Preparation method of composite material, composite plate and cryogenic storage tank
By adopting negative pressure and pressurization treatment steps in the preparation of composite materials, the impregnated solution penetrates into the material unit evenly and forms a dense protective layer, which solves the problem of heat cracking of composite materials in high-temperature environments, and improves toughness and thermal insulation performance. Extend service life.
Patent Information
- Application Number
- CN202311388209.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-10-23
AI Technical Summary
During the transportation of low-temperature storage tanks, the insulation support blocks are heat-cracked due to high temperature environment, and have poor toughness and need to be replaced frequently, which affects the thermal insulation and safety performance.
The composite material preparation method is adopted to prepare negative pressure treatment, impregnation treatment, pressurization treatment, drying treatment, balance treatment, embryo composition treatment, hot press treatment and multi-stage cooling and pressure reduction treatment. The negative pressure and pressurization operations in the vacuum container are used to make The impregnation solution penetrates into the material unit evenly, forming a dense protective layer, eliminating stress in the embryo and improving the glue strength and toughness.
Improves the toughness and thermal insulation properties of composite materials, prevents heat cracking in high temperature environments, extends service life, and reduces repair and replacement costs.
Smart Images

Figure CN117445446B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to a preparation method of a composite material, a composite plate and a low-temperature storage tank. Background Art
[0002] The composite material is made by fully immersing the material unit in a synthetic resin solution so that the resin penetrates into the material unit. After that, the material unit is dried to remove moisture. Finally, the material unit is heated to solidify the resin to form a water-insoluble polymer. The composite material has insulation and cold-insulating properties, heat-insulating properties at ultra-low temperatures of -220°C, high strength, high weather resistance, high wear resistance and high density. Its preparation process is complex and requires sophisticated equipment.
[0003] Because the composite material has ultra-low temperature insulation performance, it can be used in the field of ships and cryogenic storage tanks. Specifically, it can be used in the insulation support block in contact with the cryogenic storage tank. When the cryogenic storage tank contains and transports cryogenic liquids such as liquefied gas, LNG, LPG, ethylene, etc., the insulation support block can isolate the cold of the cryogenic liquid in the tank from being transferred to the outside world, thereby improving the cold preservation efficiency of the cryogenic storage tank.
[0004] However, the composite materials in the related art have large internal stress and low toughness after manufacturing. When the low-temperature storage tank is transported empty, the temperature of the tank gradually rises after the sunlight shines on the tank. When the temperature of the tank rises to a certain level, the insulation support block will be cracked by the heat, causing the insulation support block to be damaged and need to be replaced to ensure the safety and insulation performance of the low-temperature storage tank. Summary of the invention
[0005] The purpose of the present application is to provide a method for preparing a composite material having ultra-low temperature thermal insulation performance and high toughness, a composite plate and a cryogenic storage tank.
[0006] In order to solve the above technical problems, this application adopts the following technical solutions:
[0007] According to one aspect of the present application, the present application provides a method for preparing a composite material, which is used for processing a material unit, and includes negative pressure treatment, pressurization treatment, cleaning treatment, drying, balancing treatment, embryo processing, hot pressing treatment and multi-stage cooling and pressure reduction treatment; negative pressure treatment, the material unit is placed in a vacuum container, and the vacuum container is evacuated to reach a negative pressure state; impregnation treatment, after the negative pressure treatment, the vacuum container maintains a negative pressure state, and then an impregnation solution is injected into the vacuum container so that the impregnation solution penetrates into the material unit; pressure treatment, after the impregnation treatment, the vacuum container is pressurized so that the impregnation solution quickly diffuses in the material unit, and then the residual liquid in the vacuum container is emptied. The remaining impregnation solution; cleaning treatment, after the pressurization treatment, the vacuum container is evacuated to reach a negative pressure state, so that the residual impregnation solution on the outer surface of the material unit quickly drips into the vacuum container, and then the material unit is taken out of the vacuum container; drying and balancing treatment, the taken out material unit is first dried, and then balanced after drying; embryo assembly treatment, stacking multiple material units after balancing treatment to form an embryo body; hot pressing treatment, hot pressing the embryo body to solidify the embryo body; multi-stage cooling and pressure reduction treatment, multi-stage cooling and pressure reduction of the embryo body after hot pressing and solidification to eliminate the stress in the embryo body and ensure the bonding strength of multiple material units.
[0008] In some embodiments, the hot pressing treatment includes a low-pressure preheating stage and a hot pressing curing stage: in the low-pressure preheating stage, the embryo body is gradually heated up to melt and flow the impregnation solution in the embryo body, thereby ensuring that the impregnation solution in the embryo body is evenly distributed; in the hot pressing curing stage, the embryo body after the preheating treatment is gradually heated up and pressed, and during the hot pressing process, the impregnation solution adheres to the embryo body without overflowing, and multiple material units are bonded to each other, and the impregnation solution is cured.
[0009] In some embodiments, a secondary composite molding process is further included, wherein a plurality of the embryos are stacked, aerogel is coated on the facing sides of two adjacent embryos, and then the plurality of embryos are pressurized and composited to form the composite material.
[0010] In some embodiments, the low-pressure preheating stage includes two-stage heating, the temperature range of the first stage heating includes 50°C to 80°C, and the heating time includes 0.5min / mm to 3min / mm according to the thickness of the embryo; the temperature range of the second stage heating includes 70°C to 100°C, and the heating time includes 0.5min / mm to 3min / mm according to the thickness of the embryo; the hot pressing curing stage includes three-stage hot pressing, the temperature range of the first stage hot pressing includes 100°C to 120°C, and the pressure range includes 4kg / cm 2 ~12kg / cm2 The hot pressing time is 2 min / mm to 5 min / mm according to the thickness of the embryo; the temperature range of the second stage hot pressing is 120°C to 140°C, and the pressure is 50 kg / cm 2 ~120kg / cm 2 The hot pressing time is 2 min / mm to 5 min / mm according to the thickness of the embryo; the temperature range of the third stage hot pressing is 120°C to 140°C, and the pressure is 60 kg / cm 2 ~120kg / cm 2 The hot pressing time is 2 min / mm to 5 min / mm according to the thickness of the embryo; the multi-stage cooling and pressure reduction treatment includes five stages of cooling and pressure reduction, the temperature range of the first stage of cooling and pressure reduction includes 90°C to 110°C, and the pressure includes 60 kg / cm 2 ~120kg / cm 2 The cooling time is 3min / mm to 8min / mm according to the thickness of the embryo; the temperature range of the second stage cooling and pressure reduction is 50℃ to 80℃, and the pressure is 60kg / cm 2 ~120kg / cm 2 The cooling time is 3min / mm to 8min / mm according to the thickness of the embryo; the temperature range of the third stage cooling and pressure reduction is 30℃ to 70℃, and the pressure is 15kg / cm2 to 45kg / cm 2 The cooling time is 3min / mm to 8min / mm according to the thickness of the embryo; the temperature range of the fourth stage cooling and pressure reduction is 20℃ to 50℃, and the pressure is 10kg / cm 2 ~30kg / cm 2 The cooling time is 3min / mm to 8min / mm according to the thickness of the embryo; the temperature range of the fifth stage cooling and pressure reduction is 20℃ to 35℃, and the pressure is 4kg / cm 2 ~15kg / cm 2 The cooling time is 3 min / mm to 8 min / mm according to the thickness of the embryo.
