A method for preparing a magnetically separable cubic Fe2O3 / ZnO composite oxide adsorbent
By using iron and zinc salts to prepare Fe2O3/ZnO composite oxide adsorbent at room temperature, the problems of preparation complexity and high cost in the existing technology are solved, and efficient adsorption and magnetic separation are achieved to recover tetracycline in water, which is suitable for industry Production.
Patent Information
- Application Number
- CN202311380295.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-10-24
AI Technical Summary
The preparation methods of existing composite oxide adsorbents are complex, difficult to repeat, and costly, which limits their application in large-scale industrial production and makes it difficult to efficiently remove antibiotic residues in water, especially tetracyclines.
Iron and zinc salts are used as iron and zinc sources, the Prussian blue precursor is prepared through hydrothermal reaction, and the Fe2O3/ZnO composite oxide adsorbent is obtained by sintering at high temperature. The process is simple, the energy consumption is low, and it is suitable for operation at room temperature.
The obtained Fe2O3/ZnO composite oxide adsorbent has a high saturation adsorption capacity, can efficiently adsorb tetracycline in water, and can be magnetically separated and recycled, which solves the problems of preparation complexity and high cost in the existing technology.
Smart Images

Figure CN117427598B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic functional materials, and in particular relates to a preparation method and application of a Fe2O3 / ZnO composite oxide adsorbent. Background Art
[0002] The use of antibiotics has made many diseases curable, but it has also caused serious environmental problems. In recent years, the overuse of antibiotics has led to the emergence of many antibiotic-resistant bacteria. Most antibiotics ingested by humans and animals are not absorbed, but are discharged into the environment, resulting in the widespread spread and proliferation of antibiotic resistance genes (ARGs) in the environment, which in turn endangers human health and causes environmental pollution. Although high temperature, light and other conditions can curb the spread of ARGs in various environments to a certain extent, there are secondary pollution and ecological risk problems. Taking tetracycline (TC), the world's second largest antibiotic, as an example, improper wastewater treatment has caused more serious secondary pollution. Therefore, it is of great significance to study how to efficiently and environmentally friendly treat difficult-to-degrade organic pollutants in wastewater.
[0003] Among the various methods for removing antibiotic residues from water, adsorption has attracted widespread attention from many researchers due to its high treatment efficiency, simple operation, low cost, and no secondary pollution. Therefore, it is very important to develop an efficient and environmentally friendly way to solve the problem of tetracycline residues in the environment.
[0004] Metal organic framework (MOF) material adsorbents have received extensive attention from scholars in recent years. As adsorbents, MOFs have the advantages of large porosity, high surface area, inherent functionality and versatility. As a new type of porous nanomaterials, MOFs have multifunctional "on-demand" characteristics and have broad application prospects in magnetic separation, sensing, adsorption and catalysis. Bimetallic composite oxides prepared from metal organic framework (MOF) precursors are environmentally friendly and have excellent adsorption properties, making them ideal adsorption materials. Compared with other bimetallic oxide functionalized biochar adsorption materials.
[0005] The search for new adsorption materials that are efficient, low-cost and easy to recycle has become a hot topic in the field of adsorption research in recent years. Although researchers have prepared some composite oxide adsorbents with different morphologies and studied their performance, the most important preparation method still has defects such as complexity, difficulty in repeatability and high cost, which limits its application in large-scale industrial production. Summary of the invention
[0006] In view of this, the present invention provides a preparation method and application of a Fe2O3 / ZnO composite oxide adsorbent, wherein the present invention uses iron and zinc salts as iron and zinc sources at room temperature, centrifuges, washes and dries the hydrothermal product to obtain a Prussian blue precursor, and then sintering at high temperature to obtain a Fe2O3 / ZnO composite oxide adsorbent. The method has the advantages of mild reaction conditions, simple process, low energy consumption and short time consumption; the nanomaterial prepared by the present invention can be used in the field of adsorbing water pollutants.
