Polymeric spiro phosphorus-nitrogen intumescent flame retardant and preparation method thereof

Through the development of polymerized spirocyclophosphorus nitrogen expansion flame retardant, the problems of flammability and smoke generation of epoxy resin are solved, and the high-efficiency flame retardant and mechanical properties are achieved at low addition amounts, providing a green and environmentally friendly Flame retardant solutions.

CN118930871AActive Publication Date: 2024-11-12BEIJING INST OF TECH

Patent Information

Application Number
CN202410999932.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing epoxy resin flame retardants are flammable and produce toxic fumes when burned. The traditional halogen-free flame retardants have insufficient mechanical properties and added amounts, and have poor compatibility, making it difficult to achieve ideal resistance at low added amounts. Burning effect.

Method used

Develop a polymeric spirocyclophosphorus nitrogen expansion flame retardant, prepared by reaction of pentaerythritol with oxychloride and 4,6-dihydroxypyrimidine to form a highly symmetrical phosphorus-nitrogen structure to achieve good compatibility with the matrix and Highly efficient flame retardant effect. The flame retardant can achieve the V-0 flame retardant effect of UL-94 at an addition amount of 0.5% to 2.5%, maintain the mechanical properties of the material, and inhibit smoke and heat release through catalytic carbon formation effect.

Benefits of technology

The high-efficiency flame retardant of epoxy resin is achieved at low addition amount, reducing the production of smoke and harmful gases, improving fire safety, and the decomposition temperature is suitable for flame retardant materials, supporting the green and environmentally friendly applications of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930871A_ABST
    Figure CN118930871A_ABST
Patent Text Reader

Abstract

The invention relates to a polymeric spirocyclic phosphorus-nitrogen intumescent flame retardant and a preparation method thereof, and belongs to the technical field of flame retardants. The flame retardant is a polymeric phosphorus-nitrogen intumescent flame retardant with a highly symmetrical structure and a cage-shaped structure, pentaerythritol and phosphorus oxychloride react to obtain spirocyclic phosphate diacyl chloride, then the spirocyclic phosphate diacyl chloride reacts with 4, 6-dihydroxypyrimidine to obtain a crude product, and the crude product is purified to obtain the flame retardant. The flame retardant can reach V-0 flame-retardant epoxy resin of UL-94 only under the addition amount of 0.5%-2.5%, the efficient and environment-friendly flame-retardant effect is achieved, the mechanical property of the material is not reduced, and the tensile strength is still kept to be 54.9 MPa or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polymeric spirocyclic phosphorus nitrogen expansion flame retardant and a preparation method thereof, belonging to the technical field of flame retardants. Background Art

[0002] Epoxy resin (EP) is widely used in chemical corrosion protection, small electronic equipment, building materials, and lightweight structures of spacecraft due to its excellent chemical resistance, low shrinkage, insulation, and mechanical properties. However, epoxy resin is currently very flammable, and it emits a large amount of toxic smoke into the air during combustion, making it difficult to protect human life and property safety. For this reason, it is extremely necessary to study and prepare new flame retardants that improve the flame retardancy of EP and reduce the harm of smoke. However, most of the traditional high-efficiency flame retardants require the introduction of halogen elements, such as decabromodiphenyl ether, chlorinated paraffin, and tetrabromophthalic anhydride, which are extremely harmful to the ecological environment. In recent years, environmentally friendly halogen-free flame retardants have gradually replaced this type of flame retardant, injecting new impetus into sustainable flame retardant solutions.

[0003] In the past decade, halogen-free flame retardants have been widely used in flame-retardant polymer materials, such as 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), boron nitride, carbon nanomaterials, SiO2, organic-inorganic hybrid compounds (such as polyhedral siloxanes and metal organic frameworks), etc. Among these materials, phosphorus nitrogen expansion flame retardant, as a kind of green flame retardant, is a new type of flame retardant with potential development advantages due to its excellent free radical capture effect. As one of such flame retardants, DOPO, with its special phosphaphenanthrene structure, can give epoxy resin excellent fire resistance and antioxidant properties. The active PH bond in DOPO ensures the possibility of its various modifications, such as substitution, oxidation, addition, etc. However, DOPO derivatives mainly exhibit gas phase flame retardant mechanism, which is not conducive to suppressing the release of smoke, and often require the addition of a large amount of DOPO flame retardants, which is not conducive to ensuring the mechanical properties of polymer materials.