[0011] In some embodiments, the vacuum degree of the material unit during negative pressure treatment is maintained at 0.04Mpa~0.09Mpa, and the negative pressure time is 0.5h~1.5h; the vacuum degree of the immersion treatment is maintained at 0.04Mpa~0.09Mpa, and the immersion time is 1h~12h; the pressure of the pressurized treatment is 0.5Mpa~1.2Mpa, and the pressurized time is 1h~6h; the vacuum of the cleaning treatment is 8h~100h, and the moisture content of the material unit is 10%~15%.
[0012] In some embodiments, the cleaning process further includes a glue dripping process. After the material unit is taken out from the vacuum container, it is placed on a rack, and the glue dripping time includes 0.5h to 3h.
[0013] In some embodiments, the material unit is made of at least one of bamboo, wood, reed, non-woven fabric or paper.
[0014] A composite board, comprising: the composite board comprises a composite material board, and the composite material board is prepared by any of the preparation methods described above.
[0015] In some embodiments, the composite material board can be bonded with at least one of a wood board, a bamboo board, a bamboo-wood composite board, a plastic-wood composite board, a fiber-reinforced material, an impregnated paper, and a high-pressure laminate to form the composite board by hot pressing.
[0016] A low-temperature storage tank comprises: a tank body, a support frame and a plurality of support blocks; the tank body is used to store low-temperature liquid; the support frame is arranged on the circumference of the tank body to support the tank body; a plurality of support blocks are located between the tank body and the support frame, and the plurality of support blocks are arranged along the circumference of the tank body to prevent the cold of the tank body from being transferred to the support frame, and the support blocks are made of any of the composite plates described above.
[0017] In some embodiments, the support block is provided with a receiving groove on a side surface of the tank body, and the receiving groove extends along the axial direction of the storage tank; the tank body is provided with a protrusion relative to the receiving groove, and the protrusion is engaged in the receiving groove; the inner wall of the receiving groove is coated with aerogel to form an aerogel layer, and the aerogel layer is bonded to the inner wall of the receiving groove and the protrusion.
[0018] It can be seen from the above technical solution that the present application has at least the following advantages and positive effects:
[0019] In the present application, the material unit is subjected to negative pressure treatment so that the gas in the material unit is extracted, and then the impregnation solution is injected into the vacuum container so that the impregnation solution penetrates into the material unit. After the impregnation treatment, a pressurization treatment is performed so that the impregnation solution quickly penetrates into the material unit, and the impregnation solution is homogenized in the material unit, so that the gaps between the cell walls in the material unit are fully infiltrated with the impregnation solution. The material unit is increased in volume and the structural strength of the material unit is improved. After the pressurization is completed, a secondary negative pressure is applied in the vacuum container so that the impregnation solution remaining on the surface of the material unit falls off quickly. After the pressurization treatment, the material unit is taken out for drying, balancing, embryo assembly and hot pressing, so that the impregnation solution on the material unit forms a dense protective layer, improving the strength, weather resistance, wear resistance, insulation function and thermal insulation performance of the material unit. After the embryo body is hot pressed, a multi-stage cooling and pressure reduction treatment is performed to eliminate the stress in the embryo body and ensure the bonding strength of multiple material units, thereby effectively improving the toughness of the composite material. The composite material prepared by this composite material preparation method, when applied to fields such as low-temperature storage tanks, can effectively ensure the low-temperature thermal insulation performance of the composite material while preventing the composite material from being cracked by heat in a high-temperature environment, thereby ensuring the toughness of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a structural schematic diagram of the low-temperature storage tank of the present invention.
[0021] Figure 2 It is a schematic flow chart of steps S100 to S800 of the method for preparing the composite material of the present invention.
[0022] Figure 3 It is a schematic flow chart of step S710 to step S720 of the preparation method of the present invention.
[0023] Figure 4 It is a schematic flow chart of steps S711 to S723 of the preparation method of the present invention.
[0024] Figure 5 It is a schematic flow chart of steps S810 to S850 of the preparation method of the present invention.
[0025] Figure 6 It is a schematic flow chart of step S900 of the preparation method of the present invention.
[0026] Figure 7 It is a schematic flow chart of step S420 of the preparation method of the present invention.
[0027] Figure 8 It is a supporting block made of the composite board material of the present invention.
[0028] Fig. 9 The invention relates to a connecting piece structure made of a composite plate material.
[0029] Fig.10 It is a partial plane cross-sectional view of the cryogenic storage tank of the present invention perpendicular to its axial direction.
[0030] The reference numerals are described as follows: 100, tank body; 200, support frame; 300, support block; 400, connecting piece. DETAILED DESCRIPTION
[0031] Typical implementations that embody the features and advantages of the present application will be described in detail in the following description. It should be understood that the present application can have various changes in different implementations without departing from the scope of the present application, and the descriptions and illustrations therein are essentially used for illustrative purposes rather than for limiting the present application.
[0032] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0033] At present, there are composite materials on the market with insulation properties and ultra-low temperature thermal insulation properties below -220°C. They are generally used in manufacturing fields such as ships and cryogenic storage tanks. They are high-tech products with high safety factors used in high-risk environments and have very strict quality control standards.
[0034] In the relevant technology, Germany uses the very abundant beech, maple and birch resources in European countries to prepare related composite materials. Since beech and other woods are tall, hard and have coarse fibers, beech and other woods can form high-strength, high-wear-resistant and high-cold-insulating composite materials after relevant drying, impregnation and hot pressing curing treatments.
[0035] The material units used in the composite material preparation method of the present application are no longer limited to European beech, maple, birch and other tall wood resources, and the applicable fields are increased to ordinary bamboo, wood and other fields. On the one hand, the material sources of the composite materials are greatly improved, and there is no need to specially import European beech, maple, birch and other woods, thereby reducing the production cost of the composite materials. On the other hand, the produced composite materials can meet the relevant European and international standards. It is believed that in the near future, my country's national standards corresponding to impregnated laminated composite materials will also be formulated and implemented.
[0036] Figure 1 It is a structural schematic diagram of the low-temperature storage tank of the present invention.
