A manganese-oxidizing microalgae-carbon-based PMS catalyst and its preparation method and application
By combining manganese oxidizing microalgae with carbon-based materials, a natural manganese-doped biochar-based PMS catalyst is prepared, which solves the problems of high cost and dissolution pollution of manganese-based catalysts in the existing technology, achieves efficient degradation of organic pollutants and reduces production costs.
Patent Information
- Application Number
- CN202311432349.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-10-31
AI Technical Summary
Existing manganese-based PMS catalysts have high synthesis costs, complex production processes, and can easily lead to secondary pollution caused by dissolution of metal ions, which limits their application in water treatment.
The PMS catalyst is prepared by combining manganese oxidized microalgae with carbon-based materials, using artificially cultured or sewage-treated microalgae biochar, and using a two-step calcination method to form a natural manganese-doped biochar-based catalyst, simplifying the process and reducing costs.
It achieves efficient degradation of organic pollutants, especially refractory pharmaceutical pollutants, and the catalyst has good reusability and low production cost, avoiding secondary pollution caused by dissolution of metal ions.
Smart Images

Figure CN117443372B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PMS (permonosulfate) catalysts, and specifically relates to a manganese-oxidized microalgae-carbon-based PMS catalyst and a preparation method and application thereof. Background Art
[0002] In recent years, how to effectively degrade and remove pharmaceutical pollutants before they enter the environment and prevent water pollution has become a research hotspot in various fields. Among the many water treatment technologies, advanced oxidation technology is widely used to remove various types of difficult-to-degrade organic pollutants due to its high oxidation capacity, mild reaction conditions, good removal effect and short reaction time. Among them, the advanced oxidation technology using peroxymonosulfate (PMS) as an oxidant has significant advantages such as good water solubility, easy storage and transportation, and strong oxidation capacity, and is widely studied and applied.
[0003] PMS itself has limited ability to oxidize organic pollutants. It must rely on external substances and energy to activate and produce oxidative free radicals in order to effectively oxidize and degrade organic pollutants. At present, the main methods for activating PMS are to use external energy such as heat, ultrasound or light, and to use materials such as transition metals and their oxides as catalysts to activate PMS to produce various free radicals. Among them, the use of various catalysts to activate PMS has the characteristics of high activation efficiency and low energy consumption, and has been widely studied and applied.
[0004] Among the many PMS catalysts, manganese-based materials and carbon-based materials have significant advantages. For example, compared with other transition metal materials, manganese-based materials have the advantages of abundant reserves and low toxicity. However, the existing chemically prepared manganese-based materials have the problems of high synthesis cost, easy aggregation to reduce the catalytic effect, and secondary pollution caused by metal ion dissolution, which limits their application. Although carbon-based materials can effectively overcome the secondary pollution problem caused by the dissolution of metal ions in metal catalysts, they also have a large specific surface area to promote the adsorption and aggregation of pollutants, thereby effectively improving the PMS activation and degradation effect of pollutants. However, the existing carbon-based materials are mainly obtained by various types of loading doping modifications based on graphene, graphene oxide and biochar. The production process is complicated, the production cost is high, and it is difficult to apply on a large scale.
[0005] Studies have shown that loading manganese oxide on various carbon-based materials to prepare PMS catalysts can produce a synergistic effect and greatly enhance the activation effect of PMS. For example, the catalyst obtained by loading nano-needle-shaped manganese dioxide on graphene oxide can greatly improve the activation effect of PMS and has a high removal effect on norfloxacin.
[0006] In the existing research on preparing PMS catalysts by loading manganese oxides on carbon-based materials, although the obtained catalysts have the characteristics of good catalytic effect, high recycling efficiency, and low toxic metal ion dissolution, their synthesis methods are mainly carried out by chemical synthesis, and their preparation process is complicated and the production cost is high, which undoubtedly limits their development and application. Therefore, it is necessary to develop a new PMS catalyst with a simple production process and low cost. Summary of the invention
[0007] At least in order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a manganese oxidizing microalgae-carbon-based PMS catalyst and a preparation method and application thereof.
[0008] The present invention adopts the following technical solution.
[0009] A manganese oxidizing microalgae-carbon-based PMS catalyst, the raw materials of which include manganese oxidizing microalgae, 2+ of liquid culture medium.
[0010] As a preferred solution, the microalgae concentration (dry weight) is 500 mg / L, and the manganese-oxidizing microalgae mother liquid is inoculated at an inoculation ratio of 5% into 2L of Mn-containing 2+ The culture conditions were set as follows: light-dark ratio 12h:12h, culture temperature 25°C, light intensity 5000Lux, and aeration volume 2L / min.
