0087] In some embodiments, the P-type doped layer 302 is a P-type doped amorphous silicon layer, a nanocrystalline silicon layer, or a microcrystalline silicon layer.
[0088] In some embodiments, the thickness of the P-type doped layer 302 is 5 nm to 30 nm.
[0089] In some embodiments, the preparation of the P-type doped layer 302 on the back intrinsic amorphous silicon layer 202 of the silicon substrate 101 includes the following steps:
[0090] A P-type doping layer 302 is deposited on the intrinsic amorphous silicon layer 202 on the back side of the silicon substrate 101 by an RF-CVD device or a VHF-CVD device; the power supply of the RF-CVD device or the VHF-CVD device adopts 13.56MHz to 40MHz, such as 13.56MHz, 26MHz or 40MHz, etc., wherein the RF-CVD device preferably adopts 13.56MHz, and the VHF-CVD device preferably adopts 40MHZ. The process gas of the RF-CVD device or the VHF-CVD device includes one or more of SiH4, H2, CO2, CH4, N2O, B2H6, TMB (trimethylboron, chemical formula C3H9B), the deposition temperature is 160℃ to 200℃, and the deposition pressure is 0.5mbar to 5mbar.
[0091] In some of the embodiments, the back indium-containing TCO seed layer 402 is an ITO (tin-doped indium oxide) film, a VTTO film, a SCOT (zirconium-titanium-calcium-doped indium oxide) film, an IWO (tungsten-doped indium oxide) film, an ICO (cerium-doped indium oxide) film or an IMO (molybdenum-doped indium oxide) film.
[0092] In some embodiments, the back side Indium-containing TCO seed layer 402 has a thickness of 1 nm to 20 nm.
[0093] In some of the embodiments, when the RPD equipment is used to prepare the back indium-containing TCO seed layer 402 on the P-type doped layer 302, the process temperature is 0-200°C, the process pressure is 0.3Pa-0.8Pa, and the process gas is Ar / O2 and Ar / H2 or H2O, wherein Ar / O2 is a necessary process gas and the rest are non-necessary process gases.
[0094] In some embodiments, the thickness of the back-side indium-free TCO film 502 is 80 nm to 120 nm.
[0095] In some of the embodiments, the back-side indium-free TCO film 502 is a SnO2 (tin oxide) film, a ZnO (zinc oxide) film, an AZO (aluminum-doped zinc oxide) film, a GZO (gallium-doped zinc oxide) film or a GAZO (aluminum-gallium co-doped zinc oxide) film.
[0096] In some embodiments, when a back-side indium-free TCO film 502 is prepared on a back-side indium-containing TCO seed layer 402 using a magnetron sputtering device PVD device, the power density is 2KW / m 2 ~8KW / m 2 The process gases are Ar / O2 and Ar / H2 or H2O, among which Ar / O2 is a necessary process gas and the rest are non-essential process gases. The process pressure is 0.3Pa~0.8Pa and the process temperature is 0-100℃.
[0097] In some of the embodiments, the front indium-containing TCO seed layer 401 is an ITO film, a VTTO film, a SCOT film, an IWO film, an ICO film or an IMO film.
[0098] In some of the embodiments, the thickness of the front-side Indium-containing TCO seed layer 401 is 5 nm to 50 nm.
[0099] In some embodiments, when a PVD device is used to prepare a front indium-containing TCO seed layer 401 on the N-type doped layer 301, and a front indium-free TCO film 501 is prepared on the front indium-containing TCO seed layer 401, the power density is 2KW / m 2 ~8KW / m 2 The process gases are Ar / O2 and Ar / H2 or H2O, among which Ar / O2 is a necessary process gas and the rest are non-essential process gases. The process pressure is 0.3Pa~0.8Pa and the process temperature is 0-100℃.
[0100] In some of the embodiments, the thickness of the front-side indium-free TCO film 501 is 40 nm to 100 nm.
[0101] In some of the embodiments, the front-side indium-free TCO film 501 is a SnO2 film, a ZnO film, an AZO film, a GZO film or a GAZO film.