[0037] See also Figure 1 In the related technology, the composite materials produced according to the related process in Germany have poor toughness and poor high temperature tolerance. When the composite material is applied to the cryogenic storage tank to form a support block, it can support and abut the tank body, and isolate the transfer of cold on the tank body. However, when the cryogenic storage tank is transported empty, the tank body 100 continues to heat up under the sun. When the temperature of the tank body 100 reaches a higher temperature, the side wall of the support block 300 that contacts the tank body 100 is easily cracked due to the heat, thereby affecting the cold insulation efficiency of the cryogenic storage tank and easily causing safety hazards. At the same time, according to relevant European and international standards, the cracked support block 300 will no longer be used on the cryogenic storage tank and needs to be replaced. The overall maintenance and replacement cost is high, which will cause great economic losses.
[0038] Figure 2 It is a schematic flow chart of steps S100 to S800 of the method for preparing the composite material of the present invention.
[0039] See also Figure 2 The present application provides a method for preparing a composite material, which is used for processing a material unit, and comprises the following steps:
[0040] S100, negative pressure treatment, placing the material unit into a vacuum container, and evacuating the vacuum container to achieve a negative pressure state.
[0041] S200, impregnation treatment. After the negative pressure treatment, the vacuum container is kept in a negative pressure state, and then the impregnation solution is injected into the vacuum container to allow the impregnation solution to penetrate into the material unit.
[0042] S300, pressurization treatment, pressurizing the vacuum container after the impregnation treatment to allow the impregnation solution to diffuse quickly in the material unit, and then emptying the residual impregnation solution in the vacuum container.
[0043] S400, cleaning treatment, after the pressurization treatment, the vacuum container is evacuated to reach a negative pressure state, so that the impregnation solution remaining on the outer surface of the material unit quickly drips into the vacuum container, and then the material unit is taken out of the vacuum container.
[0044] S500, drying and balancing treatment, the taken-out material unit is first subjected to drying treatment, and then subjected to balancing treatment after the drying treatment.
[0045] S600, embryo assembly processing, stacking the plurality of material units after the balancing processing to assemble the embryos to form an embryo body.
[0046] S700, heat pressing treatment, heat pressing the embryo to solidify the embryo.
[0047] S800, multi-stage cooling and pressure reduction treatment, the embryo body after heat pressing and curing is subjected to multi-stage cooling and pressure reduction to eliminate the stress in the embryo body and ensure the bonding strength of the plurality of material units.
[0048] When the composite material is prepared according to the above preparation method, the material unit is first placed in a vacuum container, and the vacuum container reaches a negative pressure state, thereby extracting the air in and between the cells of the material unit, so that the cells inside the material unit are also in a negative pressure state.
[0049] Then, an impregnation solution is injected into the vacuum container. After the impregnation solution submerges the material unit, it diffuses in the material unit and penetrates between the cell walls in the negative pressure state to increase the volume of the material unit. During the process of the impregnation solution penetrating into the material unit, a pressurization treatment is performed. The impregnation solution under high pressure further increases the speed of penetrating into the material unit and can make the impregnation solution evenly distributed in the material unit. After the impregnation solution fully penetrates into the material unit, the impregnation solution is emptied.
[0050] After the pressurization treatment, the vacuum container is evacuated again to make the vacuum container reach a negative pressure state, and a cleaning treatment is performed to make the impregnation solution on the material unit fall into the vacuum container, and then the material unit is taken out of the vacuum container.
[0051] After the material unit is taken out of the vacuum container, it is first dried to keep the material unit dry; then it is balanced to make the moisture content in each part of the material unit more uniform, thereby improving the stability, corrosion resistance and service life of the material unit.
[0052] Afterwards, the material units are subjected to an embryonic treatment and then to a hot pressing treatment. During the hot pressing process, the impregnation solution allows the multiple material units to be fully bonded, thereby improving the connection strength of the embryonic body.
[0053] After the embryo body is hot-pressed, a multi-stage cooling and pressure reduction process is performed to eliminate the stress in the embryo body and ensure the bonding strength of multiple material units, thereby effectively improving the toughness of the composite material. When the composite material prepared by this composite material preparation method is applied to low-temperature storage tanks and other fields, it can effectively ensure the low-temperature thermal insulation performance of the composite material while preventing the composite material from being heated and cracked in a high-temperature environment, thereby ensuring the toughness and strength of the composite material.
[0054] In addition, the impregnation solution solidifies inside the embryo during the hot pressing process. On the one hand, it effectively improves the strength of the cells in the material unit, thereby improving the strength, toughness, wear resistance and corrosion resistance of the embryo. On the other hand, the impregnation solution and the embryo form a dense laminated structure, which makes the embryo have extremely high cold insulation performance, and can further make the composite material have excellent corrosion resistance, water resistance, insulation, chemical stability and other properties. At the same time, its physical and mechanical properties such as wear resistance, impact resistance, and strength are also better than other composite materials on the market, and it also meets the relevant provisions of European and international standards.
[0055] In this embodiment, the material unit is in the form of a board, which is composed of at least one of bamboo, wood, reed bamboo, non-woven fabric or paper. The material unit can be a bamboo board made of bamboo, a wooden board made of wood or a reed bamboo board made of reed bamboo. The material unit can also be a board formed by mixing materials such as bamboo, wood, and reed bamboo. In the embryo assembly process, the embryo body can be formed by assembling the material units of a single material, or by mixing multiple single boards of different materials to form the embryo body.
[0056] In some embodiments, it also includes paper made from plant fiber materials, and multiple sheets of paper are stacked to form a single board.
[0057] In this embodiment, the impregnation solution includes a synthetic resin. The synthetic resin includes at least one of melamine-formaldehyde resin, phenolic resin, urea-formaldehyde resin, isocyanates, polycarboxylic acids, etc., which has a certain viscosity and is thermosetting. In some embodiments, the concentration of the synthetic resin can be selected according to different characteristics of the material unit so that the synthetic resin can fully penetrate between the cell walls in the material unit.
[0058] See also Figure 2 In this embodiment, in step S100, during the negative pressure treatment, after the material unit is placed in the vacuum container, the vacuum container is evacuated to reach a negative pressure state. The negative pressure state can extract the air in and between the material cells in the material unit, so as to facilitate the penetration of the impregnation solution into the cell walls during the subsequent impregnation treatment and pressurization treatment.
[0059] In some embodiments, the vacuum degree of the material unit during negative pressure treatment is maintained at 0.04Mpa to 0.09Mpa, and the negative pressure time is 0.5h to 1.5h. The vacuum degree and negative pressure time are selected according to the properties of different material units to fully extract the air in and between cells.
[0060] See also Figure 2 In this embodiment, in step S200, during the impregnation process, the vacuum container is continuously kept in a negative pressure state, and then the impregnation solution is injected into the vacuum container so that the material unit is immersed in the impregnation solution. At this time, the impregnation solution can penetrate between the cell walls of the material unit to facilitate the subsequent hot pressing curing process, which can improve the wear resistance, corrosion resistance, heat insulation and other properties of the material unit.
[0061] In some embodiments, the vacuum degree of the dipping process is maintained at 0.04Mpa to 0.09Mpa, and the dipping time is 1 hour to 12 hours. The vacuum degree and dipping time of the dipping process can be adaptively selected and adjusted according to the material and thickness of the material unit.