[0004] Spirocyclic phosphoryl chloride (SPDPC) is a kind of phosphorus flame retardant. It has a stable heterocyclic structure and high thermal stability. Thanks to the presence of pentaheptanol in its spirocyclic structure, SPDPC has good carbonization performance, can inhibit the further combustion of polymer materials, and play a flame retardant effect in gas phase free radical capture and condensed phase carbonization. In addition, this type of flame retardant also has an active P-Cl bond, which can realize a variety of modification methods (introduction of amino groups) on this functional group, and prepare many new expansion flame retardants that integrate three sources. However, at present, this type of flame retardant (such as a polymeric expansion flame retardant disclosed in CN109096492A) often requires a higher addition amount (more than 5%) to achieve the desired flame retardant effect, and there is little research on new polymeric flame retardants with good compatibility with the matrix, which needs further expansion research. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a polymeric spirocyclic phosphorus nitrogen expansion flame retardant and a preparation method thereof. The flame retardant is a highly symmetrical polymeric phosphorus nitrogen expansion flame retardant, which not only has good compatibility with the matrix, but also can achieve excellent flame retardant effect at a lower addition amount, greatly ensuring the excellent mechanical properties of the material itself, which is of great significance for green flame retardancy and broadening the scope of use of the material.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] A polymeric spirocyclic phosphorus nitrogen intumescent flame retardant (DHPPC), the structural formula of the flame retardant is as follows:

[0008]

[0009] The repeating unit is C9O8N2H 10 P2, the degree of polymerization n is an integer of 8-12.

[0010] Preferably, the molecular weight of the flame retardant is 3000-4000.

[0011] A method for preparing the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant of the present invention comprises the following steps:

[0012] Step 1: In a closed system without water or oxygen, add pentaerythritol to solvent A, stir until the system is evenly mixed, heat to temperature 1, add phosphorus oxychloride, introduce nitrogen and keep warm for 2 to 4 hours, then heat to temperature 2 and stir for 8 to 16 hours, wash and dry to obtain an intermediate spirocyclic phosphate dichloride; wherein the molar ratio of pentaerythritol to phosphorus oxychloride is 1:2 to 7; temperature 1 is 40 to 70° C., and temperature 2 is 80 to 120° C.;

[0013] Step 2: In an anhydrous and oxygen-free environment, 4,6-dihydroxypyrimidine is added to solvent B, stirred until the solution is clear and transparent, the intermediate spirocyclic phosphate dichloride and the acid binding agent are added, pre-reacted at temperature 3 for 1 to 2 hours, then heated to temperature 4 and stirred and refluxed for 6 to 16 hours. After the reaction is completed, the crude flame retardant is washed and dried to obtain a yellow-brown powdery solid; wherein the molar ratio of 4,6-dihydroxypyrimidine to spirocyclic phosphate dichloride is 1:1 to 1.5, temperature 3 is 30 to 55° C., and temperature 4 is 60 to 100° C.;

[0014] Step 3: Grind the crude flame retardant, reflux and purify it, and then dry it to obtain a polymeric spirocyclic phosphorus nitrogen expansion flame retardant.

[0015] Preferably, in step 1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:3-5.

[0016] Preferably, in step 1, the stirring rate is 220-300 rpm.

[0017] Preferably, in step 1, the flow rate of nitrogen is 5 to 20 mL / min.

[0018] Preferably, in step 1, temperature 1 is 55-65° C. Under this temperature condition, the reaction is more gentle and the yield is higher.

[0019] Preferably, in step 1, temperature 2 is 90-110°C.

[0020] Preferably, in step 1, the solvent A is one or more of anhydrous acetonitrile, acetone, dichloromethane and dioxane.

[0021] Preferably, in step 1, one or more of acetone, chloroform and dichloromethane are used for washing.

