A high-epoxidized macromolecular coupling agent, its preparation method and application

The use of high-epoxidation macromolecular coupling agents has solved the problems of pollution and high cost of silane coupling agents in the rubber industry, achieving pollution-free and low-cost rubber modification, improving the dispersibility and compatibility of silica in rubber, and enhancing the performance of rubber.

CN117430907BActive Publication Date: 2026-11-17BEIJING UNIV OF CHEM TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210854001.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-13
Publication Date
2026-11-17
Estimated Expiration
2042-07-13

AI Technical Summary

Technical Problem

Existing silane coupling agents in the rubber industry suffer from problems such as volatile organic compound emissions and high costs, and are difficult to effectively improve the dispersibility and compatibility of silica in rubber.

Method used

A high-epoxidation macromolecular coupling agent is used, which is formed by mixing and vulcanizing myrcene and glycidyl methacrylate copolymer with diacid compounds to form a powdered coupling agent. The dispersibility is improved by the reactivity of epoxy groups with the surface of silica, thus avoiding the use of traditional silane coupling agents.

Benefits of technology

It achieves pollution-free and low-cost rubber modification, improves the interfacial bonding strength between silica and rubber, enhances dispersibility and compatibility, reduces rolling resistance, and strengthens the rubber's anti-slip properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a high-epoxidation macromolecular coupling agent, its preparation method, and its application, relating to the field of rubber coupling agent technology. The coupling agent is prepared by mixing and vulcanizing raw materials comprising the following components: 100 parts by weight of a copolymer of myrcene and glycidyl methacrylate; and 5-80 parts by weight of a diacid compound. The coupling agent of this invention improves the dispersion of silica by constructing reaction sites on the rubber molecular chain segments through the reactivity of epoxy with silica. The high-epoxidation macromolecular coupling agent of this invention can reduce or avoid the use of traditional silane coupling agents, is pollution-free, emits no VOCs, and is low in cost and simple to process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber coupling agent technology, and more specifically, to a high epoxidized macromolecular coupling agent, its preparation method, and its application. Background Technology

[0002] In recent years, due to increased emphasis on ecological balance, environmental protection, and sustainable development, the design and manufacture of sustainable polymers have experienced tremendous growth. The development and production of sustainable materials using biomass has become a steadily growing field of interest. Nature provides a wealth of resources for the synthesis of environmentally friendly polymers, offering unique and fascinating molecular structures in green chemistry and alternative raw materials. This allows for the synthesis of novel bio-based green polymers with a wide range of applications. This not only reduces dependence on petrochemical resources but also lowers environmental pollution during the production and use of petrochemical products, reduces VOC emissions, and lowers production costs, demonstrating significant practical value and broad development prospects.

[0003] Silica, or hydrated silica, gets its name from its excellent reinforcing properties on rubber, similar to carbon black. In the tire industry, compared to carbon black, silica can reduce rolling resistance without sacrificing the rubber's wet grip, ensuring driving safety and effectively improving fuel efficiency, thereby reducing greenhouse gas emissions. Therefore, silica is a relatively ideal filler for "green tires."

[0004] However, silica has a large number of hydroxyl groups on its surface, resulting in high surface energy and making it prone to aggregation. This leads to poor dispersion of silica in rubber and poor compatibility with the rubber matrix. In the rubber industry, the most common method to solve these problems is to use silane coupling agents, such as the widely used silane coupling agent Si69. Silane coupling agents, as special materials, play an indispensable role in industrial production, but they also have some drawbacks. For example, sulfur-containing silanes can cause sulfur precipitation and scorching during rubber compounding, and aminosilane coupling agents are prone to yellowing during the use of ketoxime-type and alcohol-type silicone rubbers.

[0005] The structural formula of the silane coupling agent is: YR-Si(Me) n X 3-n (n=0,1), where X is a hydrolyzable group, such as -Cl, -OCH, -OCH, -OOCCH. During use, it hydrolyzes to form Si-OH, which can condense and dehydrate with -OH on the surface of inorganic materials; Y is a reactive organic group, such as cyano, epoxy, vinyl, acrylic, isocyanate, mercapto, etc., which can react with organic matter.