[0062] See also Figure 2 In this embodiment, in step S300, during the pressurization process, the vacuum container is pressurized to a high pressure state. The impregnation solution quickly penetrates into the material unit under the high pressure environment and quickly diffuses in the material unit. After the vacuum container is pressurized for a certain period of time and the impregnation solution fully penetrates into the material unit, the resin in the vacuum container is discharged to facilitate the subsequent cleaning process.
[0063] The pressure treatment improves the penetration efficiency of the impregnation solution, reduces the processing time, and improves the processing efficiency. In addition, the pressure treatment can also make the impregnation solution evenly distributed in the material unit, making the performance of each part of the material unit consistent and stable, and at the same time, facilitating the subsequent embryo processing.
[0064] In some embodiments, air is introduced into the vacuum container to pressurize the vacuum container so that the vacuum container is in a high-pressure state. In other embodiments, liquid is continuously introduced into the vacuum container to pressurize the vacuum container so that the vacuum container is in a high-pressure state. In other embodiments, an impregnation solution is continuously injected into the vacuum container.
[0065] In some embodiments, the pressure of the pressurization treatment is 0.5 MPa to 1.2 MPa, and the pressurization time is 1 hour to 6 hours. The pressure parameters and pressurization time of the pressurization treatment can be adaptively selected and adjusted according to the material and thickness of the material unit.
[0066] In other embodiments, the vacuum container is connected to the impregnation solution storage tank. On the one hand, it is convenient to inject the impregnation solution in the impregnation solution storage tank into the vacuum container. On the other hand, it is convenient for the impregnation solution in the vacuum container to flow back into the impregnation solution storage tank, so as to facilitate the repeated recycling of the impregnation solution and improve the utilization efficiency of resources.
[0067] In some embodiments, when the vacuum pressure impregnation solution is used, different impregnation solutions correspond to different vacuum degrees, which will produce a "foaming" phenomenon, which will hinder the penetration of the impregnation solution into the material, affecting the impregnation effect and insulation quality. To prevent the "foaming" phenomenon, the "foaming" vacuum degree of the impregnation resin needs to be measured, so in actual production, the impregnation vacuum degree is controlled before "foaming".
[0068] The material used in the technical solution of the present invention is very different from the beech, birch, maple, etc. used in the German solution in the related art. Beech and other woods are tall, and their toughness and strength are much stronger than those of ordinary trees. Therefore, the difficulty and requirements of the processing process of beech boards during the impregnation process are much less than those of ordinary trees.
[0069] After the improvement, the present invention can adopt common wood, bamboo, reed and other materials to form a single board, and then obtain a composite material that meets European and international standards through processes such as impregnation treatment.
[0070] For example, bamboo is used to make composite materials, because the cell wall of bamboo is relatively thin and contains a large number of pores compared to wood, while the cell wall of wood contains very few pores, or even almost no pores. This is because the lining fibers of the wood cell wall have many covalent bonds, and the amount of cellulose per unit volume is more than that of bamboo, so it is also denser. Therefore, the material used in the German solution is beech, which does not need to solve the problem that the cell wall of bamboo is thin and contains a large number of pores.
[0071] The impregnation effect of the material is evaluated by the material weight gain rate. W = (M1-M0) / M0*100%, where: W is the weight gain rate, M1 is the weight of the material after impregnation, and M0 is the weight of the material before impregnation.
[0072] After studying various fiber materials such as bamboo, wood, non-woven fabrics, paper, and herbaceous plants, the present invention has obtained the effects of vacuuming time, vacuum degree, glue concentration, preheating temperature, hot pressing temperature, multi-stage cooling temperature, pressing pressure, and pressing time on the impregnation effect in order to make the weight gain rate of bamboo reach EU and international standards. Therefore, the preparation method of the composite material of the present application can achieve the best impregnation effect of various materials and solve the impregnation process problem of different materials.
[0073] In some embodiments, the impregnation treatment and the pressurization treatment can be performed multiple times, which is determined according to factors such as the thickness of the cell wall of the material unit and the gap between cells, so that the impregnation solution can fully enter the cells and between the cells, thereby supporting the cells after the subsequent impregnation solution is solidified.
[0074] See also Figure 2 In this embodiment, in step S400, during the cleaning process, the vacuum container is evacuated again to reach a negative pressure state, so that the residual impregnation solution on the outer surface of the material unit quickly drips into the vacuum container. After the residual impregnation solution on the outer surface of the material unit drips into the vacuum container, the vacuum container is restored to a normal pressure state, so that the material unit can be easily taken out of the vacuum container.
[0075] In the cleaning process, on the one hand, under negative pressure, part of the impregnation solution inside the material unit is precipitated to the outer surface of the material unit, so that when the material unit is removed from the vacuum container and is in a normal pressure state, the impregnation solution inside the material unit is prevented from being precipitated to the outside due to pressure imbalance. On the other hand, the residual impregnation solution on the outer surface of the material unit quickly drips into the vacuum container, which is convenient for the recycling and reuse of the impregnation solution, and improves the cleaning efficiency of the material unit surface, can quickly empty the vacuum container, and is convenient for the vacuum container to process the next batch of material units, improves the utilization efficiency of the vacuum container, and thus improves the production efficiency of the composite material.
[0076] In some embodiments, the vacuum degree of the cleaning process is maintained at 0.04Mpa to 0.09Mpa, and the cleaning time is 10min to 40min. The vacuum degree parameters and cleaning time of the cleaning process can be adaptively selected and adjusted according to the material and thickness of the material unit.
[0077] In this embodiment, in step S500, during the drying and balancing process, after the material unit is taken out of the vacuum container, it is first dried to reduce the moisture content in the material unit. On the one hand, it can improve the corrosion resistance and weather resistance of the material unit. On the other hand, it makes the surface of the material unit dry and rough, improves the surface adhesion of adjacent material units during the assembly and hot pressing and curing process, and can improve the connection strength of the hot pressing and curing embryo. Then, the balancing process is performed again, and the dried material unit is placed in a certain temperature and humidity environment and left to stand for a certain period of time to make the moisture content of the material unit more uniform, thereby achieving the health of the material unit and improving the stability of the quality of the material unit. After drying and balancing, the moisture content of the material unit is 10% to 15%.
[0078] In some embodiments, the temperature range of the drying process includes 25° C. to 80° C., and the drying time includes 4.8 hours to 96 hours. The drying time of the drying process can be adaptively selected and adjusted according to parameters such as the material, thickness, and cell gap of the material unit.
[0079] In some embodiments, when the material unit is wood, the drying temperature range includes 40°C to 70°C, and the drying time includes 4.8 hours to 96 hours. When the material unit is bamboo, the drying temperature range includes 30°C to 70°C, and the drying time includes 12 hours to 96 hours.