[0007] In order to solve the above technical problems, the present application discloses a method for preparing a Fe2O3 / ZnO composite oxide adsorbent, comprising the following steps:
[0008] Step 1, dissolve potassium ferrocyanide (K3[Fe(CN)6]) in water to prepare an iron salt solution, and add zinc cyanide to mix;
[0009] Step 2: After stirring for a period of time, the mixed solution is transferred to a polytetrafluoroethylene reactor and placed in an oven for hydrothermal reaction;
[0010] Step 3, centrifuging the product prepared in step 2, washing three times with deionized water, and drying to obtain a zinc iron Prussian blue precursor;
[0011] Step 4: The zinc-iron Prussian blue precursor prepared in step 3 is placed in a porcelain boat, calcined at high temperature in a tubular furnace with an Ar atmosphere, and cooled naturally to obtain a Fe2O3 / ZnO composite oxide adsorbent.
[0012] Furthermore, in step 1, the concentration of the potassium ferrocyanide solution is 0.08-1.00 mol / L;
[0013] Furthermore, in step 1, the molar ratio of potassium ferrocyanide to zinc cyanide is 1:1-1:3.
[0014] Furthermore, the stirring conditions in step 2 include a temperature of 25-30° C. and a rotation speed of 180-220 r / min.
[0015] Furthermore, the hydrothermal reaction temperature in step 2 is 140-200°C, and the reaction time is 2-12 h.
[0016] Furthermore, the calcination temperature in step 4 is 450-800°C, the calcination time is 1-5 h, and the heating rate is 1-5°C / min.
[0017] The invention also discloses a Fe2O3 / ZnO composite oxide adsorbent prepared by the above preparation method.
[0018] Compared with the prior art, the present invention can achieve the following technical effects:
[0019] (1) The present invention uses metal organic framework (MOF)-like Prussian blue cubic Zn2[Fe(CN)6]·3H2O as a precursor and obtains Fe2O3 / ZnO composite oxide adsorption by high temperature calcination.
[0020] (2) The Fe2O3 / ZnO composite oxide prepared by the present invention adsorbs tetracycline in water, and the saturated adsorption capacity is as high as 782 mg / g.
[0021] (3) The Fe2O3 / ZnO composite oxide adsorbent prepared by the present invention can be magnetically separated and recovered after adsorbing pollutants in water.
[0022] Of course, any product implementing the present invention does not necessarily need to achieve all of the above-mentioned technical effects at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0024] Figure 1 This is a SEM photograph of cubic Zn2[Fe(CN)6]·3H2O prepared in Example 1 of the present invention;
[0025] Figure 2 This is the XRD spectrum of cubic Zn2[Fe(CN)6]·3H2O prepared in Example 1 of the present invention;
[0026] Figure 3 The SEM photos of cubic Fe2O3 / ZnO composite oxides obtained by calcining the precursor cubic Zn2[Fe(CN)6]·3H2O prepared in Example 1 of the present invention at different temperatures;
[0027] Figure 4 This is the XRD spectrum of the precursor cubic Zn2[Fe(CN)6]·3H2O prepared in Example 1 of the present invention, which is formed into zinc-iron composite oxide after being calcined at different temperatures;
[0028] Figure 5 is a graph showing the variation of the adsorption amount of the Fe2O3 / ZnO composite oxide adsorbent prepared in Example 1 of the present invention over time;
[0029] Figure 6 This is a diagram showing the magnetic separation of the Fe2O3 / ZnO composite oxide adsorbent prepared in Example 1 of the present invention;
[0030] The molar ratio of potassium ferrocyanide to zinc cyanide is 1:1-1:3. DETAILED DESCRIPTION
[0031] The following will describe the implementation methods of the present invention in detail with reference to the embodiments, so that the implementation process of how the present invention applies technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.
[0032] The present application discloses a method for preparing a Fe2O3 / ZnO composite oxide adsorbent, comprising the following steps:
[0033] Step 1: Dissolve potassium ferrocyanide in water to prepare a 1.00 mol / L solution, add solid zinc cyanide, the molar ratio of potassium ferrocyanide to zinc cyanide is 1:2, and mix evenly at a stirring speed of 180-220 r / min.
[0034] Step 2: After stirring for a period of time, the mixed solution is transferred to a polytetrafluoroethylene reactor and placed in an oven for hydrothermal reaction. The hydrothermal reaction temperature is 140-200°C and the reaction time is 2-12 h.