[0011] As a preferred embodiment, the manganese oxidizing microalgae refers to microalgae that has the ability to oxidize low-valent manganese to high-valent manganese, that is, microalgae that can convert Mn(II) into Mn(III) and Mn(IV) oxides.
[0012] The preparation method of the manganese oxidizing microalgae-carbon-based PMS catalyst in the present invention comprises the following steps:
[0013] Step 1: Manganese oxidizing microalgae in Mn 2+ Cultivating in a culture medium with a concentration of 0.1-5 mM until manganese oxidation is complete, then performing solid-liquid separation to obtain a mixture of algae and biological manganese oxides;
[0014] Step 2, drying the obtained mixture and grinding it into a powder of 20±10 mesh;
[0015] Step 3, calcining the obtained powder and grinding it into a manganese oxide microalgae-carbon-based PMS catalyst with a particle size of 50-150 mesh.
[0016] As a preferred solution, the calcination process is: firstly anaerobic calcination is carried out in the manner of "temperature rise 10°C / min—850°C for 3h—cooling to room temperature", and then calcination is carried out in the air in the manner of "temperature rise 10°C / min—350°C for 3h—cooling to room temperature".
[0017] As a preferred embodiment, the temperature during the drying process in step 2 is controlled at 60±3°C.
[0018] In the present invention, the manganese-oxidizing microalgae-carbon-based PMS catalyst is used to degrade carbamazepine.
[0019] As a preferred embodiment, when the concentration of carbamazepine is 5 mg / L, the dosage of the manganese-oxidized microalgae-carbon-based PMS catalyst is controlled to be 0.4 g / L, the PMS concentration is controlled to be 1 mmol / L, and the pH is controlled to be 7.
[0020] Beneficial effects: The present invention can utilize artificially cultivated manganese-oxidizing microalgae or manganese-oxidizing microalgae after sewage treatment, and through simple solid-liquid separation, drying and calcination, thereby realizing step-by-step high-temperature pyrolysis to form a natural manganese-doped biochar-based PMS catalyst. The preparation process of this scheme is simple and easy to operate, and the raw materials can be derived from manganese-oxidizing microalgae grown after sewage treatment, realizing waste resource utilization and reducing production costs.
[0021] In the present invention, the biological manganese oxide produced by manganese-oxidizing microalgae is naturally and evenly distributed on the surface of microalgae biochar, and the porous structure of microalgae biochar can play a role in fixing and dispersing biological manganese oxide, preventing manganese oxide from aggregating and reducing the catalytic effect, while reducing the reduction in catalyst activity and the dissolution of ions caused by the loss of manganese elements to produce secondary pollution. In the process of catalyst catalyzing PMS to degrade organic pollutants, microalgae biochar can produce synergistic effects with biological manganese oxide, greatly enhancing the catalytic efficiency of PMS and the degradation effect of organic pollutants, especially microalgae biochar can provide more effective adsorption and reaction active sites, promote PMS activation to produce free radicals, and adsorb and concentrate organic pollutants into the gaps for oxidative degradation. In addition, biological manganese oxide is naturally loaded on microalgae biochar, increasing its density, which is conducive to the recovery and reuse of the catalyst.
[0022] The present invention utilizes manganese-oxidizing microalgae and biological manganese oxides generated in situ, and obtains a natural manganese-doped biochar-based PMS catalyst simply through a two-step calcination method. No external chemical reagents are required during the preparation process, and the resource utilization of microalgae after sewage treatment and the low-cost acquisition of PMS catalysts are simultaneously achieved. The present invention utilizes manganese-oxidizing microalgae and biological manganese oxides generated in situ as raw materials, and obtains a natural manganese-doped biochar-based catalyst through a simple anaerobic high-temperature cracking process. The raw materials for the production of the catalyst can be derived from manganese-oxidizing microalgae after sewage treatment. The raw materials are easy to obtain and the resource recycling of microalgae after sewage treatment can be achieved. The production process does not use any toxic and harmful raw materials or auxiliary materials, the process is simple, and the production cost is low. At the same time, the prepared PMS catalyst has a good PMS catalytic effect and good repeated use stability, and is expected to be widely used in the catalytic oxidation of difficult-to-degrade organic matter, especially difficult-to-degrade organic drugs.