[0080] In some embodiments, the temperature range of the balancing treatment includes 16°C to 60°C, the balancing time includes 40h to 384h, and the relative humidity of the environment is 50% to 80%. The balancing time of the balancing treatment can be adaptively selected and adjusted according to parameters such as the material, thickness, and cell gap of the material unit.
[0081] In some embodiments, when the material unit is wood, the equilibrium temperature range includes 18°C to 50°C, and the equilibrium time includes 48h to 384h. When the material unit is bamboo, the equilibrium temperature range includes 18°C to 40°C, and the equilibrium time includes 48h to 384h.
[0082] See also Figure 2 In this embodiment, in step S600, during the embryo assembly process, multiple material units are stacked to form an embryo body, so as to facilitate subsequent hot pressing. In some embodiments, adjacent material units can be assembled with parallel, staggered or tangential texture directions to improve the structural strength of the embryo body and increase the bearing capacity of the embryo body.
[0083] Figure 3 It is a schematic flow chart of step S710 to step S720 of the preparation method of the present invention. Figure 4 It is a schematic flow chart of steps S711 to S723 of the preparation method of the present invention.
[0084] See also Figures 2 to 4 In this embodiment, in step S700, during the hot pressing process, the embryo is hot pressed so that when the impregnation solutions in the multiple material units are heated and flow, the impregnation solutions between the multiple material units are in contact with each other, and the impregnation solutions in the embryo are integrated. After that, the embryo is heated and pressed to solidify the impregnation solution in the embryo, so that a dense laminated structure is formed on the surface and inside of the embryo, so as to improve the density of the embryo, and improve the wear resistance, impact resistance, corrosion resistance, water resistance, insulation and heat insulation of the embryo.
[0085] See also Figures 2 to 4 In this embodiment, step S700 is a hot pressing process, which includes step S710, a low pressure preheating stage and step S720, a hot pressing curing stage.
[0086] S710, low-pressure preheating stage, gradually raise the temperature of the embryo to melt and flow the uncured impregnation solution in the embryo, ensuring uniform distribution of the impregnation solution in the embryo. The impregnation solutions between two adjacent material units in the embryo are in contact, so that after the impregnation solution is cured in the subsequent hot pressing curing stage, the connection strength and physical and chemical properties of the material units in the embryo can be guaranteed.
[0087] S720, hot pressing and curing stage, the preheated embryo is gradually heated and pressed, and the impregnation solution is adhered to the embryo without overflowing during the hot pressing process, and multiple material units are adhered and bonded, and the impregnation solution is solidified. When the embryo is in the hot pressing state, the gaps between multiple material units gradually decrease, and the cell spacing of the material unit itself is also smaller under the pressure, which can effectively improve the wear resistance, structural strength, weather resistance, heat insulation, insulation and other properties of the embryo.
[0088] In some embodiments, the low-pressure preheating stage and the hot pressing curing stage of the embryo are both processed in a hot press. After the embryo is placed in the hot press, the temperature of the hot press is continuously increased so that the temperature in the hot press reaches the temperature required for preheating the embryo. At this time, the impregnation solution melts and flows. After preheating for a certain period of time, the impregnation solutions of adjacent material units contact and flow with each other to fully fill and distribute throughout the embryo. After the low-pressure preheating stage is completed, the temperature continues to rise to reach the hot pressing temperature, and pressure is applied to the embryo to gradually increase the density of the embryo, and the impregnation solution in the embryo is gradually solidified to ensure the adhesion strength of each material unit in the embryo, and improve the wear resistance, strength, weather resistance, heat insulation, insulation, corrosion resistance and other properties of the embryo.
[0089] In this embodiment, the preheating temperature range of the low-pressure preheating stage includes 50°C to 90°C, and the heating time includes 1min / mm to 6min / mm according to the thickness of the embryo. The preheating time of the low-pressure preheating stage can be adaptively selected and adjusted according to the material and thickness of the material unit.
[0090] See also Figures 2 to 4 , step S710, the low-pressure preheating stage includes step S711, the first stage heating and step S712, the second stage heating. Step S711, the first stage heating, the temperature range of the first stage heating includes 50℃~80℃, and the heating time includes 0.5min / mm~3min / mm according to the thickness of the embryo. Step S712, the second stage heating, the temperature range of the second stage heating includes 70℃~100℃, and the heating time includes 0.5min / mm~3min / mm according to the thickness of the embryo.
[0091] In some embodiments, during the preheating process, the embryo body in the low-pressure preheating stage is subjected to a relatively small pressure to compact the embryo body, and the compacting pressure to which the embryo body is subjected ranges from 0.01 kg / cm 2 to 0.5 kg / cm 2 .
[0092] In some embodiments, during the low-pressure preheating stage, the preheating temperature of the embryo body is increased from room temperature at a rate of 2° C. per minute until it reaches the preheating temperature corresponding to the different material units.
[0093] In this embodiment, the temperature range of the hot pressing curing stage includes 100°C to 160°C, and the pressure includes 4kg / cm 2 ~120kg / cm 2 The hot pressing time ranges from 6min / mm to 15min / mm according to the thickness of the embryo.
[0094] See also Figures 2 to 4 In this embodiment, step S720, the hot pressing curing stage includes three-stage hot pressing steps, which include:
[0095] Step S721, first stage hot pressing, the first stage hot pressing temperature range includes 100 ℃ ~ 120 ℃, pressure includes 4kg / cm 2 ~12kg / cm 2 The hot pressing time ranges from 2min / mm to 5min / mm according to the thickness of the embryo.
[0096] Step S722, second stage hot pressing, the temperature range of the second stage hot pressing includes 120℃~140℃, the pressure includes 50kg / cm 2 ~120kg / cm 2 The hot pressing time ranges from 2min / mm to 5min / mm according to the thickness of the embryo.
[0097] Step S723, the third stage of hot pressing, the temperature range of the third stage of hot pressing includes 120℃~140℃, the pressure includes 60kg / cm 2 ~120kg / cm 2 The hot pressing time ranges from 2min / mm to 5min / mm according to the thickness of the embryo.
[0098] The processing time of the hot pressing curing stage can be adaptively selected and adjusted according to the material and thickness of the material unit.
[0099] In some embodiments, the pressure in the hot pressing curing stage increases in proportion to the increase in temperature, thereby making the embryo body denser and having better connection strength during the hot pressing curing process.
[0100] In some embodiments, in the method for preparing the composite material of the present application, only in step S720, the hot pressing curing stage, the processing temperature first reaches the temperature required for thermal curing of the impregnation solution, so that the impregnation solution is cured and the processing of the material unit is completed.
[0101] Figure 5 It is a schematic flow chart of steps S810 to S850 of the preparation method of the present invention.
[0102] See also Figure 2 and Figure 5 In this embodiment, the method further includes step S800, which is a multi-stage cooling and pressure reduction process, wherein the embryo body after hot pressing is subjected to multi-stage cooling and pressure reduction to eliminate stress in the embryo body and ensure the bonding strength of multiple material units. After the embryo body is cooled and pressure reduced from a high temperature state, the internal stress of the embryo body can be reduced, and incomplete bonding between multiple material units can be prevented, thereby ensuring bonding strength.