[0006] Si69 possesses both ethoxy groups that react with the hydroxyl groups on the surface of silica and sulfur groups that can crosslink with rubber, thus effectively coupling silica and rubber to improve silica dispersion and enhance the interfacial bonding between silica and rubber. However, the process of silanizing silica surface using silane coupling agents typically generates volatile organic compounds (VOCs) (such as methanol and ethanol), which pose certain hazards to the environment and human health. Furthermore, the use of silane coupling agents increases costs and simplifies the preparation process. Summary of the Invention

[0007] To address the problems existing in the prior art, this invention provides a high-epoxidation macromolecular coupling agent, its preparation method, and its application. The coupling agent of this invention can reduce or even replace the use of silane coupling agents, and has the advantages of being pollution-free, emitting no VOCs, low cost, and having a simple preparation process.

[0008] One objective of this invention is to provide a high-epoxidation macromolecular coupling agent, which is obtained by mixing and vulcanizing raw materials comprising the following components: Each component, by weight: 100 parts by weight of a copolymer of myrcene and glycidyl methacrylate; 5-80 parts by weight of dicarboxylic acid compounds.

[0009] The GMA structure is as follows:

[0010] The structural formula of myrcene is:

[0011] By selecting glycidyl methacrylate (GMA), which has both carbon-carbon double bonds and epoxy groups, as a suitable modifying monomer, and copolymerizing it with myrcene to obtain raw rubber, the elastomer is over-crosslinked by reacting it with diacid compounds to form a hard and brittle resin, which is then ground into powder to obtain the high epoxidized macromolecular coupling agent.

[0012] Preferably, the components are expressed in parts by weight as follows: 100 parts by weight of a copolymer of myrcene and glycidyl methacrylate; 10-40 parts by weight of diacid compounds.

[0013] Preferably, the number-average molecular weight (Mn) of the copolymer of myrcene and glycidyl methacrylate is 100,000 to 1,000,000, more preferably 100,000 to 200,000; and the molecular weight distribution (Mw / Mn) is 1.5 to 5.0, more preferably 1.5 to 2.5. When the molecular weight and molecular weight distribution reach the above values, it can be ensured that the material has sufficient epoxy groups and good processing performance, making it suitable for industrial applications.

[0014] Preferably, the dicarboxylic acid compound is at least one selected from oxalic acid, glutamic acid, sebacic acid, isophthalic acid, phthalic acid, itaconic acid, maleic acid, and dithiodipropionic acid; more preferably, dithiodipropionic acid.

[0015] Preferably, the copolymer of myrcene and glycidyl methacrylate is prepared from raw materials comprising the following components: Water-soluble components, oil-soluble components, initiators, and flocculants; The water-soluble components include deionized water, emulsifier, electrolyte, and activator. Oil-soluble components include myrcene monomer, glycidyl methacrylate monomer, and chain transfer agent; Each component, by weight: The total weight of myrcene monomer and glycidyl methacrylate monomer is 100 parts by weight, and the weight ratio of myrcene monomer to glycidyl methacrylate monomer is (50-95):(50-5). The initiator is 0.01-5 parts by weight; The flocculant content is 100-400 parts by weight; Deionized water is 100-300 parts by weight; The emulsifier is 2-10 parts by weight; The electrolyte is 0.1-3 parts by weight; The activator is 0.01-0.5 parts by weight; The chain transfer agent is 0.03-0.25 parts by weight.

[0016] Preferably, the components are expressed in parts by weight as follows: The total weight of myrcene monomer and glycidyl methacrylate monomer is 100 parts by weight, and the weight ratio of myrcene monomer to glycidyl methacrylate monomer is (70-90):(30-10). The initiator is 0.02-3 parts by weight; The flocculant content is 100-300 parts by weight; Deionized water is 150-300 parts by weight; The emulsifier is 2.5-8 parts by weight; The electrolyte content is 0.1-1.5 parts by weight; The activator is 0.02-0.3 parts by weight; The chain transfer agent is 0.05-0.2 parts by weight.