[0035] Step 3: The product prepared in step 2 is separated by centrifugation, washed three times with deionized water, and dried to obtain a zinc iron Prussian blue precursor. The reaction temperature is 25-30°C.
[0036] Step 4: Place the zinc-iron Prussian blue precursor prepared in step 3 in a crucible, and calcine it in a tubular furnace with an Ar atmosphere at 450-800 °C at a heating rate of 1-5 °C / min for 1-5 hours, and obtain a Fe2O3 / ZnO composite oxide adsorbent after natural cooling.
[0037] In the preparation method, 1. The zinc source used is solid zinc cyanide instead of free zinc ions, and the iron source is potassium ferrocyanide instead of directly using potassium ferrocyanide, because if the precursor Zn2[Fe(CN)6]·3H2O obtained by the rapid reaction of zinc ions and ferrocyanate directly has poor adsorption performance after calcination.
[0038] 2. Zinc cyanide solid zinc source is selected because zinc cyanide has a low solubility in water. On the one hand, the concentration of zinc ions can be controlled, thereby controlling the generation rate of the precursor Zn2[Fe(CN)6]·3H2O particles; on the other hand, after zinc cyanide is dissolved in water, the cyanide generated has reducing and coordination capabilities.
[0039] 3. Under high temperature hydrothermal conditions, cyanide has reducing properties and acts as a reducing agent to reduce Fe 3+ Reduction to Fe 2+ In the presence of a large amount of cyanide with strong coordination ability, the final product is cubic Zn2[Fe(CN)6]·3H2O.
[0040] 4. In an inert atmosphere of argon (Ar), a cubic Fe2O3 / ZnO composite oxide adsorbent with excellent adsorption performance and magnetic separation is obtained after high-temperature calcination.
[0041] Example 1
[0042] Potassium ferrocyanide was dissolved in deionized water to obtain a 0.10 mol / L potassium ferrocyanide solution. Zinc cyanide was added to the potassium ferrocyanide solution under stirring conditions of 200 r / min and 25 °C. The molar ratio of potassium ferrocyanide to zinc cyanide was 1:1. The mixed solution was stirred for a period of time and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction. The hydrothermal temperature was 120 °C and the reaction time was 2h. The product was separated by centrifugation, washed three times with deionized water, and dried at 60 °C to obtain a zinc-iron Prussian blue precursor. The obtained Prussian blue precursor was placed in a porcelain boat and calcined for 2 h at 450 °C in a tubular furnace with an Ar atmosphere at a heating rate of 2 °C / min. After natural cooling, a Fe2O3 / ZnO composite oxide adsorbent was obtained. The scanning electron microscope photograph of the obtained product is shown in Figure 2. Figure 1 As shown in the figure, the original morphology can be maintained after high temperature calcination. The XRD spectrum is shown in Figure 2 As shown in the figure, each diffraction peak is consistent with the standard spectrum diffraction peak of Fe2O3 / ZnO composite oxide, and no other impurity peaks are found, indicating that the prepared magnetic separation Fe2O3 / ZnO composite oxide has a high purity. The SEM images of the zinc-iron composite oxide calcined at different temperatures are shown in the figure. Figure 3 As shown (where a is ZFO-450; b is ZFO-500; c is ZFO-520); XRD spectra are shown Figure 4 The adsorption performance of tetracycline by the prepared Fe2O3 / ZnO composite oxide adsorbent is shown in Figure 5 As shown in Figure 2, the adsorption capacity can reach 692 mg / g after 2 hours of adsorption in 200 ppm tetracycline wastewater.