[0103] It is understandable that the number of multi-stage cooling and pressure reduction stages can be selected as needed.
[0104] Step, S800, multi-stage cooling and pressure reduction processing includes step S810, first stage cooling and pressure reduction, step S820, second stage cooling and pressure reduction, step S830, third stage cooling and pressure reduction, step S840, fourth stage cooling and pressure reduction and step S850, fifth stage cooling and pressure reduction.
[0105] Step S810, first stage cooling and pressure reduction, the temperature range of the first stage cooling and pressure reduction includes 90℃~110℃, the pressure includes 60kg / cm 2 ~120kg / cm 2 The cooling time ranges from 3min / mm to 8min / mm according to the thickness of the embryo.
[0106] Step S820, second stage cooling and pressure reduction, the temperature range of the second stage cooling and pressure reduction includes 50℃~80℃, and the pressure includes 60kg / cm 2 ~120kg / cm 2 The cooling time ranges from 3min / mm to 8min / mm according to the thickness of the embryo.
[0107] Step S830, the third stage of cooling and pressure reduction, the temperature range of the third stage of cooling and pressure reduction includes 30℃~70℃, and the pressure includes 15kg / cm 2 ~45kg / cm 2 The cooling time ranges from 3min / mm to 8min / mm according to the thickness of the embryo.
[0108] Step S840, the fourth stage of temperature reduction and pressure reduction, the temperature range of the fourth stage of temperature reduction and pressure reduction includes 20℃~50℃, and the pressure includes 10kg / cm 2~30kg / cm 2 The cooling time ranges from 3min / mm to 8min / mm according to the thickness of the embryo.
[0109] Step S850, fifth stage cooling and pressure reduction, the temperature range of the fifth stage cooling and pressure reduction includes 20℃~35℃, and the pressure includes 4kg / cm 2 ~15kg / cm 2 The cooling time ranges from 3min / mm to 8min / mm according to the thickness of the embryo.
[0110] The embryo is first cooled from the hot pressing curing temperature to 90℃~110℃ of the first level of cooling and pressure reduction, and then cooled to 50℃~80℃ of the second level of cooling and pressure reduction after a certain period of time. After a certain period of time at the temperature of the second level of cooling and pressure reduction, the temperature is cooled to 30℃~70℃ of the third level of cooling and pressure reduction. After a certain period of time at the third level of cooling and pressure reduction, the temperature is cooled to 20℃~50℃ of the fourth level of cooling and pressure reduction. After a certain period of time at the fourth level of cooling and pressure reduction, the temperature is cooled to 20℃~35℃ of the fifth level of cooling and pressure reduction. After a certain period of time, the embryo is taken out of the hot press, thereby completing the multi-stage cooling and pressure reduction process.
[0111] After the embryo body has been subjected to multi-stage cooling and pressure reduction treatment, on the one hand, the internal stress inside the material unit is fully reduced, which improves the toughness of the embryo body. On the other hand, the internal stress between multiple material units in the embryo body is reduced to improve the structural strength and toughness of the embryo body. Due to the good toughness of the embryo body, the embryo body surface will not crack due to high brittleness when subjected to high temperature, so that the embryo body can be effectively used in the field of low-temperature storage tanks.
[0112] In some embodiments, during the hot pressing treatment and the multi-stage temperature and pressure reduction treatment, the internal stress and adhesive properties of the material itself should be fully considered.
[0113] Take the composite material of 10mm to 40mm as an example. It goes through the following steps: S711, the temperature after the first stage heating is 70℃, and the preheating time is 30min. S712, the temperature after the second stage heating is 90℃, and the preheating time is 20min.
[0114] S721, the first stage hot pressing temperature is 110℃, the pressing pressure is 5kg / cm 2 ~10kg / cm 2 , hot pressing time is 20min. S722, the temperature of the second stage hot pressing is 130℃, and the pressing pressure is 60kg / cm 2 ~90kg / cm 2 , hot pressing time is 20min. S723, the temperature of the third stage hot pressing is 130℃, and the pressing pressure is 70kg / cm 2 ~120kg / cm 2 , hot pressing time is 30min.
[0115] S810, the temperature of the first stage of cooling and pressure reduction is 100℃, and the pressure is 70kg / cm 2 ~120kg / cm 2 , the cooling time is 40min. S820, the temperature of the second stage cooling and pressure reduction is 60℃, and the pressure is 70kg / cm 2 ~120kg / cm 2 , the cooling time is 40min. S830, the temperature of the third stage cooling and pressure reduction is 40℃, and the pressure includes 20kg / cm 2 ~40kg / cm 2 , the cooling time is 30min. S840, the temperature of the fourth stage cooling and pressure reduction is 30℃, and the pressure includes 10kg / cm 2 ~20kg / cm 2 , the cooling time is 30min. S850, the temperature of the fifth stage cooling and pressure reduction is 25℃, the pressure includes 5kg / cm 2 ~10kg / cm 2 , the cooling time is 30min.
[0116] Figure 6 It is a schematic flow chart of step S900 of the preparation method of the present invention.
[0117] See also Figure 2 and Figure 6 In this embodiment, step S900 is also included, in which a secondary composite molding process is performed, in which a plurality of embryos are stacked, aerogel is coated between two adjacent embryos, and the plurality of embryos are pressurized and composited to form a composite material.
[0118] After the embryo has undergone multiple stages of cooling and pressure reduction, it has become a densely laminated composite material that can be used in the market. However, because some application scenarios have certain requirements for the thickness of the product, it is also possible to stack multiple embryos and coat aerogel between two adjacent embryos to make the multiple embryos bonded to each other. Afterwards, the multiple embryos are cold-pressed so that the aerogel is fully distributed on the side surfaces facing the two adjacent embryos, thereby improving the bonding strength between the multiple embryos. After the multiple embryos are bonded and cold-pressed, a composite material is formed for use in the market.
[0119] In some embodiments, the secondary composite molding process is performed by cold pressing at room temperature, the pressure is 15 MPa to 25 MPa, and the cold pressing time is 1 hour to 5 hours.
[0120] In some embodiments, the aerogel includes at least one of epoxy resin, epoxy putty, or polyurethane.
[0121] Figure 7It is a schematic flow chart of step S420 of the preparation method of the present invention.
[0122] See also Figure 2 and Figure 7 In this embodiment, after the cleaning process in step S400, step S420 is also included, in which the material unit is taken out from the vacuum container and placed on the rack, and the glue dripping time ranges from 0.5h to 3h.
[0123] After the cleaning process, the material unit is placed on the rack to allow the residual impregnation solution precipitated on the outer surface of the material unit during the cleaning process to further drip, so as to fully remove the impregnation solution on the surface of the material unit, thereby facilitating subsequent embryo processing and hot pressing processing, preventing the material unit from occupying the work station of the vacuum container, and improving the utilization efficiency of the vacuum container.