[0102] In some embodiments, the preparation of the back electrode 602 on the back indium-free TCO film 502 and the preparation of the front electrode 601 on the front indium-free TCO film 501 are independently selected from one or more of the following methods:
[0103] (1) preparing the back electrode 602 or the front electrode 601 by screen printing or laser transfer of one or more of low-temperature silver paste, low-temperature copper paste and silver-coated copper paste;
[0104] (2) A patterned metal grid line is formed by electroplating one or more alloys of Al, Ti, Ni, Co, Ag, Cu and Sn to prepare the back electrode 602 or the front electrode 601.
[0105] An embodiment of the present application further provides a heterojunction solar cell 10 .
[0106] A heterojunction solar cell 10 is prepared by the above-mentioned preparation method. Figure 2 As shown, Figure 2 This is a schematic structural diagram of a heterojunction solar cell 10 provided in an embodiment of the present application. The heterojunction solar cell 10 includes a silicon substrate 101, and the front side of the silicon substrate 101 is sequentially stacked with an intrinsic amorphous silicon layer 201, an N-type doped layer 301, a front indium-containing TCO seed layer 401, a front indium-free TCO film 501, and a front electrode 601, and the back side of the silicon substrate 101 is sequentially stacked with an intrinsic amorphous silicon layer 202, a P-type doped layer 302, a back indium-containing TCO seed layer 402, a back indium-free TCO film 502, and a back electrode 602.
[0107] Example 1
[0108] This embodiment provides a heterojunction solar cell 10. The heterojunction solar cell 10 is prepared by the following preparation method.
[0109] A method for preparing a heterojunction solar cell 10 comprises the following steps:
[0110] (1) An N-type single crystal silicon wafer is used as the silicon substrate 101 . The thickness of the silicon substrate 101 is 100 μm, and the resistivity of the silicon substrate 101 is 1 Ω.cm.
[0111] The silicon substrate 101 is cleaned and textured, and a chain-type doping device is used to dope the silicon substrate 101. After doping, the square resistance of the silicon substrate 101 is 30Ω / □. Then, a tank-type wet acid solution is used to remove the PSG layer on the surface of the silicon substrate 101 after doping, and an alkaline solution is used to texture the surface of the silicon substrate 101, so that both sides of the silicon substrate 101 have a pyramid-shaped surface light trapping structure.
[0112] After the silicon substrate 101 is subjected to RCA cleaning (or a solution formula equivalent to RCA cleaning), the silicon substrate 101 is cleaned with HF solution to remove the surface oxide layer, and finally cleaned with deionized water and the surface is dried.
[0113] (2) Intrinsic amorphous silicon layers 201 and 202 are respectively prepared on two surfaces of the silicon substrate 101 by RF-PECVD process. In the RF-PECVD process, the power supply of the equipment is 13.56 MHz, the process gas contains SiH4, the deposition temperature is 180°C, the deposition pressure is 1 mbar, and the thickness of the intrinsic amorphous silicon layers 201 and 202 is 8 nm.
[0114] (3) Depositing an N-type doped layer 301 on the front intrinsic amorphous silicon layer 201 of the silicon substrate 101 by RF-CVD equipment, wherein the N-type doped layer 301 is an N-type doped amorphous silicon layer. The power supply of the RF-CVD equipment is 13.56 MHz, the process gas includes SiH4, the deposition temperature is 180° C., the deposition pressure is 1 mbar, and the deposition thickness of the N-type doped layer 301 is 10 nm.
[0115] (4) A P-type doped layer 302 is deposited on the intrinsic amorphous silicon layer 202 on the back side of the silicon substrate 101 by using an RF-CVD device. The P-type doped layer 302 is a P-type doped amorphous silicon layer. The power supply of the RF-CVD device is 13.56 MH. The process gas of the RF-CVD device includes SiH4 and TMB, the deposition temperature is 180° C., the deposition pressure is 1 mbar, and the thickness of the P-type doped layer 302 is 20 nm.
[0116] (5) An ITO film is prepared on the P-type doped layer 302 by using an RPD device as the back indium-containing TCO seed layer 402. The thickness of the back indium-containing TCO seed layer 402 is 5 nm. During deposition, the process temperature is 100°C, the process pressure is 0.5 Pa, and the process gases are Ar / O2 and Ar / H2. A SnO2 film is prepared on the back indium-containing TCO seed layer 402 by using a magnetron sputtering device PVD device as the back indium-free TCO film 502. The thickness of the back indium-free TCO film 502 is 100 nm. During deposition, the power density is 5 KW / m 2 The process gases are Ar / O2 and Ar / H2, the process pressure is 0.5Pa, and the process temperature is 60℃.