[0043] Example 2
[0044] Potassium ferrocyanide was dissolved in deionized water to obtain a 0.50 mol / L potassium ferrocyanide solution. Zinc cyanide was added to the potassium ferrocyanide solution under stirring conditions of 200 r / min and 25 °C. The molar ratio of potassium ferrocyanide to zinc cyanide was 1:2. The mixed solution was stirred for a period of time and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction. The hydrothermal temperature was 140 °C and the reaction time was 2.5 h. The product was centrifuged, washed three times with deionized water, and dried at 70 °C to obtain a zinc-iron Prussian blue precursor. The obtained Prussian blue precursor was placed in a crucible and calcined for 1 h at 500 °C in a tubular furnace with an Ar atmosphere at a heating rate of 1 °C / min. After natural cooling, a Fe2O3 / ZnO composite oxide adsorbent was obtained. The performance of the prepared Fe2O3 / ZnO composite oxide adsorbent in adsorbing tetracycline is shown in the following figure. Figure 5 As shown. After 2 hours of adsorption in 200 ppm tetracycline wastewater, the adsorption capacity can reach 782 mg / g. Figure 6 For magnetically separable photos, under the action of magnetic force, the adsorbent can be effectively separated and recovered.
[0045] Example 3
[0046] Potassium ferrocyanide was dissolved in deionized water to obtain a 0.80 mol / L potassium ferrocyanide solution. Zinc cyanide was added to the potassium ferrocyanide solution under stirring conditions of 200 r / min and 30 ℃. The molar ratio of potassium ferrocyanide to zinc cyanide was 1:3. The mixed solution was stirred for a period of time and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction. The hydrothermal temperature was 180 ℃ and the reaction time was 3 h. The product was centrifuged, washed three times with deionized water, and dried at 80 ℃ to obtain a zinc-iron Prussian blue precursor. The obtained Prussian blue precursor was placed in a crucible and calcined for 3 h at 520 ℃ in a tubular furnace with an Ar atmosphere at a heating rate of 5 ℃ / min. After natural cooling, a Fe2O3 / ZnO composite oxide adsorbent was obtained. After adsorption in 200 ppm tetracycline wastewater for 2 hours, the adsorption capacity can reach 597 mg / g.
[0047] The above description shows and describes several preferred embodiments of the invention, but as mentioned above, it should be understood that the invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge of the relevant field. Changes and modifications made by those skilled in the art should be within the scope of protection of the claims attached to the invention without departing from the spirit and scope of the invention.
Claims
1. A method for preparing a magnetically separable cubic Fe2O3 / ZnO composite oxide adsorbent, characterized in that: The following steps are involved: Step 1, dissolve potassium ferrocyanide (K3[Fe(CN)6]) in water to prepare an iron salt solution, and add zinc cyanide to mix; Step 2, transferring the stirred mixed aqueous solution of potassium ferrocyanide and zinc cyanide into a polytetrafluoroethylene reactor, placing it in an oven for reaction, the temperature of the hydrothermal reaction is 140-200° C., and the reaction time is 2-12 h; Step 3, the product prepared in step 2 is centrifuged, washed three times with deionized water, and dried to obtain a zinc iron Prussian blue precursor; Step 4: Place the Prussian blue precursor prepared in step 3 in a porcelain boat, calcine it at high temperature in a tubular furnace with an Ar atmosphere, and obtain a cubic Fe2O3 / ZnO composite oxide adsorbent after natural cooling.
2. The method for preparing the magnetically separable cubic Fe2O3 / ZnO composite oxide adsorbent according to claim 1, characterized in that The concentration of potassium ferrocyanide solution is 0.08-1.00 mol / L.
3. The method for preparing a magnetically separable cubic Fe2O3 / ZnO composite oxide adsorbent according to claim 1, characterized in that: The molar ratio of potassium ferrocyanide to zinc cyanide is 1:1-1:
3.
4. The method for preparing a magnetically separable cubic Fe2O3 / ZnO composite oxide adsorbent according to claim 1, characterized in that: The stirring conditions in step 2 are a temperature of 25-30° C. and a rotation speed of 180-220 r / min.
5. The method for preparing a magnetically separable cubic Fe2O3 / ZnO composite oxide adsorbent according to claim 1, characterized in that: The calcination temperature in step 4 is 450-800°C, the calcination time is 1-5 h, and the heating rate is 1-5°C / min.
Citation Information
Patent Citations
Preparation method and application of magnetic porous Fe3O4 nanocube
CN112028128A
Dried persimmon-shaped magnetic separation LaFeO3 / CeO2 compound adsorbent and preparation method thereof
CN113856612A