[0124] In some embodiments, carbonization treatment is also included. When the material unit is made of bamboo, because its cell wall is thin, the gaps between the cell walls are large, and there are a large number of pores on the cell wall, before the material unit is impregnated, carbonization treatment is performed by saturated steam to further reduce the nutrients in the bamboo, so that the bamboo is more permeable and the impregnation solution is filled and penetrated more fully.
[0125] See also Figures 1 to 7 In this embodiment, different fiber materials are made into material units. After the material units are treated with negative pressure, the air inside the material units is evacuated so that the impregnation solution can penetrate into the material units during the impregnation treatment.
[0126] After the material unit is subjected to negative pressure treatment, it is subjected to impregnation treatment and pressure treatment, so that the impregnation solution can fully penetrate into the material unit and the impregnation solution can be evenly distributed in the material unit.
[0127] After the pressure treatment, the material unit undergoes a cleaning treatment and a glue dripping treatment to remove the residual impregnation solution on the surface of the material unit so that the impregnation solution can be recycled and reused.
[0128] After the glue dripping treatment, the material units are assembled to form an embryo body, and then the embryo body is placed in a hot press for hot pressing. First, the material unit enters the low-pressure preheating stage, and the impregnation solution in the embryo body melts and flows, so that the impregnation solutions between multiple material units in the embryo body flow with each other, and the impregnation solutions in the embryo body form a whole. Then, the material unit enters the hot pressing and curing stage, and the hot press continues to increase the temperature and pressure to increase the overall density of the embryo body and solidify the impregnation solution to improve the connection strength, structural strength, wear resistance, thermal insulation performance, weather resistance and other characteristics of the embryo body.
[0129] After the hot pressing and curing stage, the embryo body undergoes a multi-stage cooling and pressure reduction treatment to effectively reduce the internal stress in the embryo body, improve the toughness of the embryo body, and thus improve the high temperature tolerance of the embryo body.
[0130] After the embryos are subjected to multi-stage cooling and pressure reduction, secondary composite molding treatment is performed to form a composite material from multiple embryos.
[0131] The composite material prepared by the preparation method of the present invention has a relatively uniform internal structure distribution and a short preparation reaction time. Under different impregnation pressures, evacuation speeds and pressure holding times, the impregnation effect, preparation efficiency, hot pressing effect and other aspects are significantly different from those of the existing German method.
[0132] Moreover, when the composite material is used in fields such as low-temperature storage tanks, it can effectively ensure the low-temperature thermal insulation performance of the composite material while preventing the composite material from cracking due to heat in a high-temperature environment, thereby ensuring the toughness of the composite material.
[0133] Figure 8 It is a supporting block made of the composite board material of the present invention. Fig. 9 The invention relates to a connecting piece structure made of a composite plate material.
[0134] See also Figure 1 , Figure 2 , Figure 8 and Fig. 9 The present invention also provides a composite plate material, the composite plate material includes a composite material plate, and the composite material plate is prepared by the above-mentioned composite material preparation method. It has extremely high structural strength, wear resistance, weather resistance, heat insulation, insulation, high temperature resistance and other properties. The composite plate material meets special requirements such as low low-temperature thermal conductivity, high pressure resistance, electrical insulation, weather resistance and corrosion resistance, low linear expansion coefficient, high wear resistance, and low friction coefficient. The composite plate material can be used as core components in the fields of cryogenic equipment such as cryogenic tanks, electrical insulation materials, special molds, piano core components, chemical equipment, bulletproof facilities, etc.
[0135] In some embodiments, the composite material board can be assembled and bonded with at least one of a wood board, a bamboo board, a bamboo-wood composite board, a plastic-wood composite board, a fiber-reinforced material, an impregnated paper, and a high-pressure laminate to form the composite board by hot pressing.
[0136] In some embodiments, the composite sheet material can be used to manufacture a support block 300 of a cryogenic storage tank.
[0137] In other embodiments, the composite board can also be used to manufacture structures such as the insulating connector 400 .
[0138] Fig.10 It is a partial plane cross-sectional view of the cryogenic storage tank of the present invention perpendicular to its axial direction.
[0139] See also Figure 1 , Figure 2 , Figure 8 and Fig.10The present invention also provides a cryogenic storage tank, which includes: a tank body 100, a support frame 200 and a plurality of support blocks 300. The tank body 100 is used to store cryogenic liquid; the support frame 200 is arranged on the periphery of the tank body 100 to support the tank body 100; the plurality of support blocks 300 are located between the tank body 100 and the support frame 200, and the plurality of support blocks 300 are arranged along the periphery of the tank body 100 to prevent the cold energy of the tank body 100 from being transferred to the support frame 200, and the support blocks 300 are made of the composite plate prepared by the above-mentioned preparation method.
[0140] In some embodiments, the support frame 200 is located at both ends of the tank body 100, and the support frame 200 extends along the circumference of the tank body 100 to support the tank body 100. A plurality of support blocks 300 are arranged along the circumference of the tank body 100, and the plurality of support blocks 300 can transfer the weight of the tube body to the support frame 200, and the plurality of support blocks 300 can isolate the cold transfer between the tank body 100 and the support frame 200.
[0141] When the cryogenic storage tank is transported empty, the temperature of the tank body 100 continues to rise when the sun shines on the tank body 100. However, since the support block 300 has extremely high toughness, the surface of the support block 300 will not crack due to excessive brittleness, thereby ensuring the safety performance of the empty cryogenic tank body 100 during transportation.
[0142] In some embodiments, a receiving groove is provided on a side of the support block 300 facing the tank body 100, and the receiving groove extends along the axial direction of the storage tank. A convex block is provided on the tank body 100 relative to the receiving groove, and the convex block is engaged in the receiving groove.
[0143] In some embodiments, the inner wall of the receiving groove is coated with aerogel to form an aerogel layer, and the aerogel layer is bonded to the inner wall of the receiving groove and the protrusion to improve the connection strength between the support block 300 and the tank body 100. In addition, because the support block 300 has good low temperature resistance, high temperature resistance, structural strength, thermal insulation performance, and insulation performance, it can be applied to various extreme environments and has a long service life. Compared with the support block 300 produced by the German method in the prior art, it has a wide source of materials, low cost, good performance, long service life, and low failure rate.
[0144] Although the present application has been described with reference to several typical embodiments, it should be understood that the terms used are illustrative and exemplary, rather than restrictive. Since the present application can be implemented in a variety of forms without departing from the spirit or essence of the invention, it should be understood that the above embodiments are not limited to any of the foregoing details, but should be interpreted broadly within the spirit and scope defined by the appended claims, so all changes and modifications falling within the scope of the claims or their equivalents should be covered by the appended claims.