[0017] Preferably, the initiator is a low-temperature emulsion polymerization initiator or a high-temperature emulsion polymerization initiator; The low-temperature emulsion polymerization initiator is at least one of p-menthol peroxide, azobisisobutyronitrile, tert-butyl hydroperoxide, and cumene hydroperoxide, preferably p-menthol peroxide or cumene hydroperoxide. The high-temperature emulsion polymerization initiator is at least one of potassium persulfate, ammonium persulfate, benzoyl peroxide, azobisisobutyronitrile, and azobisheptanenitrile; The chain transfer agent is at least one selected from n-dodecyl mercaptan, tert-dodecyl mercaptan, mercaptoethanol, carbon tetrabromide, and isooctyl 3-mercaptopropionate. The addition of a special chain transfer agent with a large chain transfer constant is to adjust the molecular weight of the rubber product. The chain transfer agent becomes a free radical through a chain transfer reaction, which can initiate the reaction, act as an activation center, and ultimately bind to the polymer and be consumed. A small amount can effectively interfere with excessive growth and branching of macromolecular chains, reducing gelation. The emulsifier can be a commonly used emulsifier in the rubber industry, such as sodium dodecylbenzene sulfonate (SDBS), sodium dodecyl sulfonate (SDS), potassium disproportionate, sodium fatty acid, alkylphenol polyoxyethylene ether (OP-10); preferably, it is a mixture of potassium disproportionate and sodium fatty acid. The activator can be a commonly used activator in the rubber industry, such as at least one of sodium formaldehyde sulfoxylate, ferrous sulfate, sodium ethylenediaminetetraacetate, and tetrasodium ethylenediaminetetraacetate; preferably sodium formaldehyde sulfoxylate, ferrous sulfate, and tetrasodium ethylenediaminetetraacetate. The electrolyte is at least one of potassium chloride, potassium phosphate, sodium chloride, and sodium phosphate, preferably potassium chloride or potassium phosphate.

[0018] The flocculant used in the demulsification and drying process can be a commonly used flocculant in the rubber industry, such as methanol, ethanol, calcium chloride, sodium chloride, dicyandiamine formaldehyde condensate, epoxy amine compounds, dilute sulfuric acid, etc.; in this invention, ethanol and epoxy amine compounds are preferred.

[0019] In the copolymer formulation of myrcene and glycidyl methacrylate of the present invention, conventional additives such as sodium dithionite, stearic acid, and antioxidant 4020 can also be added according to actual conditions. The dosage is conventional and can be added by technicians according to actual conditions.

[0020] Preferably, the copolymer is prepared by the following steps: The copolymer was prepared by redox emulsion polymerization of the components according to the specified weight parts.

[0021] The following solutions can be adopted: First, the water-soluble and oil-soluble components are mixed and pre-emulsified, then an initiator is added to polymerize and obtain a myrcene / glycidyl methacrylate copolymer latex. Finally, the latex is demulsified with a flocculant and dried to obtain the copolymer of myrcene and glycidyl methacrylate.

[0022] The pre-emulsification time is 1-5 h, preferably 1-2 h; if low-temperature emulsion polymerization is used, the reaction temperature is 0-30℃, preferably 5-20℃, and the polymerization reaction time is 3-20 h, preferably 4-12 h; if high-temperature emulsion polymerization is used, the reaction temperature is 50-70℃, preferably 60-70℃, and the polymerization time is 10-24 h, preferably 12-24 h.

[0023] A second objective of this invention is to provide a method for preparing a high-epoxidized macromolecular coupling agent, the method comprising: The coupling agent is obtained by mixing and vulcanizing the components according to the specified weight proportions.

[0024] The mixing and vulcanization is preferably carried out at 120-180℃ using compression molding vulcanization.

[0025] The third objective of this invention is to provide an application of a high-epoxidation macromolecular coupling agent in the rubber modification process, wherein the coupling agent, silica, and rubber are mixed and vulcanized to obtain modified rubber.

[0026] Because silica has a large number of hydroxyl groups on its surface, by giving rubber some functional groups that can react with hydroxyl groups, the interaction between silica and rubber will be greatly enhanced by the formation of covalent bonds; the aggregation of silica will also be effectively prevented; and the hydroxyl groups on the surface of silica will undergo ring-opening reactions with polymers containing epoxy groups under the action of mechanical shear and heat.

[0027] The amount of the high epoxidized macromolecular coupling agent is 5-40 parts by weight per 100 parts by weight of the rubber matrix.

[0028] During the vulcanization process of mixing with silica and rubber, commonly used rubber additives can be added, such as zinc oxide, stearic acid, antioxidant 4020, antioxidant RD, accelerator CZ, accelerator NS, and sulfur. The dosage is the conventional dosage, and technicians can add according to the actual situation.