[0023] The manganese-oxidized microalgae-carbon-based PMS catalyst obtained by the present invention can efficiently degrade carbamazepine, a difficult-to-degrade organic pharmaceutical pollutant in water. The degradation efficiency of the catalyst for 5 mg / L carbamazepine can reach 100% within 10 minutes. Through simple precipitation recovery, the degradation efficiency of carbamazepine can still reach more than 95% after 5 cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The microalgae and biological manganese oxide mixture powder in Example 1;
[0025] Figure 2 This is a physical picture of the manganese-oxidized microalgae-carbon-based PMS catalyst prepared in Example 1;
[0026] Figure 3 This is a surface morphology of the manganese-oxidizing microalgae-carbon-based PMS catalyst prepared in Example 1;
[0027] Figure 4 The effect diagram of the degradation of carbamazepine by PMS catalyzed by the manganese-oxidizing microalgae-carbon-based PMS catalyst with different concentrations in Example 1;
[0028] Figure 5 This is a graph showing the variation of carbamazepine degradation efficiency with cycle number in Example 1. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] A method for preparing a manganese-oxidizing microalgae-carbon-based PMS catalyst, comprising the following steps:
[0032] Step 1: Manganese oxidizing microalgae (inoculation amount of 5%) was added to the 2+ The culture medium (2 L) with a concentration of 3 mM was cultured until the manganese oxidation was completed, and then solid-liquid separation was performed to obtain a mixture of algae and biological manganese oxides (such as Figure 1 As shown); wherein, the solid-liquid separation is specifically carried out by centrifugal separation, with a rotation speed of 4000 rpm and a time of 10 min; the basis for determining the completion of manganese oxidation is that the Mn2+ contained in the culture medium is less than 0.1 mM;
[0033] Step 2, drying the obtained mixture at 60±3°C and grinding it into a powder of 20±10 mesh;
[0034] Step 3, the obtained powder is calcined and then ground into a manganese oxide microalgae-carbon-based PMS catalyst (such as Figure 2 shown);
[0035] The calcination process is as follows: firstly, anaerobic calcination is performed in the manner of "temperature rise of 10°C / min—maintaining at 850°C for 3h—cooling to room temperature 25°C", and then calcination is performed in the manner of "temperature rise of 10°C / min—maintaining at 350°C for 3h—cooling to room temperature 25°C" in air.
[0036] The manganese-oxidized microalgae-carbon-based PMS catalyst obtained in this example was subjected to electron microscopy scanning detection, and the results were as follows: Figure 3 As shown in the surface morphology diagram, manganese oxide is relatively evenly loaded on the surface and in the voids of the algae-based biochar.
[0037] Example 2
[0038] A method for preparing a manganese-oxidizing microalgae-carbon-based PMS catalyst, comprising the following steps:
[0039] Step 1: Manganese oxidizing microalgae (inoculation amount of 5%) was added to the 2+ The culture medium (2 L) with a concentration of 1 mM was cultured until the manganese oxidation was completed, and then the solid-liquid separation was performed to obtain a mixture of algae and biological manganese oxide (such as Figure 1 shown);
[0040] Step 2, drying the obtained mixture at 60±3°C and grinding it into a powder of 20±10 mesh;
[0041] Step 3, the obtained powder is calcined and then ground into a manganese oxide microalgae-carbon-based PMS catalyst (such as Figure 2 shown);
[0042] The calcination process is as follows: firstly, anaerobic calcination is performed in the manner of "temperature rise 10°C / min—850°C for 3.2h—cooling to room temperature 25°C", and then calcination is performed in the air in the manner of "temperature rise 10°C / min—350°C for 3h—cooling to room temperature 25°C".
[0043] Example 3
[0044] A method for preparing a manganese-oxidizing microalgae-carbon-based PMS catalyst, comprising the following steps:
[0045] Step 1: Manganese oxidizing microalgae (inoculation amount 5%) were added to the 2+ The culture medium (2 L) with a concentration of 5 mM was cultured until the manganese oxidation was completed, and then solid-liquid separation was performed to obtain a mixture of algae and biological manganese oxides (such as Figure 1 shown);
[0046] Step 2, drying the obtained mixture at 60±3°C and grinding it into a powder of 20±10 mesh;
[0047] Step 3, the obtained powder is calcined and then ground into a manganese oxide microalgae-carbon-based PMS catalyst (such as Figure 2 shown);
[0048] The calcination process is as follows: firstly, anaerobic calcination is performed in the manner of "temperature rise of 10°C / min—maintaining at 850°C for 3h—cooling to room temperature 25°C", and then calcination is performed in the manner of "temperature rise of 10°C / min—maintaining at 350°C for 3h—cooling to room temperature 25°C" in air.