[0022] Preferably, in step 2, the solvent B is one or more of acetone, tetrahydrofuran, xylene, anhydrous acetonitrile and N,N-dimethylformamide.

[0023] Preferably, in step 2, the acid binding agent is one or more of triethylamine, cerium chloride, anhydrous potassium carbonate and pyridine.

[0024] Preferably, in step 2, the molar ratio of the 4,6-dihydroxypyrimidine to the acid binding agent is 1:1.5-2.2.

[0025] Preferably, in step 2, temperature 4 is 70-85°C.

[0026] Preferably, in step 2, one or more of deionized water, ether, anhydrous methanol, anhydrous ethanol, dichloromethane and acetonitrile are used for washing.

[0027] Preferably, in step three, during the reflux purification, the solvent is one or more of acetone, dichloromethane, anhydrous ethanol and tetrahydrofuran.

[0028] Preferably, in step three, during the reflux purification, the temperature is 60 to 90° C., and the cooling reflux is performed for 3 to 12 hours.

[0029] Preferably, in step 1, step 2 and step 3, during drying, vacuum drying is performed at 80-100° C. for 12-24 hours.

[0030] Beneficial Effects

[0031] 1. The present invention provides a polymeric phosphorus-nitrogen intumescent flame retardant, which is a highly symmetrical polymeric phosphorus-nitrogen intumescent flame retardant with a cage structure. It can achieve UL-94 V-0 grade flame retardant epoxy resin with an addition amount of only 0.5% to 2.5%, achieving a highly efficient and environmentally friendly flame retardant effect, and the mechanical properties of the material itself are not reduced, and the tensile strength is still maintained above 54.9MPa.

[0032] 2. The present invention provides a polymeric phosphorus-nitrogen intumescent flame retardant. When the addition amount is only 1% in the flame-retardant epoxy resin, the limiting oxygen index can reach 29.8%, and when the addition amount is 2.5%, the limiting oxygen index can reach 31.8%. After adding 1% of this flame retardant, the peak heat release rate can be reduced by 42.3%, the carbon dioxide production can be reduced by 32.5%, and the carbon monoxide production can be reduced by 38.3%, and the smoke suppression effect is outstanding.

[0033] 3. The polymeric phosphorus-nitrogen intumescent flame retardant provided by the present invention is a new type of green and environmentally friendly flame retardant. The product has a small amount of smoke and no molten droplets, and has high fire safety.

[0034] 4. The polymeric phosphorus-nitrogen intumescent flame retardant provided by the present invention has a symmetrical structure and, thanks to its pentaerythritol spirocyclic structure, has a decomposition temperature in the range of 250 to 300°C, which is lower than the decomposition temperature of epoxy resin. It can preferentially decompose and flame retardant during the combustion process, and has a good catalytic carbonization effect.

[0035] 5. The polymeric phosphorus-nitrogen intumescent flame retardant provided by the present invention has a simple preparation method and easily controllable reaction conditions, a yield of more than 98.5%, a high purity can be ensured through simple purification, and can be scaled up for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is the infrared spectrum of the flame retardant described in Example 1.

[0037] Figure 2 This is the nuclear magnetic phosphorus spectrum of the flame retardant described in Example 1.

[0038] Figure 3This is the H NMR spectrum of the flame retardant described in Example 1. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below in conjunction with specific embodiments.

[0040] A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant, the specific steps are as follows:

[0041] Step 1: In a closed system without water or oxygen, add fully ground pentaerythritol to solvent A, first stir at room temperature until the system is evenly mixed, raise the system temperature to temperature 1, add freshly distilled phosphorus oxychloride, introduce nitrogen and react under this temperature condition until the system is stable (this process takes 2 to 4 hours), further slowly heat to temperature 2, stir and react until no gas is generated (this process takes 8 to 16 hours), wash the product with solvent B for multiple times, filter and vacuum dry to obtain the intermediate spirocyclic phosphate dichloride.