[0029] Compared with the prior art, the present invention has the following superior effects: This invention prepares a bio-based high-epoxy macromolecular coupling agent. By utilizing the reactivity of epoxy with silica, reactive sites are constructed on the rubber molecular chain segments to improve silica dispersion. Specifically, this invention involves the co-curing and vulcanization of a copolymer of myrcene and glycidyl methacrylate with a diacid compound. This allows the copolymer to undergo over-crosslinking, resulting in a powdered product that functions as a coupling agent during rubber compounding. Furthermore, the myrcene monomer used in this invention is a bulk bio-based terpene olefin with broad applications in industrial production. The copolymer of myrcene and glycidyl methacrylate is prepared using low-temperature and high-temperature redox emulsion polymerization techniques, resulting in a simple process suitable for industrial production. This high-epoxy macromolecular coupling agent reduces or avoids the use of traditional silane coupling agents, is pollution-free, emits no VOCs, and is low-cost and simple to process. Detailed Implementation

[0030] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.

[0031] All raw materials used in the embodiments of this invention are commercially available products, and specific information is shown in Table 1: Table 1

[0032] The experimental testing instruments used in this embodiment are as follows: DSC: A SATRE System DSC analyzer manufactured by Mettler Toledo, Switzerland, was used. The test conditions were as follows: the temperature was first raised from room temperature to 100°C at a rate of 20°C / min, held at 100°C for 3 min, then lowered from 100°C to -80°C at a rate of 20°C / min, and then raised back to 100°C at a rate of 10°C / min. The heat change during the second heating process was recorded. The glass transition temperature was the midpoint of the thermomelting transition on the curve.

[0033] GPC: The tests were performed using a Waters 515 HPLC pump and a Waters 2410 R1 Detector gel chromatography system manufactured by Waters Corporation, USA, with polystyrene as the standard and tetrahydrofuran as the mobile phase.

[0034] 1H-NMR: Nuclear magnetic resonance spectroscopy was performed using a Bruker AV400MHz high-resolution liquid nuclear magnetic resonance spectrometer, with deuterated chloroform (CDCl3) as solvent and tetramethylsilane (TMS) as internal standard.

[0035] Example 1 In a reactor, 1.5 parts by weight of potassium disproportionated rosinate, 1 part by weight of sodium fatty acid, 150 parts by weight of deionized water, 0.005 parts by weight of ferrous sulfate, 0.01 parts by weight of sodium formaldehyde sulfoxylate, 0.005 parts by weight of tetrasodium ethylenediaminetetraacetate, 0.1 parts by weight of potassium chloride, 0.05 parts by weight of tert-dodecyl mercaptan, 50 parts by weight of myrcene, and 50 parts by weight of glycidyl methacrylate were added. The reactor was sealed and purged with a nitrogen atmosphere (nitrogen was evacuated three times to remove oxygen). Pre-emulsification was carried out at 25°C for 1 h. Then, 0.01 parts by weight of hydrogen peroxide was added to p-menthol to initiate polymerization. The reaction was carried out at 10°C for 8 h to obtain a copolymer latex. The latex was demulsified with 100 parts by weight of ethanol and dried in a vacuum oven to constant weight to obtain a copolymer of myrcene and glycidyl methacrylate. NMR calculations showed that the structural units of myrcene monomer accounted for 65% of the copolymer, with a conversion rate of 72%, and Mn = 11.2 × 10⁻⁶. 4 Mw / Mn=1.89.

[0036] 100 parts by weight of the copolymer of the above myrcene and glycidyl methacrylate, dimethylimidazole, zinc acetate, and 10 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0037] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0038] Example 2 In a reactor, 1.5 parts by weight of potassium disproportionated rosinate, 1 part by weight of sodium fatty acid, 150 parts by weight of deionized water, 0.005 parts by weight of ferrous sulfate, 0.01 parts by weight of sodium formaldehyde sulfoxylate, 0.005 parts by weight of tetrasodium ethylenediaminetetraacetate, 0.1 parts by weight of potassium chloride, 0.05 parts by weight of tert-dodecyl mercaptan, 70 parts by weight of myrcene, and 30 parts by weight of glycidyl methacrylate were added. The reactor was sealed and purged with a nitrogen atmosphere (nitrogen was evacuated three times to remove oxygen). Pre-emulsification was carried out at 25°C for 1 h. Then, 0.01 parts by weight of hydrogen peroxide was added to p-menthol to initiate polymerization. The reaction was carried out at 10°C for 8 h to obtain a copolymer latex. The latex was demulsified with 100 parts by weight of ethanol and dried in a vacuum oven to constant weight to obtain a copolymer of myrcene and glycidyl methacrylate. NMR calculations showed that the structural units of myrcene monomer accounted for 66% of the copolymer, with a conversion rate of 71%, and Mn = 12.2 × 10⁻⁶.4 Mw / Mn=1.86.