[0117] (6) Using PVD equipment, an ITO film is prepared on the N-type doped layer 301 as the front indium-containing TCO seed layer 401, and the thickness of the front indium-containing TCO seed layer 401 is 10 nm; and a SnO2 film is prepared on the front indium-containing TCO seed layer 401 as the front indium-free TCO film 501, and the thickness of the front indium-free TCO film 501 is 80 nm. During the deposition of the PVD equipment, the power density is 5 KW / m 2 The process gases are Ar / O2 and Ar / H2, the process pressure is 0.5Pa, and the process temperature is 60℃.
[0118] (7) A back electrode 602 is prepared on the back indium-free TCO film 502 by screen printing a low-temperature silver paste, and a front electrode 601 is prepared on the front indium-free TCO film 501 .
[0119] Example 2
[0120] This embodiment provides a heterojunction solar cell 10. The heterojunction solar cell 10 is prepared by the following preparation method.
[0121] A method for preparing a heterojunction solar cell 10 comprises the following steps:
[0122] (1) An N-type single crystal silicon wafer is used as the silicon substrate 101 . The thickness of the silicon substrate 101 is 180 μm, and the resistivity of the silicon substrate 101 is 5 Ω.cm.
[0123] The silicon substrate 101 is cleaned and textured, and the silicon substrate 101 is treated with gettering by high-temperature tubular phosphorus diffusion. After gettering, the square resistance of the silicon substrate 101 is 40Ω / □. Then, a tank-type wet acid solution is used to remove the PSG layer on the surface of the silicon substrate 101 after gettering, and the surface of the silicon substrate 101 is textured by an alkaline solution, so that both sides of the silicon substrate 101 have a pyramid-shaped surface light trapping structure.
[0124] After the silicon substrate 101 is cleaned by RCA, the silicon substrate 101 is cleaned by HF solution to remove the surface oxide layer, and finally cleaned by deionized water and the surface is dried.
[0125] (2) Intrinsic amorphous silicon layers 201 and 202 are respectively prepared on two surfaces of the silicon substrate 101 by RF-PECVD process. In the RF-PECVD process, the power supply of the equipment is 13.56 MHz, the process gas includes SiH4 and H2, the deposition temperature is 200° C., the deposition pressure is 2 mbar, and the thickness of the intrinsic amorphous silicon layers 201 and 202 is 10 nm.
[0126] (3) Depositing an N-type doped layer 301 on the front intrinsic amorphous silicon layer 201 of the silicon substrate 101 by a VHF-CVD device, wherein the N-type doped layer 301 is an N-type doped microcrystalline silicon layer. The power supply of the VHF-CVD device is 40 MHZ, and the process gas of the VHF-CVD device includes SiH4 and H2; the deposition temperature is 200° C., the deposition pressure is 5 mbar, and the deposition thickness of the N-type doped layer 301 is 20 nm.
[0127] (4) A P-type doped layer 302 is deposited on the intrinsic amorphous silicon layer 202 on the back side of the silicon substrate 101 by a VHF-CVD device. The P-type doped layer 302 is a P-type doped microcrystalline silicon layer. The power supply of the VHF-CVD device is 40 MHZ. The process gas of the VHF-CVD device includes SiH4, H2, and TMB. The deposition temperature is 200° C., the deposition pressure is 5 mbar, and the thickness of the P-type doped layer 302 is 30 nm.
[0128] (5) An ITO film is prepared on the P-type doped layer 302 by using an RPD device as the back indium-containing TCO seed layer 402. The thickness of the back indium-containing TCO seed layer 402 is 20 nm. During deposition, the process temperature is 200°C, the process pressure is 0.8 Pa, and the process gases are Ar / O2 and Ar / H2. A SnO2 film is prepared on the back indium-containing TCO seed layer 402 by using a magnetron sputtering device PVD device as the back indium-free TCO film 502. The thickness of the back indium-free TCO film 502 is 120 nm. During deposition, the power density is 8 KW / m 2 The process gases are Ar / O2 and Ar / H, the process pressure is 0.8Pa, and the process temperature is 100℃.