[0042] In some embodiments, the molar ratio of pentaerythritol to phosphorus oxychloride in step 1 is preferably 1:(2-7), and more preferably 1:(3-5);

[0043] In some embodiments, the solvent A in step 1 is one of anhydrous acetonitrile, acetone, dichloromethane, dioxane or a mixed solvent, and all solvents need to be dried before use to prevent the introduction of moisture;

[0044] In some embodiments, the flow rate of nitrogen in step 1 is 5 to 20 mL / min;

[0045] In some embodiments, the temperature 1 in step 1 is 40-70° C., and the more preferred temperature is 55-65° C. Under this temperature condition, the reaction is more gentle and the yield is higher;

[0046] In some embodiments, the temperature 2 in step 1 is 80-120° C., and a more preferred temperature is 90-110° C.;

[0047] In some embodiments, the stirring rate in step 1 is 220-300 rpm;

[0048] In some embodiments, the solvent B in step 1 is acetone, chloroform, or dichloromethane, and the order of washing is not important.

[0049] Step 2: In an anhydrous and oxygen-free environment, 4,6-dihydroxypyrimidine is added to solvent C, stirred at room temperature until the solution is clear and transparent, the intermediate spirocyclic phosphate dichloride synthesized in step 1 is added, and an acid binding agent is added to make the nucleophilic substitution reaction more complete, pre-react at temperature 3, further slowly heat up, and stir and reflux at temperature 4. After the reaction is completed, the solvent D is used for alternate washing multiple times, filtered, and vacuum dried to obtain a crude flame retardant as a yellow-brown powdery solid.

[0050] In some embodiments, the solvent C in step 2 is one of acetone, tetrahydrofuran, xylene, anhydrous acetonitrile, and N,N-dimethylformamide. All solvents are analytical grade and are soaked in molecular sieves to remove water for 48 hours before use.

[0051] In some embodiments, the molar ratio of 4,6-dihydroxypyrimidine and spirocyclic phosphate dichloride in step 2 is preferably 1:(1-1.5);

[0052] In some embodiments, the temperature 3 in step 2 is 30-55° C., and the pre-reaction is 1-2 hours;

[0053] In some embodiments, the temperature 4 in step 2 is 60-100° C.; more preferably 70-85° C.;

[0054] In some embodiments, the reflux time in step 2 is preferably 12 to 36 hours;

[0055] In some embodiments, the acid-binding agent in step 2 is triethylamine, cerium chloride, anhydrous potassium carbonate and pyridine. The introduction of the acid-binding agent will increase the product yield, but will produce certain ion salts that affect the product purity; therefore, the molar ratio of 4,6-dihydroxypyrimidine to the acid-binding agent is 1:1.5-2.2;

[0056] In some embodiments, the solvent D in step 2 is one or more of deionized water, ether, anhydrous methanol, anhydrous ethanol, dichloromethane, and acetonitrile, and the washing order is not distinguished.

[0057] Step 3: Grind the obtained polymeric flame retardant crude product thoroughly, transfer it to filter paper for wrapping after weighing, and wrap a circle of rubber rope around the filter paper to prevent the loss of the sample during the purification process. Put the filter paper wrapped with the sample horizontally into a Soxhlet extractor with a condensing device, add solvent E to completely soak the filter paper, raise the reaction temperature to 5, cool and reflux for purification, and vacuum dry it after purification to obtain a polymeric spirocyclic phosphorus nitrogen expansion flame retardant.

[0058] In some embodiments, the solvent E in step 3 is one or more of acetone, dichloromethane, anhydrous ethanol, and tetrahydrofuran;

[0059] In some embodiments, the temperature 5 described in step 3 is 60-90° C., which can be selected according to different types of purification solvents to ensure that the selected temperature range is higher than the boiling point of the solvent;

[0060] In some embodiments, the reflux time in step three is preferably 3 to 12 hours, and the reflux time is adjusted according to the solubility of the solvent.

[0061] In some embodiments, the vacuum drying temperature is 80-100° C., and the drying time is 12-24 hours.

[0062] Example 1

[0063] A method for preparing a polymeric intumescent flame retardant DHPPC, the specific steps are as follows:

[0064] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 250mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under nitrogen protection until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 65°C and quickly add 69.3g (0.45mol) of newly distilled phosphorus oxychloride, react until the system is stable (this process takes 3h), then slowly increase the temperature to 100°C, and react until no HCl gas is produced at the tail gas outlet (reaction ends). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and dry it at 100°C under vacuum conditions (-0.1MPa) for 12h to obtain 32.4g of white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 85.8%.