[0039] 100 parts by weight of the copolymer of the above myrcene and glycidyl methacrylate, dimethylimidazole, zinc acetate, and 10 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0040] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0041] Example 3 In a reactor, 1.5 parts by weight of potassium disproportionated rosinate, 1 part by weight of sodium fatty acid, 150 parts by weight of deionized water, 0.005 parts by weight of ferrous sulfate, 0.01 parts by weight of sodium formaldehyde sulfoxylate, 0.005 parts by weight of tetrasodium ethylenediaminetetraacetate, 0.1 parts by weight of potassium chloride, 0.05 parts by weight of tert-dodecyl mercaptan, 90 parts by weight of myrcene, and 10 parts by weight of glycidyl methacrylate were added. The reactor was sealed and purged with nitrogen (nitrogen was evacuated three times to remove oxygen). Pre-emulsification was carried out at 25°C for 1 h. Then, 0.01 parts by weight of hydrogen peroxide was added to p-menthol to initiate polymerization. The reaction was carried out at 10°C for 8 h to obtain a copolymer latex. The latex was demulsified with 100 parts by weight of ethanol and dried in a vacuum oven to constant weight to obtain a copolymer of myrcene and glycidyl methacrylate. NMR calculations showed that the structural units of myrcene monomer accounted for 66% of the copolymer, with a conversion rate of 73%, and Mn = 11.5 × 10⁻⁶. 4 Mw / Mn=1.91.

[0042] 100 parts by weight of the copolymer of the above myrcene and glycidyl methacrylate, dimethylimidazole, zinc acetate, and 10 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0043] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0044] Example 4 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 3, dimethylimidazole, zinc acetate, and 10 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0045] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 5 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0046] Example 5 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 3, dimethylimidazole, zinc acetate, and 10 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0047] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 10 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0048] Example 6 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 3, dimethylimidazole, zinc acetate, and 10 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0049] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 30 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0050] Example 7 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 3, dimethylimidazole, zinc acetate, and 10 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0051] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 40 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0052] Example 8 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 3, dimethylimidazole, zinc acetate, and 25 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0053] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0054] Example 9 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate, dimethylimidazole, zinc acetate, and 40 parts by weight of dithiodipropionic acid from Example 3 were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0055] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0056] Example 10 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 3, dimethylimidazole, zinc acetate, and 80 parts by weight of dithiodipropionic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0057] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0058] Example 11 In a reactor, 3.5 parts by weight of potassium disproportionated rosinate, 1.5 parts by weight of sodium fatty acid, 200 parts by weight of deionized water, 0.025 parts by weight of ferrous sulfate, 0.05 parts by weight of sodium formaldehyde sulfoxylate, 0.025 parts by weight of tetrasodium ethylenediaminetetraacetate, 1 part by weight of sodium chloride, 0.1 parts by weight of n-dodecyl mercaptan, 70 parts by weight of myrcene, and 30 parts by weight of glycidyl methacrylate were added. The reactor was sealed and purged with a nitrogen atmosphere (nitrogen was evacuated three times to remove oxygen). Pre-emulsification was carried out at 25°C for 1 h. Polymerization was initiated by adding 1 part by weight of tert-butyl hydroperoxide and reacted at 10°C for 8 h to obtain a copolymer latex. The latex was demulsified with 200 parts by weight of ethanol and dried in a vacuum oven to constant weight to obtain a copolymer of myrcene and glycidyl methacrylate. NMR calculations showed that the structural units of myrcene monomer accounted for 66% of the copolymer, with a conversion rate of 73% and Mn = 16.3 × 10⁻⁶. 4 Mw / Mn=1.75.