[0049] Example 4
[0050] In Example 1, the manganese-oxidized microalgae-carbon-based PMS catalyst was used to degrade carbamazepine. Specifically, when the concentration of carbamazepine was controlled to 5 mg / L, the amount of the manganese-oxidized microalgae-carbon-based PMS catalyst was controlled to 0.4 g / L, the PMS concentration was controlled to 1 mmol / L, and the pH was controlled to 7. The results showed that carbamazepine could be completely degraded within 10 minutes. Figure 4 and 5 When the dosage of manganese-oxidizing microalgae-carbon-based PMS catalyst was controlled at 0.3 g / L, 0.2 g / L, and 0.1 g / L, the degradation effect of carbamazepine was as shown in Figure 2. Figure 4 As shown, when the dosage of manganese-oxidized microalgae-carbon-based PMS catalyst was controlled at 0.3 g / L and 0.2 g / L respectively, carbamazepine could still be completely degraded within 10 minutes.
[0051] Example 5
[0052] The waste liquid in Example 4 was centrifuged (4000 rpm, 10 min), and the manganese-oxidized microalgae-carbon-based PMS catalyst was recovered. Carbamazepine was degraded again according to the parameters in Example 4. The results showed that 99.2% of carbamazepine could be degraded within 10 min. Figure 5 shown.
[0053] Example 6
[0054] The waste liquid in Example 5 was centrifuged (4000 rpm, 10 min), and the manganese-oxidized microalgae-carbon-based PMS catalyst was recovered. Carbamazepine was degraded again according to the parameters in Example 4. The results showed that 98.7% of carbamazepine could be degraded within 10 min. Figure 5 shown.
[0055] Example 7
[0056] The waste liquid in Example 6 was centrifuged (4000 rpm, 10 min), and the manganese-oxidized microalgae-carbon-based PMS catalyst was recovered. Carbamazepine was degraded again according to the parameters in Example 4. The results showed that 97.5% of carbamazepine could be degraded within 10 min. Figure 5 shown.
[0057] Example 8
[0058] The waste liquid in Example 7 was centrifuged (4000 rpm, 10 min), and the manganese-oxidized microalgae-carbon-based PMS catalyst was recovered. Carbamazepine was degraded again according to the parameters in Example 4. The results showed that 96.8% of carbamazepine could be degraded within 10 min. Figure 5 shown.
Claims
1. A method for preparing a manganese-oxidized microalgae-carbon-based PMS catalyst, characterized in that the steps include: Step 1: Manganese oxidizing microalgae in Mn 2+ Cultivating in a culture medium with a concentration of 0.1-5 mM until manganese oxidation is complete, followed by solid-liquid separation to obtain a mixture of algae and biological manganese oxide; Step 2, drying the obtained mixture and grinding it into a 20±10 mesh powder; Step 3, calcining the obtained powder and then grinding it into a manganese oxide microalgae-carbon-based PMS catalyst with a particle size of 50-150 mesh; Manganese oxidizing microalgae uses a manganese oxidizing microalgae mother solution with a dry weight of 500 mg / L, containing Mn 2+ The amount of liquid culture medium used is 2 L; manganese oxidizing microalgae refers to microalgae that has the ability to oxidize low-valent manganese to high-valent manganese, that is, microalgae that can convert Mn (II) into Mn (III) and Mn (IV) oxides; The calcination process is as follows: first, anaerobic calcination is carried out in the manner of "temperature rise of 10°C / min—850°C, holding for 3 hours—cooling to room temperature", and then calcination is carried out in air in the manner of "temperature rise of 10°C / min—350°C, holding for 3 hours—cooling to room temperature".
2. The preparation method according to claim 1, wherein: The temperature during the drying process in step 2 was controlled at 60±3°C.
3. Use of the manganese-oxidizing microalgae-carbon-based PMS catalyst prepared by the method of claim 1 or 2, characterized in that: The manganese-oxidizing microalgae-carbon-based PMS catalyst is used for degrading carbamazepine.
4. The use according to claim 3, characterized in that: When the concentration of carbamazepine is 5 mg / L, the dosage of the manganese-oxidizing microalgae-carbon-based PMS catalyst is controlled to be 0.4 g / L, the PMS concentration is controlled to be 1 mmol / L, and the pH is controlled to be 7.