[0065] The molar ratio of spirocyclic phosphate dichloride and 4,6-dihydroxypyrimidine was 1:1. 1.12g (0.01mol) of 4,6-dihydroxypyrimidine was weighed and added to a 100mL three-necked flask. The magnetic stirring, condenser and tail gas treatment device were connected. The mixture was stirred in 50mL acetonitrile under nitrogen protection until it became clear and transparent. 2.97g (0.01mol) of spirocyclic phosphate dichloride was added, the temperature was raised to 40°C for reaction for 1h, and the temperature was further raised to 65°C for stirring and reflux for 20h. The precipitate obtained by the reaction was filtered, and washed alternately with water, ether and acetone three times. The crude flame retardant was obtained, and the yellow powder solid was 2.71g with a yield of 80.9%.

[0066] The dried crude flame retardant was tightly wrapped with filter paper and transferred to a Soxhlet extractor with a reflux condenser. Acetone was used as a purification solvent. The temperature was raised to 65°C and refluxed for 3 hours. After drying, 2.63 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 97.04%.

[0067] like Figure 1-3 As shown in the figure, the peak position of the hydroxyl group newly appeared in the infrared spectrum of the flame retardant (3500cm -1 ) and P-Cl peak (550cm -1 ), the disappearance of the single peak of the P spectrum in the NMR spectrum, and the retention of the two raw material spectra in the hydrogen spectrum (the methylene double peak at 4.23ppm and the peak at the pyrimidine benzene ring at 8-9ppm) all confirmed the successful preparation of the flame retardant. The results showed that the structural formula of the flame retardant is:

[0068]

[0069] After GPC gel chromatography testing of the flame retardant, it was found that its molecular weight was maintained at 3000 to 4000. The decomposition temperature of the flame retardant was in the range of 250 to 350°C, and the maximum weight loss temperature was at 275°C, which has a beneficial effect on timely response to flame retardancy.

[0070] When the flame retardant is applied to flame retardant epoxy resin, when the addition amount is 0.5% to 2.5% of the mass of the epoxy resin, the vertical burning V-0 grade test can be achieved, and the flame retardant within this range has no damage to the mechanical properties of the material itself, and the tensile strength remains above 54.9MPa. With the increase of the amount of flame retardant, its oxygen index value can reach 31.8% at an addition amount of 2.5%, showing an excellent self-extinguishing effect, and excellent smoke suppression and heat insulation effects. After adding 1% of this flame retardant, the peak heat release rate can be reduced by 42.3%, the carbon dioxide production can be reduced by 32.5%, and the carbon monoxide production can be reduced by 38.3%, with an outstanding smoke suppression effect.

[0071] Embodiment 2:

[0072] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 250mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under vacuum conditions (-0.1MPa) until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 60°C and quickly add 92.4g (0.6mol) of newly distilled phosphorus oxychloride. After the system is stable (the time for this process is 2h), slowly increase the temperature to 105°C in a gradient manner, and react until no HCl gas is produced at the tail gas outlet (reaction is over). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and vacuum dry it at 105°C for 12h to obtain 38.6g of white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 90.8%.

[0073] The molar ratio of spirocyclic phosphate dichloride to 4,6-dihydroxypyrimidine was 1:1.1. Weigh 1.12g (0.011mol) of 4,6-dihydroxypyrimidine and add it to a 100mL three-necked flask. Connect the magnetic stirring, condenser and tail gas treatment device. Stir in 50mL acetone under nitrogen protection until it is clear and transparent. Add 2.97g (0.01mol) of spirocyclic phosphate dichloride, heat to 45℃ for 2h, further heat to 70℃, stir and reflux for 22h, filter the precipitate obtained by the reaction, wash it alternately with dichloromethane, ether and acetone three times, and dry it in a vacuum oven at 80℃ for 16h to obtain a crude flame retardant, 2.88g of yellow powder solid, with a yield of 85.9%.