[0059] 100 parts by weight of the copolymer of the above myrcene and glycidyl methacrylate, dimethylimidazole, zinc acetate, and 10 parts by weight of itaconic acid phthalate were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0060] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0061] Example 12 In a reactor, 5.5 parts by weight of potassium disproportionated rosinate, 2.5 parts by weight of sodium fatty acid, 300 parts by weight of deionized water, 0.075 parts by weight of ferrous sulfate, 0.15 parts by weight of sodium formaldehyde sulfoxylate, 0.075 parts by weight of tetrasodium ethylenediaminetetraacetate, 1.5 parts by weight of potassium phosphate, 0.2 parts by weight of mercaptoethanol, 70 parts by weight of myrcene, and 30 parts by weight of glycidyl methacrylate were added. The reactor was sealed and purged with a nitrogen atmosphere (nitrogen was evacuated three times to remove oxygen). Pre-emulsification was carried out at 25°C for 1 h. Then, 3 parts by weight of azobisisobutyronitrile (AIBN) was added to initiate polymerization. The reaction was carried out at 10°C for 8 h to obtain a copolymer latex. The latex was demulsified with 300 parts by weight of ethanol and dried in a vacuum oven to constant weight to obtain a copolymer of myrcene and glycidyl methacrylate. NMR calculations showed that the structural units of myrcene monomer accounted for 66% of the copolymer, with a conversion rate of 77%, and Mn = 15.3 × 10⁻⁶. 4 Mw / Mn=1.77.

[0062] 100 parts by weight of the copolymer of the above myrcene and glycidyl methacrylate, dimethylimidazole, zinc acetate, and 10 parts by weight of isophthalic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0063] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0064] Example 13 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate, dimethylimidazole, zinc acetate, and 25 parts by weight of isophthalic acid from Example 11 were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0065] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0066] Example 14 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 11, dimethylimidazole, zinc acetate, and 40 parts by weight of isophthalic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0067] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above-mentioned macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizates, and their performance was then tested. Example 15 100 parts by weight of the copolymer of myrcene and glycidyl methacrylate from Example 11, dimethylimidazole, zinc acetate, and 80 parts by weight of isophthalic acid were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 160°C to prepare a macromolecular coupling agent.

[0068] 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of the above macromolecular coupling agent were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0069] Comparative Example 100 parts by weight of styrene-butadiene rubber, 5 parts by weight of zinc oxide, 2 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 1 part by weight of accelerator CZ, 1.2 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, 65 parts by weight of silica 1165, and 20 parts by weight of Si69 were mixed evenly on a two-roll mill to obtain a compound. The compound was then molded and vulcanized at 150°C to prepare styrene-butadiene rubber vulcanizate, and its performance was then tested.

[0070] The performance test results of each embodiment and comparative sample are shown in Table 2: Table 2

[0071] The performance of the above embodiments was tested according to the following standards: tensile testing was conducted according to ASTM D412 (dumbbell-shaped specimen); tensile strength and elongation at break were tested according to GB / T 528-2009; hardness testing was conducted according to ASTM D395; and the loss factor (tan) was measured using a dynamic viscoelastic spectrometer. d The relationship between temperature and temperature was studied using a tensile test with conditions of 10 Hz, 0.3% strain, and a temperature increase of 3℃ / min from -80℃ to 100℃.

[0072] As can be seen from the data in Table 2, compared with the use of traditional silane coupling agents (comparative example), the styrene-butadiene rubber reinforced by the macromolecular coupling agent of the present invention combined with silica in the examples has a higher tensile strength, reaching about 30 MPa; the elongation at break and hardness are comparable to those of the comparative example.

[0073] 0℃ tan d The loss factor is higher than that of the comparative example, indicating that the styrene-butadiene rubber prepared using the coupling agent of this application has superior anti-slip properties; while the loss factor of the example at 60℃ tan d The ratio is between 0.03 and 0.15, which is low compared to the control ratio, indicating that the styrene-butadiene rubber prepared using the coupling agent of this application has lower rolling resistance. Therefore, the styrene-butadiene rubber prepared in the examples has excellent overall performance and is significantly better than styrene-butadiene rubber using traditional silane coupling agents.

[0074] Furthermore, the macromolecular coupling agent of the present invention is pollution-free, does not emit VOCs, and is low in cost and simple in process, which conforms to the concept of green chemical industry. It is of great significance for rubber processing and manufacturing, reducing costs and alleviating environmental pressure.