[0129] (6) Using PVD equipment, an ITO film is prepared on the N-type doped layer 301 as the front indium-containing TCO seed layer 401, and the thickness of the front indium-containing TCO seed layer 401 is 50nm; and a SnO2 film is prepared on the front indium-containing TCO seed layer 401 as the front indium-free TCO film 501, and the thickness of the front indium-free TCO film 501 is 100nm. During the deposition of the PVD equipment, the power density is 8KW / m 2 The process gases are Ar / O2 and Ar / H2, the process pressure is 0.8Pa, and the process temperature is 100℃.
[0130] (7) A back electrode 602 is prepared on the back indium-free TCO film 502 by laser transfer of silver-coated copper paste, and a front electrode 601 is prepared on the front indium-free TCO film 501.
[0131] The performance test was performed on the heterojunction solar cell 10 in Examples 1 and 2. The test results are shown in Table 1. As can be seen from Table 1, various performance parameters of the heterojunction solar cell 10 in Examples 1 and 2 of the present application meet the requirements.
[0132] Table 1
[0133]
[0134] In summary, the preparation method of the above-mentioned heterojunction solar cell 10 can reduce the coating thickness of the RPD device, shorten its PM cycle, and improve its production capacity. At the same time, the combination of indium-free materials can further reduce the TCO film cost of the heterojunction solar cell, maximize the battery conversion efficiency, and facilitate industrial development. The present application can effectively increase the normal operation time and effective operation time of the RPD and PVD combined equipment, increase the effective production capacity of the equipment, reduce the TCO film manufacturing cost and raw material cost, maximize the technical advantages of the RPD equipment's own coating, ensure battery efficiency, reduce the manufacturing cost of heterojunction solar cells, and facilitate its large-scale manufacturing production.
[0135] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0136] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0137] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a heterojunction solar cell, characterized in that: The steps include: Cleaning and texturing the silicon substrate; Intrinsic amorphous silicon layers are respectively prepared on two surfaces of a silicon substrate; Preparing an N-type doped layer on the front intrinsic amorphous silicon layer of the silicon substrate; Preparing a P-type doped layer on the back intrinsic amorphous silicon layer of the silicon substrate; A back indium-containing TCO seed layer is prepared on the P-type doped layer using an RPD device, and a back indium-free TCO film is prepared on the back indium-containing TCO seed layer using a PVD device; wherein the back indium-containing TCO seed layer has a thickness of 1 nm to 20 nm, and the back indium-free TCO film has a thickness of 80 nm to 120 nm; Preparing a front indium-containing TCO seed layer on the N-type doped layer using a PVD device, and preparing a front indium-free TCO film on the front indium-containing TCO seed layer; and A back electrode is prepared on the back indium-free TCO film, and a front electrode is prepared on the front indium-free TCO film.
2. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: The silicon substrate is an N-type single crystal silicon wafer, the thickness of the silicon substrate is 60 μm to 180 μm, and the resistivity is 0.2 Ω.cm to 5 Ω.cm.
3. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: When cleaning and texturing the silicon substrate, the following steps are included: The silicon substrate is treated with gettering equipment using a high-temperature tubular phosphorus diffusion or chain gettering equipment. The square resistance of the silicon substrate after gettering is 20Ω / □~40Ω / □; A trough-type wet acid solution is used to remove the PSG layer on the surface of the silicon substrate after doping, and an alkaline solution is used to texture the surface of the silicon substrate so that both sides of the silicon substrate have a pyramid-shaped surface light-trapping structure. The silicon substrate is cleaned to remove the surface oxide layer.
4. The method for preparing a heterojunction solar cell according to claim 2, characterized in that: When cleaning the silicon substrate, the following steps are included: after performing RCA cleaning on the silicon substrate, the silicon substrate is cleaned with HF solution to remove the surface oxide layer, and finally the silicon substrate is cleaned with deionized water and the surface is dried.
5. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: When the intrinsic amorphous silicon layers are prepared on two surfaces of the silicon substrate respectively, the steps specifically include: The intrinsic amorphous silicon layer is deposited by RF-PECVD; wherein, the equipment power supply in the RF-PECVD process adopts 13.56MHz, 26MHz or 40MHz, the process gas contains one or more of SiH4, H2, CO2, CH4, N2O, the deposition temperature is 160℃~220℃, and the deposition pressure is 0.2mbar~2mbar.
6. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: The thickness of the intrinsic amorphous silicon layer is 2nm-10nm.
7. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: The N-type doped layer is an N-type doped amorphous silicon layer, a nanocrystalline silicon layer, or a microcrystalline silicon layer; And / or, the thickness of the N-type doping layer is 5 nm to 20 nm.
8. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: When an N-type doping layer is prepared on the front intrinsic amorphous silicon layer of a silicon substrate, the following steps are included: An N-type doped layer is deposited on the front intrinsic amorphous silicon layer of a silicon substrate by using an RF-CVD device or a VHF-CVD device; wherein the power supply of the RF-CVD device or the VHF-CVD device adopts 13.56MHz to 40MHz, and the process gas contains one or more of SiH4, H2, CO2, CH4, N2O, and PH3; the deposition temperature is 160°C to 200°C, and the deposition pressure is 0.5mbar to 5mbar.
9. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: The P-type doped layer is a P-type doped amorphous silicon layer, a nanocrystalline silicon layer, or a microcrystalline silicon layer; And / or, the thickness of the P-type doping layer is 5 nm to 30 nm.
10. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: When preparing a p-type doped layer on the intrinsic amorphous silicon layer on the back side of a silicon substrate, the method includes the following steps: depositing a p-type doped layer on the intrinsic amorphous silicon layer on the back side of a silicon substrate by using an RF-CVD device or a VHF-CVD device; wherein the power supply of the RF-CVD device or the VHF-CVD device adopts 13.56MHz to 40MHz, the process gas comprises one or more of SiH4, H2, CO2, CH4, N2O, B2H6, and TMB, the deposition temperature is 160°C to 200°C, and the deposition pressure is 0.5mbar to 5mbar.
11. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: The back indium-containing TCO seed layer is an ITO film, a VTTO film, a SCOT film, an IWO film, an ICO film or an IMO film.
12. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: When the RPD equipment is used to prepare the back indium-containing TCO seed layer on the P-type doped layer, the process temperature is 0-200°C, the process pressure is 0.3Pa-0.8Pa, and the process gas is a mixed gas of Ar and O2, a mixed gas of Ar and H2, or a mixed gas of Ar and H2O, wherein the mixed gas of Ar and O2 is a necessary process gas, and the rest are non-essential process gases.
13. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: The back indium-free TCO film is a SnO2 film, a ZnO film, an AZO film, a GZO film or a GAZO film.
14. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: When a back-side indium-free TCO film is prepared on the back-side indium-containing TCO seed layer using a magnetron sputtering device PVD device, the power density is 2KW / m 2 ~8KW / m 2 The process gas is a mixture of Ar and O2, a mixture of Ar and H2, or a mixture of Ar and H2O, wherein the mixture of Ar and O2 is a necessary process gas, and the rest are non-essential process gases. The process pressure is 0.3Pa~0.8Pa, and the process temperature is 0-100℃.
15. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: The front indium-containing TCO seed layer is an ITO film, a VTTO film, a SCOT film, an IWO film, an ICO film or an IMO film; And / or, the thickness of the front indium-containing TCO seed layer is 5 nm to 50 nm.
16. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: When a front indium-containing TCO seed layer is prepared on the N-type doped layer using a PVD device, and a front indium-free TCO film is prepared on the front indium-containing TCO seed layer, the power density is 2KW / m 2 ~8KW / m 2 The process gas is a mixture of Ar and O2, a mixture of Ar and H2, or a mixture of Ar and H2O, wherein the mixture of Ar and O2 is a necessary process gas, and the rest are non-essential process gases. The process pressure is 0.3Pa~0.8Pa, and the process temperature is 0-100℃.
17. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: The thickness of the front indium-free TCO film is 40nm to 100nm; And / or, the front indium-free TCO film is a SnO2 film, a ZnO film, an AZO film, a GZO film or a GAZO film.
18. The method for preparing a heterojunction solar cell according to any one of claims 1 to 6, characterized in that: The preparation of the back electrode on the back indium-free TCO film and the preparation of the front electrode on the front indium-free TCO film are independently selected from one or more of the following methods: (1) preparing the back electrode or the front electrode by screen printing or laser transfer of one or more of low-temperature silver paste, low-temperature copper paste and silver-coated copper paste; (2) The back electrode or the front electrode is prepared by forming a patterned metal grid line by electroplating one or more alloys of Al, Ti, Ni, Co, Ag, Cu and Sn.
19. A heterojunction solar cell, characterized in that: The preparation method is described in any one of claims 1 to 18.