[0074] The crude flame retardant after drying was tightly wrapped with filter paper and transferred to a Soxhlet extractor with a reflux condenser. Dichloromethane was used as a purification solvent, the temperature was raised to 55°C and refluxed for 6 hours. After drying, 2.76 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 98.83%.

[0075] The performance of the flame retardant is similar to that of Example 1.

[0076] Embodiment 3:

[0077] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 500mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under vacuum conditions (-0.1MPa) until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 55°C and quickly add 115.5g (0.75mol) of newly distilled phosphorus oxychloride. After the system is stable (this process takes 4h), slowly increase the temperature to 105°C in a gradient manner, and react until no HCl gas is produced at the tail gas outlet (reaction is over). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and vacuum dry it at 100°C for 12h to obtain 41.3g of a white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 92.8%.

[0078] The molar ratio of spirocyclic phosphate dichloride to 4,6-dihydroxypyrimidine is 1:1.2. 6.72g (0.06mol) of 4,6-dihydroxypyrimidine is weighed and added to a 250mL three-necked flask. The magnetic stirring, condenser and tail gas treatment device are connected. Stir in 100mL tetrahydrofuran under nitrogen protection until it is clear and transparent. 14.84g (0.05mol) of spirocyclic phosphate dichloride is ultrasonically dispersed in a beaker containing 80ml tetrahydrofuran for 30min, added to the three-necked flask and stirred evenly, 20ml of triethylamine is added and the temperature is raised to 45℃ for pre-reaction for 2h, and the temperature is further raised to 75℃ for reaction for 20h. The precipitate obtained by the reaction is filtered, and washed alternately with water, acetone and ether three times, and dried in a vacuum oven at 80℃ for 24h to obtain 15.15g of yellow-brown powder solid with a yield of 90.2%.

[0079] The crude flame retardant after drying was divided into three parts, tightly wrapped with multiple layers of filter paper, and transferred to a Soxhlet extractor with a reflux condenser. Anhydrous ethanol was used as a purification solvent. The temperature was raised to 80°C and refluxed for 8 hours. After drying, 14.72 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 97.16%.

[0080] The performance of the flame retardant is similar to that of Example 1.

[0081] Embodiment 4:

[0082] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 250mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under vacuum conditions (-0.1MPa) until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 60°C and quickly add 115.5g (0.75mol) of newly distilled phosphorus oxychloride. After the system is stable (the time of this process is 3h), slowly increase the temperature to 105°C gradually, and react until no HCl gas is produced at the tail gas outlet (reaction is over). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and vacuum dry it at 100°C for 12h to obtain 42.1g of white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 94.6%.

[0083] The molar ratio of spirocyclic phosphate dichloride to 4,6-dihydroxypyrimidine was 1:1.3, 24.7g (0.065mol) of 4,6-dihydroxypyrimidine was weighed, added to a 500mL three-necked flask, connected with magnetic stirring, condenser, and tail gas treatment device, and stirred in 200mL acetonitrile under nitrogen protection until clear and transparent. 14.84g (0.05mol) of spirocyclic phosphate dichloride was ultrasonically dispersed in a beaker containing 160ml tetrahydrofuran for 50min, added to the three-necked flask and stirred evenly, 28ml of triethylamine was added and heated to 50℃ for pre-reaction for 2h, and further heated to 80℃ for reaction for 24h, and the precipitate obtained by the reaction was filtered, washed alternately with water and ether acetone three times, and dried in a vacuum oven at 80℃ for 24h to obtain a crude flame retardant, 15.97g of yellow-brown powder solid, and a yield of 95.1%.

[0084] The crude flame retardant after drying was divided into three parts, tightly wrapped with multiple layers of filter paper, and transferred to a Soxhlet extractor with a reflux condenser. Tetrahydrofuran was used as a purification solvent, and the temperature was raised to 75°C and refluxed for 12 hours. After drying, 15.33 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 95.99%.

[0085] The performance of the flame retardant is similar to that of Example 1.

[0086] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.