Claims

1. Use of a hyper-epoxidized macromolecular coupling agent in a rubber modification process, characterized in that, Modified rubber is obtained by mixing and vulcanizing a high-epoxidation macromolecular coupling agent, silica, and rubber. The amount of the high epoxidized macromolecular coupling agent is 10-40 parts by weight, based on 100 parts by weight of the rubber matrix. The high-epoxidation macromolecular coupling agent is prepared by mixing and vulcanizing raw materials comprising the following components: Each component, by weight: 100 parts by weight of a copolymer of myrcene and glycidyl methacrylate; 5-80 parts by weight of diacid compounds; The copolymer of myrcene and glycidyl methacrylate is prepared from raw materials comprising the following components: Water-soluble components, oil-soluble components, initiators, and flocculants; The water-soluble components include deionized water, emulsifier, electrolyte, and activator. Oil-soluble components include myrcene monomer, glycidyl methacrylate monomer, and chain transfer agent; Each component, by weight: The total weight of myrcene monomer and glycidyl methacrylate monomer is 100 parts by weight, and the weight ratio of myrcene monomer to glycidyl methacrylate monomer is (70-90):(30-10). The initiator is 0.01-5 parts by weight; The flocculant content is 100-400 parts by weight; Deionized water is 100-300 parts by weight; The emulsifier is 2-10 parts by weight; The electrolyte is 0.1-3 parts by weight; The activator is 0.01-0.5 parts by weight; The chain transfer agent is 0.03-0.25 parts by weight; The copolymer of myrcene and glycidyl methacrylate is prepared by the following steps: The copolymer was prepared by redox emulsion polymerization of the components of the copolymer of myrcene and glycidyl methacrylate in the specified weight proportions.

2. The application as described in claim 1, characterized in that: The components of the high-epoxidized macromolecular coupling agent, by weight parts: 100 parts by weight of a copolymer of myrcene and glycidyl methacrylate; 10-40 parts by weight of diacid compounds.

3. Use according to claim 1, characterized in that: The copolymer of myrcene and glycidyl methacrylate has a number-average molecular weight of 100,000 to 1,000,000 and a molecular weight distribution of 1.5 to 5.

0.

4. Use according to claim 3, wherein: The copolymer of myrcene and glycidyl methacrylate has a number-average molecular weight of 100,000 to 200,000 and a molecular weight distribution of 1.5 to 2.

5.

5. The use according to claim 1, characterized in that: The dicarboxylic acid compound is at least one of oxalic acid, glutamic acid, sebacic acid, isophthalic acid, phthalic acid, itaconic acid, maleic acid, and dithiodipropionic acid.

6. The use according to claim 1, characterized in that: The copolymer of myrcene and glycidyl methacrylate comprises the following components in parts by weight: The total weight of myrcene monomer and glycidyl methacrylate monomer is 100 parts by weight; The initiator is 0.02-3 parts by weight; The flocculant content is 100-300 parts by weight; Deionized water is 150-300 parts by weight; The emulsifier is 2.5-8 parts by weight; The electrolyte content is 0.1-1.5 parts by weight; The activator is 0.02-0.3 parts by weight; The chain transfer agent is 0.05-0.2 parts by weight.

7. The use according to claim 1, characterized in that: The initiator is a low-temperature emulsion polymerization initiator or a high-temperature emulsion polymerization initiator; The low-temperature emulsion polymerization initiator is at least one of p-menthol peroxide, azobisisobutyronitrile, tert-butyl hydroperoxide, and diisopropylbenzene hydroperoxide. The high-temperature emulsion polymerization initiator is at least one of potassium persulfate, ammonium persulfate, benzoyl peroxide, and azobisheptanonitrile; The chain transfer agent is at least one of n-dodecyl mercaptan, tert-dodecyl mercaptan, mercaptoethanol, carbon tetrabromide, and isooctyl 3-mercaptopropionate. The electrolyte is at least one of potassium chloride, potassium phosphate, sodium chloride, and sodium phosphate.

8. The application as described in claim 7, characterized in that: The low-temperature emulsion polymerization initiator is p-menthane hydrogen peroxide or diisopropylbenzene hydrogen peroxide.

9. The use according to claim 1, wherein The highly epoxidized macromolecular coupling agent is prepared by the following steps: The coupling agent is obtained by mixing and vulcanizing the components of the high epoxidized macromolecular coupling agent according to the specified weight proportions.

Citation Information

Patent Citations

  • Rubber composite material using cardanol glycidyl ether modified silica and preparation method thereof

    CN109467770A

  • Softener for polypropylene, its production method, and soft polypropylene resin composition

    JP2002256122A