Claims
1. A method for preparing a composite material, which is used for processing a material unit, characterized in that: The material of the material unit includes at least one of bamboo, wood, reed, non-woven fabric or paper; the preparation method includes the following steps: Negative pressure treatment, the material unit is placed in a vacuum container, and the vacuum container is evacuated to reach a negative pressure state; the vacuum degree of the material unit during the negative pressure treatment is maintained at 0.04Mpa~0.09Mpa, and the negative pressure time includes 0.5h~1.5h; Impregnation treatment, after the negative pressure treatment, the vacuum container is kept in a negative pressure state, and then an impregnation solution is injected into the vacuum container so that the impregnation solution penetrates into the material unit; the impregnation solution includes at least one of melamine-formaldehyde resin, phenolic resin, urea-formaldehyde resin, isocyanate and polycarboxylic acid; the vacuum degree of the impregnation treatment is maintained at 0.04Mpa~0.09Mpa, and the impregnation time is 1h~12h; Pressurizing treatment, pressurizing the vacuum container after the impregnation treatment to allow the impregnation solution to diffuse rapidly in the material unit, and then emptying the residual impregnation solution in the vacuum container; the pressure of the pressurizing treatment includes 0.5Mpa~1.2Mpa, and the pressurizing time includes 1h~6h; Cleaning treatment: after the pressurization treatment, the vacuum container is evacuated to reach a negative pressure state, so that the impregnation solution remaining on the outer surface of the material unit quickly drips into the vacuum container, and then the material unit is taken out of the vacuum container; the vacuum degree of the cleaning treatment is maintained at 0.04Mpa~0.09Mpa, and the cleaning time includes 10min~40min; Drying and balancing treatment, first drying the taken-out material unit, and then performing balancing treatment after drying; Embryo formation treatment, stacking the plurality of material units after balancing treatment to form an embryo body; Hot pressing treatment, hot pressing the embryo to solidify the embryo; the hot pressing treatment includes a low-pressure preheating stage and a hot pressing solidification stage: the embryo in the low-pressure preheating stage is heated to 0.01 kg / cm 2 -0.5kg / cm 2 Under the compacting pressure, the embryo body is heated from room temperature at a rate of 2°C per minute, so that the impregnation solution in the embryo body melts and flows, ensuring that the impregnation solution in the embryo body is evenly distributed; the low-pressure preheating stage includes two-stage heating, the temperature range of the first stage heating includes 50°C~80°C, and the heating time includes 0.5min / mm~3min / mm according to the thickness of the embryo body; the temperature range of the second stage heating includes 70°C~100°C, and the heating time includes 0.5min / mm~3min / mm according to the thickness of the embryo body; In the hot pressing and curing stage, the embryo body after the preheating treatment is gradually heated and pressed, and during the hot pressing process, the impregnation solution is adhered to the embryo body without overflowing, and the plurality of material units are adhered to each other, and the impregnation solution is cured; The hot pressing curing stage includes three stages of hot pressing, the temperature range of the hot pressing in the first stage includes 100°C~120°C, the pressure range includes 4kg / cm²~12kg / cm², and the hot pressing time includes 2min / mm~5min / mm according to the thickness of the embryo; the temperature range of the hot pressing in the second stage includes 120°C~140°C, the pressure includes 50kg / cm²~120kg / cm², and the hot pressing time includes 2min / mm~5min / mm according to the thickness of the embryo; the temperature range of the hot pressing in the third stage includes 120°C~140°C, the pressure includes 60kg / cm²~120kg / cm², and the hot pressing time includes 2min / mm~5min / mm according to the thickness of the embryo; Multi-stage cooling and pressure reduction treatment, wherein the embryo body after heat pressing and curing is subjected to multi-stage cooling and pressure reduction to eliminate stress in the embryo body and ensure the bonding strength of the plurality of material units; The multi-stage cooling and pressure reduction treatment includes five stages of cooling and pressure reduction, the temperature range of the first stage cooling and pressure reduction includes 90℃~110℃, the pressure includes 60kg / cm²~120kg / cm², and the cooling time includes 3 min / mm~8min / mm according to the thickness of the embryo; the temperature range of the second stage cooling and pressure reduction includes 50℃~80℃, the pressure includes 60kg / cm²~120kg / cm², and the cooling time includes 3 min / mm~8min / mm according to the thickness of the embryo; the temperature range of the third stage cooling and pressure reduction includes 30℃~70℃, the pressure includes 15kg / cm2~45kg / cm², and the cooling time includes 3 min / mm~8min / mm according to the thickness of the embryo; the temperature range of the fourth stage cooling and pressure reduction includes 20℃~50℃, the pressure includes 10kg / cm²~30kg / cm², and the cooling time includes 3min / mm according to the thickness of the embryo ~8min / mm; the temperature range of the fifth stage of cooling and pressure reduction includes 20℃~35℃, the pressure includes 4kg / cm²~15kg / cm², and the cooling time includes 3 min / mm ~8min / mm according to the thickness of the embryo.
2. The method for preparing a composite material according to claim 1, characterized in that: The method also includes a secondary composite molding process, in which a plurality of the embryos are stacked, aerogel is coated on the facing sides of two adjacent embryos, and the plurality of embryos are pressurized and composited to form the composite material.
3. The method for preparing a composite material according to claim 1, characterized in that: The cleaning process also includes a glue dripping process. After the material unit is taken out from the vacuum container, it is placed on a rack, and the glue dripping time includes 0.5h~3h.
4. A composite sheet, characterized in that: include: The composite plate comprises a composite material plate, and the composite material plate is prepared by the preparation method according to any one of claims 1 to 3.
5. The composite sheet material according to claim 4, characterized in that: The composite material board can be bonded with at least one of a wood board, a bamboo board, a bamboo-wood composite board, a plastic-wood composite board, a fiber-reinforced material, an impregnated paper, and a high-pressure laminate to form the composite board by hot pressing.
6. A cryogenic storage tank, characterized in that: include: A tank for storing cryogenic liquids; A support frame, which is arranged on the peripheral side of the tank body to support the tank body; A plurality of support blocks are located between the tank body and the support frame. The plurality of support blocks are arranged along the circumference of the tank body to prevent the cold of the tank body from being transferred to the support frame. The support blocks are made of the composite plate material as described in any one of claims 4 to 5.
7. The cryogenic storage tank according to claim 6, characterized in that: The support block is provided with a receiving groove on one side facing the tank body, and the receiving groove extends along the axial direction of the storage tank; the tank body is provided with a protrusion relative to the receiving groove, and the protrusion is engaged in the receiving groove; the inner wall of the receiving groove is coated with aerogel to form an aerogel layer, and the aerogel layer is bonded to the inner wall of the receiving groove and the protrusion.
Citation Information
Patent Citations
Bamboo-wood composite board and preparation method thereof
CN101745947A
Insulating wood laminating product and preparation method thereof
CN101941217A
Bamboo plate manufacturing process
CN102744760A
Dipping compression strengthened floor and manufacturing method thereof
CN102990759A
Hot pressing process for plywood
CN105382889A