Claims

1. A polymeric spirocyclic phosphorus nitrogen intumescent flame retardant, Features: The structural formula of the flame retardant is as follows: The repeating unit is C 9 O 8 N 2 H 10 P 2 , the degree of polymerization n is an integer of 8 to 12.

2. A polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 1, Features: The molecular weight of the flame retardant is 3000-4000.

3. A method for preparing the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 1 or 2, Features: The method steps include: Step 1: In a closed system without water or oxygen, add pentaerythritol to solvent A, stir until the system is evenly mixed, heat to temperature 1, add phosphorus oxychloride, introduce nitrogen and keep warm for 2 to 4 hours, then heat to temperature 2 and stir for 8 to 16 hours, wash and dry to obtain an intermediate spirocyclic phosphate dichloride; wherein the molar ratio of pentaerythritol to phosphorus oxychloride is 1:2 to 7; temperature 1 is 40 to 70° C., and temperature 2 is 80 to 120° C.; Step 2: In an anhydrous and oxygen-free environment, 4,6-dihydroxypyrimidine is added to solvent B, stirred until the solution is clear and transparent, the intermediate spirocyclic phosphate dichloride and the acid binding agent are added, pre-reacted at temperature 3 for 1 to 2 hours, then heated to temperature 4 and stirred and refluxed for 6 to 16 hours. After the reaction is completed, the crude flame retardant is washed and dried to obtain a yellow-brown powdery solid; wherein the molar ratio of 4,6-dihydroxypyrimidine to spirocyclic phosphate dichloride is 1:1 to 1.5, temperature 3 is 30 to 55° C., and temperature 4 is 60 to 100° C.; Step 3: Grind the crude flame retardant, reflux and purify it, and then dry it to obtain a polymeric spirocyclic phosphorus nitrogen expansion flame retardant.

4. A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 3, Features: In step 1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:3-5.

5. A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 3, Features: In step 1, the stirring rate is 220-300 rpm; the flow rate of nitrogen is 5-20 mL / min; temperature 1 is 55-65° C.; and temperature 2 is 90-110° C.

6. A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 3, Features: In step 1, the solvent A is one or more of anhydrous acetonitrile, acetone, dichloromethane and dioxane; and one or more of acetone, chloroform and dichloromethane are used for washing.

7. A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 3, Features: In step 2, the acid-binding agent is one or more of triethylamine, cerium chloride, anhydrous potassium carbonate and pyridine; the molar ratio of 4,6-dihydroxypyrimidine to the acid-binding agent is 1:1.5-2.

2. Temperature 4 is 70-85°C.

8. A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 3, Features: In step 2, the solvent B is one or more of acetone, tetrahydrofuran, xylene, anhydrous acetonitrile and N,N-dimethylformamide; and the washing is carried out using one or more of deionized water, ether, anhydrous methanol, anhydrous ethanol, dichloromethane and acetonitrile.

9. A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 3, Features: In step 3, during reflux purification, the solvent is one or more of acetone, dichloromethane, anhydrous ethanol and tetrahydrofuran; the temperature is 60-90° C., and the cooling reflux is performed for 3-12 hours.

10. A method for preparing a polymeric spirocyclic phosphorus nitrogen intumescent flame retardant as claimed in claim 3, Features: In step 1, step 2 and step 3, during drying, vacuum drying is performed at 80-100° C. for 12-24 hours.

Citation Information

Patent Citations

  • Flame retarder comprising condensed phosphonic acid ester and flame-retardant resin composition

    CN103703070A

  • Phosphaphenanthrene compound and preparation method and application thereof

    CN108864193A

  • Polymeric intumescent flame retardant and preparation method thereof

    CN109096492A

  • Method for recovering phosphorus oxychloride in chlorination reaction of hydroxyl-containing compound

    CN114455557A

Cited By

  • Corrosion-resistant coating and application thereof in aluminum alloy heat exchange tube

    CN120775464A

  • Corrosion resistant coating and its use in aluminium alloy heat exchanger tubes

    CN120775464B

  • Flame-retardant polyolefin cable material and preparation method thereof

    CN121136278A

  • Flame-retardant degradable epoxy resin containing phosphate structure and preparation method of flame-retardant degradable epoxy resin

    CN122502616A